Tissue repair membrane

By treating the modified layer of the fiber membrane with energy line irradiation, the problem of swelling and deformation of electrospun fiber membranes in liquid environment is solved, the structural stability and mechanical properties of the membrane material are improved, the risk of material residue is avoided, and it is suitable for industrial applications.

CN114681671BActive Publication Date: 2024-11-29MEDPRIN REGENERATIVE MEDICAL TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202011608751.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-30
Publication Date
2024-11-29
Estimated Expiration
2040-12-30

AI Technical Summary

Technical Problem

Existing electrospun fiber membranes are prone to swelling and deformation in liquid environments, affecting dimensional stability, and the introduction of crosslinking agents may increase the risk of substance residue.

Method used

By irradiating the modified layer of the fiber membrane with energy lines, cladding, cross-linking, or shrinkage can be achieved, maintaining the structural stability of the fiber membrane in a liquid environment while avoiding the introduction of new residual substances.

Benefits of technology

It alleviates the problem of dimensional changes in fiber membranes in liquid environments, improves mechanical properties and self-support, reduces processing costs, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114681671B_ABST
    Figure CN114681671B_ABST
Patent Text Reader

Abstract

The present invention relates to a tissue repair membrane, which is a fiber membrane, comprising a base layer and a modified layer, wherein at least a portion of the modified layer is irradiated with energy lines to produce cladding, cross-linking and / or shrinkage; the fiber membrane comprises fibers derived from a composition containing natural hydrophilic materials. The present invention can alleviate or inhibit the problem of changes in size or shape of the tissue repair membrane due to swelling during use by isomerizing at least one modified layer of the tissue repair membrane, without the need to introduce other components, while maintaining the fiber structure inside the tissue repair membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of medical materials, and specifically relates to a biomedical restorative material, and more specifically, to a fiber membrane for human tissue repair and a medical repair product comprising the fiber membrane. Background Art

[0002] In surgical practice, various clinical repair products have been tried for tissue defects caused by trauma, accidents, cancer, etc. Usually, products that can be used for tissue repair are not only required to have good biocompatibility, appropriate degradability and certain strength, but also to add components that facilitate cell adhesion or growth in order to promote post-traumatic tissue regeneration or accelerate wound healing.

[0003] Such tissue repair products can usually be provided in the form of scaffolds or repair membranes. Among them, the repair membrane can usually be formed by nanofibers through a spinning process, especially an electrospinning process. And the electrospinning process has good application effects in the field of tissue repair due to its advantages such as nanoscale, high specific surface area, and simulation of extracellular matrix.

[0004] Furthermore, due to the particularity of human tissue structure and function, the ideal fiber membrane for tissue repair needs to have the following properties: good biocompatibility, able to guide tissue growth to achieve ideal repair; easy for cell adhesion, crawling and growth to achieve tissue regeneration; a certain strength to resist mechanical stress, and be able to provide sufficient mechanical support before healthy tissue is fully formed, such as being used in the repair of tissues such as peritoneum, ligaments, and tendons; soft texture to reduce patient discomfort and improve surgical results; strong clinical practicality, easy to cut, not loose, easy to suture with tissue or fit with tissue anatomical structure; able to maintain good dimensional stability after implantation in the human body, without shrinkage and deformation; prevent bacteria from hiding and breeding, and avoid infection caused by the use of artificial biosynthetic materials; more preferably, the tissue repair membrane is degraded and absorbed in the body after the repair is completed.

[0005] Reference 1 discloses a chitosan-based nerve fiber membrane and a preparation method thereof. The chitosan-based nerve fiber membrane is formed by a plurality of oriented composite nanofibers; each composite nanofiber is a core-shell structure, wherein the shell layer contains a degradable functional material, carbon nanotubes modified with hydrophilic functional groups, wolfberry polysaccharides, and chitosan and / or chitosan derivatives, and the core layer contains nerve growth factor and a stabilizer.

[0006] Reference 2 discloses a functional guided muscle tissue repair membrane and its preparation method and application. The repair membrane is made of polycaprolactone and collagen as the matrix material, and is a randomly arranged micron-scale fiber membrane with a fiber diameter of 1 to 10 μm and a membrane thickness of 50 to 500 μm prepared by electrospinning. It may also include a hydrogel loaded with a protein having a coagulation function on the repair membrane and a protein that promotes cell growth bound to the hydrogel.

