Preparation method of temperature compensation filter, temperature compensation filter and electronic device
By using photolithography and overlay processes to peel off the photoresist during the preparation of the temperature compensation filter, and preparing an initial temperature compensation film on magnetron sputtering equipment, the problems of photoresist contamination and harmful etching are solved and improved Improved temperature compensation film performance and expanded photoresist types.
Patent Information
- Application Number
- CN202210341696.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-03-29
AI Technical Summary
Among the existing temperature compensation filter preparation methods, the vacuum chamber of the magnetron sputtering equipment is easily contaminated by photoresist, and the dry or wet etching process is not friendly to the environment and human health, and the types of photoresists are limited.
A first metal film is prepared on the substrate through a photolithography process and the photoresist is peeled off. Then a second metal film is prepared in some areas and the photoresist in the overlay process is peeled off. Magnetron sputtering equipment is used to prepare the two films. Initial temperature repair film, and remove unnecessary film through chemical mechanical polishing and polishing to avoid contamination and harmful etching.
It effectively avoids photoresist contamination, improves the performance of the temperature compensation film, avoids the adverse effects of dry or wet etching, and expands the optional types of photoresists.
Smart Images

Figure CN114679146B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of temperature compensation filters, and in particular to a preparation method of a temperature compensation filter, a temperature compensation filter and electronic equipment. Background Art
[0002] Temperature compensation filter (TCSAW), also known as temperature compensated surface acoustic wave filter, is currently prepared by first making a metal interdigital transducer on a piezoelectric substrate, then growing or sputtering a layer of silicon dioxide of a certain thickness to form a multilayer structure, and using the positive temperature coefficient of silicon dioxide to compensate for the negative temperature coefficient of the piezoelectric substrate. The commonly used process routes are divided into the following two types:
[0003] 1) The first process route is: cleaning substrate → photolithography of the first layer of pattern → metal film coating → stripping of the first layer of pattern → overlay bonding area → sputtering temperature compensation film - chemical mechanical polishing (CMP) → stripping, which has the following disadvantages:
[0004] Since the temperature compensation film is deposited by magnetron sputtering equipment, it is relatively dense and not conducive to stripping. If the stripping process is used when depositing the temperature compensation film, it is necessary to carry the photoresist into the sputtering chamber. Photoresist is an organic matter. Under the influence of plasma and heating, the organic matter in the photoresist will volatilize into the vacuum chamber, causing the high-purity target material and the lining of the vacuum chamber of the magnetron sputtering equipment to be contaminated, affecting the purity of the subsequent deposited film and the service life of the target material.
[0005] 2) The second process route is: cleaning substrate → photolithography of the first layer of pattern → metal film coating → stripping of the first layer of pattern → sputtering temperature compensation film → chemical mechanical polishing (CMP) → overlay bonding area → wet etching or dry etching, which has the following disadvantages:
[0006] Dry etching equipment is expensive, and the etching gas is generally not friendly to the environment and human health. Wet etching requires the use of hydrofluoric acid series chemicals, which is also not friendly to the environment and human health. And there are few types of photoresists that are resistant to hydrofluoric acid etching. Summary of the invention
[0007] The technical problem to be solved by the present invention is to address the deficiencies of the prior art and provide a method for preparing a temperature compensation filter, a temperature compensation filter and an electronic device.
[0008] The technical solution of a method for preparing a temperature compensation filter of the present invention is as follows:
[0009] Using a photolithography process, preparing a first metal film on a substrate, and stripping off the photoresist used in the photolithography process;
[0010] Preparing a second metal film on a partial area of the first metal film through an overlay process, and stripping off the photoresist used in the overlay process;
[0011] An initial temperature compensation film is prepared on the first metal film and the second metal film by using a magnetron sputtering device, and the second metal film and part of the initial temperature compensation film on the second metal film are removed to obtain a temperature compensation filter.
[0012] The beneficial effects of the method for preparing a temperature compensation filter of the present invention are as follows:
[0013] Before using the magnetron sputtering equipment to prepare the initial temperature compensation film, the photoresist used in the photolithography process and the photoresist used in the overlay process have been stripped to avoid contamination caused by carrying the photoresist into the vacuum chamber coating of the magnetron sputtering equipment. Since there is no photoresist, there is no need to deliberately lower the process temperature when preparing the initial temperature compensation film. The performance of the temperature compensation film can be improved by increasing the process temperature. In addition, the adverse effects of dry etching and wet etching can be avoided, and there are many types of photoresists to choose from.