[0007] Cited document 3 discloses a fiber membrane for tissue repair, which is interwoven with fiber filaments with a diameter of 10 nm to 100 μm and formed by electrospinning. The material of the fiber filaments is one or more selected from the following polymer materials or their derivatives: collagen, cellulose, chondroitin sulfate, chitosan, modified chitosan, fibrin, silk protein, elastin-mimicking peptide polymers, heparin, agar, dextran, alginate, modified cellulose, alginic acid, starch, polyols, block polyethers, gelatin, polyvinyl pyrrolidone, polycaprolactone, polyglycolic acid, polylactic acid-glycolic acid copolymer, 1,3-propylene glycol polymer, polylactic acid-caprolactone copolymer or polylactic acid, etc.

[0008] Furthermore, in the field of tissue repair using existing electrospun membranes, as mentioned above, in order to improve the biocompatibility and tissue repair performance of the membranes, natural hydrophilic materials such as collagen, gelatin, and polysaccharides are usually added with synthetic materials such as polylactic acid for composite electrospinning to promote the adhesion and growth of tissue cells and membranes. However, in some cases where there is a lot of tissue fluid or other fluid and it exists for a long time, the hydrophilic materials such as collagen, gelatin, and polysaccharides in the electrospun membrane will swell, resulting in structural changes such as fiber slippage or membrane deformation, and such changes usually lead to displacement of the membrane after implantation or loss of the original pore barrier function.

[0009] In order to maintain the original structure of hydrophilic materials that are easily swellable, such as collagen and gelatin, and to improve the stability of the structure during use, the current common method is to cross-link and fix them through cross-linking agents. However, after the introduction of cross-linking agents, some cross-linking agents are difficult to remove from porous membrane materials, which may increase concerns about the risk of new residual substances. If traditional fusion methods such as hot pressing are used, it is easy to destroy the overall fiber pore structure of the electrospinning membrane material, making the entire membrane material dense, resulting in poor flexibility and poor adherence to the human body.

[0010] It can be seen that there is still room for further improvement in the field of providing restorative medical products with better usability.

[0011] References:

[0012] Reference 1: CN111632193A

[0013] Reference 2: CN110404117A

[0014] Reference 3: CN106492272B Summary of the invention

[0015] Problem that the invention aims to solve

[0016] The fiber membranes for tissue repair commonly used in the prior art, especially when the fiber membranes are prepared by the electrospinning method, usually use natural hydrophilic materials combined with artificial synthetic materials such as polylactic acid as spinning materials. Therefore, the membrane material obtained after electrospinning is prone to swelling, deformation and other problems in the solution, which affects the dimensional stability of the fiber membrane.

[0017] To address this problem, the present invention provides a tissue repair membrane based on a fiber membrane, by isomerizing at least a portion of the structure of the repair membrane, so that the fibers in this portion of the structure of the repair membrane are isomerized and modified while the fibers in other parts remain in their original state. The isomerized modified fibers can maintain the electrospun membrane material, especially the membrane material obtained by electrospinning, without swelling and deformation in a liquid environment.

[0018] In addition, the repair membrane provided by the present invention does not increase the risk of new residual substances, while maintaining the internal fiber structure of the membrane material without change.

[0019] Solutions for solving problems

[0020] After long-term research by the inventors of the present invention, it is found that the above technical problems can be solved by implementing the following technical solutions:

[0021] The present invention first provides a tissue repair membrane, wherein the repair membrane is a fiber membrane.

[0022] The fiber membrane comprises a base layer and at least one modified layer, wherein at least a part of the modified layer is irradiated with energy rays to generate cladding, cross-linking or shrinkage;

[0023] The fiber membrane includes fibers derived from a composition containing a natural hydrophilic material.

[0024] The modified layer exists at least in one main surface of the fiber membrane or the modified layer forms at least one main surface of the fiber membrane.

[0025] Furthermore, based on 100% of the average thickness of the fiber membrane, the average thickness of each modified layer is less than 10%.

[0026] Furthermore, the area of ​​the modified layer irradiated by the energy line forms a grid-like, stripe-like, staggered or array-like dot-like pattern or a combination of these patterns.

[0027] Furthermore, the energy line includes an energy particle flow or a photon beam flow.

[0028] Preferably, the energy line is a laser, and the ratio between the laser power W and the laser scanning speed V is 0.15-0.25.

[0029] Furthermore, the average thickness of the fiber membrane is less than 0.5 mm, preferably 0.1 mm to 0.3 mm.

[0030] Furthermore, the average porosity of the fiber membrane is less than 85%, preferably 40% to 80%.

[0031] Furthermore, the composition containing natural hydrophilic materials also includes artificial synthetic materials.

[0032] Preferably, the natural hydrophilic material in the composition containing natural hydrophilic materials is selected from one or more of gelatin, collagen, and polysaccharides, and the artificial synthetic material includes one or more of polyester materials; preferably, the mass ratio between the artificial synthetic material and the natural hydrophilic material is (20%:80%) to (80%:20%).

[0033] Furthermore, the present invention also provides a laminate for tissue repair, wherein at least one layer of the laminate comprises the above-mentioned tissue repair membrane.

[0034] Effects of the Invention

[0035] By implementing the above technical solution of the present invention, the following technical effects can be obtained:

[0036] 1) By isomerizing at least one modified layer of the tissue repair membrane, the problem of the tissue repair membrane changing in size or shape due to swelling during use, thereby affecting the fit or fixation with human tissue and thus reducing the usability, can be alleviated or suppressed;

[0037] 2) The isomerization treatment of the modified layer of the tissue repair membrane provided by the present invention can not only suppress the problem of dimensional change during use, but also, in a preferred case, provide improved mechanical properties for the repair membrane, or help increase the self-supporting property of the repair membrane, and also provide better convenience when cutting the repair membrane;

[0038] 3) By isomerizing the modified layer of the tissue repair membrane, the above effects can be achieved without introducing other components, thus avoiding the risk of residual substances caused by the introduction of new substances.

[0039] 4) The tissue repair membrane provided by the present invention has the advantages of easy processing and low cost, which is conducive to large-scale industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 : Dry microscope transmission image of a sample before and after laser surface treatment in a specific embodiment of the present invention;

[0041] Figure 2 : Wet microscope transmission image of a sample after laser surface treatment in a specific embodiment of the present invention;

[0042] Figure 3 : Wet microscope reflection image of a sample before and after laser surface treatment in a specific embodiment of the present invention;

[0043] Figure 4 : Wet microscope reflection image of a sample after laser surface treatment in a specific embodiment of the present invention;

[0044] Figure 5 : SEM image of a sample after laser surface treatment in a specific embodiment of the present invention (400 times);

[0045] Figure 6 : SEM image of a sample treated with laser surface in a specific embodiment of the present invention (1000 times); Figure 7 : Comparison of hydrophilicity of the repair film surface before and after laser surface treatment in a specific embodiment of the present invention;

[0046] Figure 8 : Photos of samples implanted in animal experiments before and after laser surface treatment in a specific embodiment of the present invention;

[0047] Fig. 9 : Photograph of a sample 14 days after implantation in an animal experiment after laser surface treatment in a specific embodiment of the present invention;

[0048] Fig.10 : Photograph of a sample 4 days after implantation in an animal experiment before laser surface treatment in a specific embodiment of the present invention.

[0049] Fig.11 : Schematic diagram of the structure of the repair film in a specific embodiment of the present invention (A: modified layer, B: substrate layer)

[0050] Fig.12 : Schematic diagram of suture removal observation 7 days after surgery in one specific embodiment of the present invention. DETAILED DESCRIPTION

[0051] The following describes the embodiments of the present invention, but the present invention is not limited thereto. The present invention is not limited to the various structures described below, and various changes can be made within the scope of the invention claim, and the embodiments and embodiments obtained by appropriately combining the technical means disclosed in different embodiments and embodiments are also included in the technical scope of the present invention. In addition, all the documents recorded in this specification are cited in this specification as references.

[0052] Unless defined otherwise, technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0053] In this specification, the numerical range expressed using "numerical value A to numerical value B" or "numerical value A-numerical value B" means a range including the endpoints numerical values ​​A and B.

[0054] In this specification, the meaning of "may" includes both the meaning of performing a certain process and the meaning of not performing a certain process. In this specification, "optional" or "optionally" means that the event or situation described below may or may not occur, and the description includes the situation where the event occurs and the situation where the event does not occur.

[0055] In this specification, when "%" appears, it means the percentage by mass or weight, that is, "mass %" or "weight %", unless otherwise specified.

[0056] In this specification, the "average thickness" is obtained by the following method: taking a unit area (e.g. 1 cm 2 ) of a film to be tested, and measure any 10 points in the unit area of ​​the film. The average value of the thickness of the 10 points is the "average thickness".

[0057] In this specification, the use of “substantially” or “essentially” means that the range of industrial error or experimental error is taken into consideration.

[0058] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "some specific / preferred technical solutions", "other specific / preferred technical solutions", etc. refer to the specific elements (e.g., features, structures, properties and / or characteristics) related to the embodiments described herein being included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0059] The term "comprising" and any variations thereof in the specification and claims of the present invention and the above drawings are intended to cover non-exclusive inclusions. For example, a process, method or system, product or device comprising a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.