[0014] On the basis of the above scheme, the method for preparing a temperature compensation filter of the present invention can be further improved as follows.
[0015] Further, the stripping of the photoresist used in the photolithography process comprises:
[0016] stripping the photoresist used in the photolithography process by a first stripping solution;
[0017] The stripping of the photoresist used in the overlay process comprises:
[0018] The photoresist used in the photolithography process is stripped by the first stripping solution.
[0019] Further, the removing of the second metal film and a portion of the initial temperature compensation film on the second metal film includes:
[0020] The initial temperature compensation film is polished and leveled until the second metal film is exposed to obtain a temperature compensation film, and the second metal film is peeled off.
[0021] Furthermore, the first metal film and the second metal film are made of different materials.
[0022] Furthermore, the first metal film is made of titanium or aluminum.
[0023] Further, the peeling off the second metal film comprises:
[0024] The second metal film is peeled off by a second peeling liquid.
[0025] Furthermore, the first stripping liquid is acetone.
[0026] The present invention provides a temperature compensation filter prepared by using any one of the above-mentioned methods for preparing a temperature compensation filter.
[0027] An electronic device of the present invention comprises the above-mentioned temperature compensation filter. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A schematic flow chart of a method for preparing a temperature compensation filter according to an embodiment of the present invention;
[0029] Figure 2 A schematic diagram of the structure for preparing a first photoresist layer;
[0030] Figure 3 is a schematic diagram of the structure for depositing the first initial metal layer;
[0031] Figure 4 A schematic diagram of the structure for preparing a first metal film;
[0032] Figure 5 A schematic diagram of the structure for preparing a second photoresist layer;
[0033] Figure 6 A schematic diagram of the structure for preparing a second initial metal layer;
[0034] Figure 7 A schematic diagram of the structure for preparing a second metal film;
[0035] Figure 8 It is a schematic diagram of the structure for preparing the initial temperature compensation film;
[0036] Fig. 9 It is a schematic diagram of the structure after flattening and polishing;
[0037] Fig.10 The figure is a schematic diagram of the structure of a temperature compensation filter prepared. DETAILED DESCRIPTION
[0038] like Figure 1 As shown, a method for preparing a temperature compensation filter according to an embodiment of the present invention comprises the following steps:
[0039] S1. Prepare a first metal film 4 on a substrate 1 by using a photolithography process, and peel off the photoresist used in the photolithography process; wherein the substrate 1 is a piezoelectric substrate 1.
[0040] S2, preparing a second metal film 7 on a partial area of the first metal film 4 through an overlay process, and stripping off the photoresist used in the overlay process;
[0041] S3, using magnetron sputtering equipment to prepare an initial temperature compensation film 8 on the first metal film 4 and the second metal film 7, and removing the second metal film 7 and part of the initial temperature compensation film 8 on the second metal film 7 to obtain a temperature compensation filter.
[0042] Before using the magnetron sputtering device to prepare the temperature compensation film 9, the photoresist used in the photolithography process and the photoresist used in the overlay process have been stripped, avoiding the contamination caused by carrying the photoresist into the vacuum chamber coating of the magnetron sputtering device. Since there is no photoresist, there is no need to deliberately reduce the process temperature when preparing the temperature compensation film 9. The performance of the temperature compensation film 9 can be improved by increasing the process temperature. Moreover, the adverse effects of dry etching and wet etching can be avoided, and there are many types of photoresists to choose from.
[0043] Optionally, in the above technical solution, in S1, stripping the photoresist used in the photolithography process includes:
[0044] S10, stripping the photoresist used in the photolithography process by using a first stripping solution;
[0045] In S2, the photoresist used in the overlay process is stripped, including:
[0046] S20, stripping the photoresist used in the photolithography process using a first stripping solution.
[0047] The photoresist used in the photolithography process and the photoresist used in the overlay process may be the same or different, but generally speaking, both are soluble in acetone. Therefore, acetone is determined as the first stripping solution.