[0060] <First aspect>

[0061] In a first aspect of the present invention, a repair membrane for repairing human tissue is provided.

[0062] The repair membrane described in the present invention is a fiber membrane, which includes a base layer and at least one modified layer, wherein at least a portion of the modified layer is irradiated with energy lines to produce melting, cross-linking and / or shrinkage; the fiber membrane includes fibers derived from a composition containing natural hydrophilic materials.

[0063] Human tissue

[0064] The human tissue targeted by the present invention is usually tissue that is destroyed, missing or otherwise damaged due to external accidental trauma or surgery, etc. Such tissue can be repaired, treated or healed by using the repair membrane of the present invention.

[0065] Such tissues include but are not limited to the following tissues: skin tissue, bone tissue, cartilage tissue, fat tissue, dense connective tissue, loose connective tissue, muscle tissue and nerve tissue, etc. Therefore, the repair membrane provided by the present invention can be used on the surface of human skin and also can be used inside the human body.

[0066] Fiber raw materials

[0067] The repair membrane of the present invention is a fiber membrane formed by fibers. The raw materials for forming the fibers should generally have good biocompatibility and degradability, and at the same time, the material should be soft but have a certain strength to meet the requirements of fit and support with human tissues.

[0068] Therefore, in some specific embodiments of the present invention, such fiber raw materials may include natural hydrophilic materials, and in addition, preferably also include artificial synthetic materials with degradability, biocompatibility, etc.

[0069] In some specific embodiments of the present invention, the natural hydrophilic material may be selected from hydrophilic colloids, proteins or polysaccharides. In some preferred embodiments, it may be selected from one or more of gelatin, proprotein, human recombinant collagen, cellulose, chondroitin sulfate, chitosan, modified chitosan, fibrin, silk protein, elastin-mimicking peptide polymers, heparin, agar, dextran, alginic acid, modified cellulose, alginic acid, starch, etc., and their modified (e.g., cross-linked, etc.) products.

[0070] There is no particular limitation on the synthetic materials with degradability and biocompatibility, and they can be selected from conventional synthetic materials in the art. In some specific embodiments of the present invention, such materials can be selected from one or more of polylactic acid, polycaprolactone, polyhydroxybutyric acid and valeric acid copolyester, polydioxanone, polyvinyl pyrrolidone, polycaprolactone, polyglycolic acid, polylactic acid-glycolic acid copolymer, 1,3-propylene glycol polymer, polylactic acid-caprolactone copolymer, polyvinyl alcohol, etc. Preferably, the synthetic materials include polyester materials.

[0071] In addition, for the above fiber raw materials, in addition to the above natural hydrophilic materials and artificial synthetic materials, other auxiliary components can also be used without affecting the technical effect of the present invention. There is no special restriction on such components, and they can be selected from:

[0072] i) Inorganic components, for example, nano-metal oxide particles, hydroxyapatite and its modified products, graphene oxide, etc.;

[0073] ii) biologically active ingredients, for example, biological growth factors (including epidermal growth factor, fibroblast growth factor and other ingredients that can promote rapid wound healing and prevent adhesion, etc.) and inorganic ingredients modified by biological activity;

[0074] iii) pharmaceutical ingredients, for example, various antibiotics and other ingredients;

[0075] iv) Auxiliary ingredients, such as dispersants, initiators, crosslinking agents, etc.

[0076] In the present invention, the fiber for the fiber membrane can be prepared by forming a raw material composition by any mixing of the above fiber raw materials. In some specific embodiments of the present invention, such fibers can have substantially the same composition, or in other words, they are fibers processed by fiber materials of the same composition; in other specific embodiments of the present invention, such fibers can also have different compositions, or in other words, the fibers forming the fiber membrane are mixed fibers processed from fiber raw materials of different compositions.

[0077] Furthermore, the composition of the fiber raw material or raw material composition of the present invention can be adjusted according to various practical needs. In a preferred embodiment of the present invention, based on the total mass of the synthetic material and the natural hydrophilic material in the fiber membrane as 100%, the mass ratio of the synthetic material to the natural hydrophilic material in the fiber membrane is 20%:80% to 80%:20%, preferably 30%:70% to 70%:30%, and more preferably 35%:65% to 65%:35%.

[0078] Fiber membrane

[0079] The fiber membrane of the present invention is formed from fibers obtained from the above-mentioned fiber raw material.