[0048] Optionally, in the above technical solution, in S3, removing the second metal film 7 and part of the temperature compensation film 9 on the second metal film 7 includes:
[0049] S30 , polishing the initial temperature compensation film 8 until the second metal film 7 is exposed to obtain the temperature compensation film 9 , and peeling off the second metal film 7 .
[0050] Optionally, in the above technical solution, the first metal film 4 and the second metal film 7 are made of different materials, specifically:
[0051] The first metal film 4 is made of titanium or aluminum, and the second metal film 7 is made of copper. Titanium and aluminum are both insoluble in N-methylpyrrolidone, but copper is soluble in N-methylpyrrolidone, so N-methylpyrrolidone is used as the second stripping solution.
[0052] In another embodiment, the second metal film 7 and part of the initial temperature compensation film 8 on the second metal film 7 can be directly removed by mechanical methods or other means to prepare a temperature compensation filter.
[0053] The following is another example of a method for preparing a temperature compensation filter of the present application.
[0054] S100, cleaning substrate 1, specifically:
[0055] The piezoelectric substrate 1 is cleaned with an electronic cleaning agent, a megasonic cleaning machine, a brush, high-pressure deionized water, etc., and then dried.
[0056] S101, preparing a first metal film 4, specifically:
[0057] S1010, using a coating machine to coat the photoresist to prepare a first photoresist layer 2, wherein the rotation speed of the coating machine is 3000 revolutions per minute, the pre-baking temperature is 94° C., the pre-baking time is 2 minutes, the exposure is 380 ms, and the development is 8 seconds. Figure 2 As shown;
[0058] S1011, depositing the first initial metal layer 3: depositing metal Ti or Al etc. through an electron beam evaporation station to obtain the first initial metal layer 3, such as Figure 3 As shown;
[0059] S1012, obtain the first initial metal layer 3, immerse it in a first stripping solution, dissolve the photoresist of the first photoresist layer 2, and then use a stripping machine to strip it to achieve metallization of the first layer of graphics, that is, obtain the first metal film 4, such as Figure 4 shown.
[0060] S102, preparing a second metal film 7. Specifically:
[0061] S1020, protect the area except the bonding area with photoresist, the thickness of the photoresist coating needs to be greater than the thickness of the metal mask, i.e., the second initial metal layer 6, and the photoresist coating is recorded as the second photoresist layer 5. Figure 5 As shown, an electron beam evaporation station is used to deposit metal copper to obtain a second initial metal layer 6, such as Figure 6 As shown, the rotation speed of the engraving machine is 5000 revolutions per minute, the pre-baking temperature is 94°C, the pre-baking time is 2 minutes, the exposure is 10 seconds, the post-baking temperature is 94°C, the post-baking time is 2 minutes, and the development is 18 seconds. Among them, the material of the second metal film 7 is different from that of the first metal film 4. The material of the first metal film 4 is titanium or aluminum, and the material of the second metal film 7 is copper.
[0062] S1021, after the second initial metal layer 6 is deposited, it is immersed in a first stripping solution, the first stripping solution can dissolve the photoresist, but cannot dissolve the second metal film 7 and the first metal film 4, and then it is stripped to prepare the metal mask film of the bonding area, that is, to obtain the second metal film 7, such as Figure 7 As shown, specifically, the second metal film 7 may only cover a local area of the first metal film 4, that is, the second metal film 7 is prepared on a partial area of the first metal film 4, and the actual position of the local area can be set according to actual conditions, which will not be elaborated here.
[0063] S103, preparing a temperature compensation film 9, specifically:
[0064] S1030, using a magnetron sputtering device to prepare an initial temperature compensation film 8 on the first metal film 4 and the second metal film 7, the thickness of the initial temperature compensation film 8 is 1 μm, such as Figure 8 shown.
[0065] S1030, chemically mechanically flattening and polishing the initial temperature compensation film 8 by CMP process to make the initial temperature compensation film 8 flat until the second metal film 7 is exposed. Fig. 9 As shown, a temperature compensation film 9 is obtained, and the second metal film 7 is peeled off. Specifically:
[0066] By soaking in a second stripping solution, the second stripping solution is N-methylpyrrolidone, the second stripping solution can dissolve the second metal film 7 made of copper, but does not dissolve the first metal film 4 made of titanium or aluminum, and then the second metal film 7 is stripped to expose the bonding area for connection, thereby preparing a temperature compensation filter, such as Fig.10 shown.
[0067] In another embodiment, after S1030, the process includes: directly removing the second metal film 7 and a portion of the initial temperature compensation film on the second metal film 7 by mechanical means or other means to prepare Fig.10 The temperature compensated filter is shown.
[0068] In the above embodiments, although the steps are numbered S1, S2, etc., these are only specific embodiments given in the present application. Those skilled in the art may adjust the execution order of S1, S2, etc. according to actual conditions, which is also within the scope of protection of the present invention. It can be understood that in some embodiments, some or all of the above embodiments may be included.
[0069] A temperature compensation filter in an embodiment of the present invention is prepared by using any one of the above methods for preparing a temperature compensation filter.
[0070] An electronic device according to an embodiment of the present invention comprises the above-mentioned temperature compensation filter. The electronic device may be a computer or a mobile phone.
[0071] In the present invention, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0072] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0073] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a temperature compensation filter, characterized in that: include: Using a photolithography process, preparing a first metal film on a substrate, and stripping off the photoresist used in the photolithography process; Preparing a second metal film on a partial area of the first metal film through an overlay process, and stripping off the photoresist used in the overlay process; Using a magnetron sputtering device to prepare an initial temperature compensation film on the first metal film and the second metal film, and removing the second metal film and a portion of the initial temperature compensation film on the second metal film to obtain a temperature compensation filter; The stripping of the photoresist used in the photolithography process comprises: stripping the photoresist used in the photolithography process by a first stripping solution; The stripping of the photoresist used in the overlay process comprises: stripping the photoresist used in the photolithography process by using the first stripping solution; The removing of the second metal film and a portion of the temperature compensation film on the second metal film comprises: The initial temperature compensation film is polished and leveled until the second metal film is exposed to obtain a temperature compensation film, and the second metal film is peeled off; The first metal film and the second metal film are made of different materials; The material of the first metal film is titanium or aluminum; The material of the second metal film is copper; The stripping of the second metal film comprises: stripping the second metal film by a second stripping solution; The first stripping liquid is acetone; Also includes: The piezoelectric substrate is cleaned with an electronic cleaning agent, a megasonic cleaning machine, a brush and high-pressure deionized water, and then dried; Using a coating machine to coat the photoresist to prepare a first photoresist layer, wherein the rotation speed of the coating machine is 3000 revolutions per minute, the pre-baking temperature is 94° C., the pre-baking time is 2 minutes, the exposure is 380 milliseconds, and the development is 8 seconds; using an electron beam evaporation table, metal Ti or Al is deposited to obtain a first initial metal layer, the first initial metal layer is immersed in a first stripping solution to dissolve the photoresist of the first photoresist layer, and then a stripping machine is used to strip it to achieve metallization of the first layer of graphics, that is, to obtain a first metal film; The area other than the bonding area is protected with a photoresist, the thickness of the photoresist coating is greater than the thickness of the metal mask, i.e., the second initial metal layer, and the photoresist coating is recorded as the second photoresist layer. The metal copper is deposited by an electron beam evaporation station to obtain the second initial metal layer. The speed of the overlay machine is 5000 revolutions per minute, the pre-baking temperature is 94° C., the pre-baking time is 2 minutes, the exposure is 10 seconds, the post-baking temperature is 94° C., the post-baking time is 2 minutes, and the development is 18 seconds; After the second initial metal layer is deposited, it is immersed in a first stripping solution, the first stripping solution dissolves the photoresist but does not dissolve the second metal film and the first metal film, and is later stripped to achieve the preparation of the metal mask film in the bonding area, that is, to obtain the second metal film, which only covers a local area of the first metal film; An initial temperature compensation film is prepared on the first metal film and the second metal film by using a magnetron sputtering device, and the thickness of the initial temperature compensation film is 1 μm; The initial temperature compensation film is subjected to chemical mechanical flattening and polishing by a CMP process to flatten the initial temperature compensation film until the second metal film is exposed to obtain the temperature compensation film, and then the second metal film is peeled off.
2. A temperature compensation filter prepared by the method for preparing a temperature compensation filter according to claim 1.
3. An electronic device, characterized in that: A temperature compensation filter is included as claimed in claim 2.