[0080] There is no particular limitation on the method of forming the fiber membrane, and the fiber membrane can be formed by nonwoven or woven methods.

[0081] In some preferred embodiments of the present invention, from the perspective of controllability and processability, an electrostatic spinning method is used to obtain the fiber membrane of the present invention.

[0082] The principle of electrospinning is to apply high voltage to the polymer liquid during the electrospinning process to introduce electric charges into the liquid. When the charge in the liquid accumulates to a certain amount, the liquid will form a Taylor cone at the nozzle, and overcome the surface tension under the action of the external electric field force to form a liquid jet. Then, under the combined action of electrostatic repulsion, Coulomb force (Coulomb) and surface tension, the polymer jet moves along an irregular spiral trajectory. The jet is pulled and stretched in a very short time, and as the solvent evaporates or heat dissipates, the polymer jet solidifies to form micron / nano fibers. In the electrospinning process, many parameters will affect the final electrospun fibers. By controlling the process parameters, micron / nano fibers of different sizes, shapes and structures can be prepared.

[0083] In some specific embodiments of the present invention, the electrospinning method mainly includes the following electrospinning film forming steps, solvent removal steps and other subsequent processing steps:

[0084] (Electrospinning Film Forming)

[0085] In the electrospinning membrane forming step, the fiber raw material is mainly mixed with a solvent, and the fiber membrane is obtained by electrospinning.

[0086] Specifically, a fiber raw material is prepared in advance, and the fiber raw material is dissolved in a suitable solvent to prepare a spinning solution of a certain concentration of the fiber raw material.

[0087] There is no particular limitation on the specific concentration of the solvent type used to form the solution, as long as it can meet the requirements of the subsequent electrospinning process. For example, a suitable solvent may be one or a combination of two or more of trifluoroethanol, hexafluoroisopropanol, trifluoroacetic acid, cyclohexanone, acetone, butanone, tetrahydrofuran, chloroform, glacial acetic acid, formic acid, propionic acid or water. In some preferred embodiments of the present invention, a solvent containing fluorine atoms is used from the perspective of solubility and solution viscosity.

[0088] In some specific embodiments of the present invention, in the electrospinning solution containing fiber raw materials, the total mass volume percentage concentration of the artificial material and the natural hydrophilic material in the electrospinning solution is in the range of 5g / 100mL to 10g / 100mL, preferably, in the range of 6g / 100mL to 9g / 100mL.

[0089] The fiber raw materials may be prepared as raw materials with the same composition, or may be prepared as two or more raw materials with different compositions, and each of them may be formed into a raw material liquid.

[0090] Further, there is no special requirement for the electrospinning equipment used in the electrospinning film formation, and the single spinning or co-spinning equipment commonly used in the art can be used. The required (nanoscale) fiber material can be prepared by adjusting the spinning parameters in these equipments during the electrospinning film formation process. For example, voltage, extrusion flow rate, electric field receiving distance, spinning environment, etc. In some specific embodiments, the electrospinning process parameters described in the present invention can be:

[0091] The advancement rate of the feed liquid is 3 to 8 mL / h, preferably 3.5 to 7 mL / h;

[0092] The spinning voltage is 10 to 40 kV, preferably 20 to 40 kV, more preferably 22 to 38 kV, and more preferably 26 to 36 kV;

[0093] The solution extrusion flow rate is 0.1 to 15 mL / h, preferably 0.3 to 10 mL / h;

[0094] The electric field receiving distance is 5 to 30 cm, preferably 10 to 25 cm;

[0095] In addition, there is no particular limitation on the environmental conditions for electrospinning, and they can be adjusted according to actual needs. For example, the relative humidity of the spinning environment can be controlled below 60%, and the environmental temperature can be controlled at 10-40°C.

[0096] The spinning can be stopped when the thickness of the fiber membrane obtained by spinning meets the requirements. For example, the electrospinning can be stopped at any time when the average thickness of the fiber membrane does not exceed 0.5 mm.

[0097] (Solvent Removal)

[0098] After the spinning is stopped, the solvent of the obtained fiber membrane is removed. In some specific embodiments of the present invention, the solvent can be removed by directly heating or freeze-drying the fiber membrane obtained by electrospinning, or by immersing the fiber membrane in an organic solvent and then drying it.

[0099] In some preferred embodiments of the present invention, the fiber membrane containing solvent obtained by electrospinning can be immersed in a solution containing medium- or low-boiling point alcohol substances (such as methanol or ethanol, etc.) (boiling point not exceeding 100°C, preferably not exceeding 90°C) for cleaning to dissolve the solvent contained in the fiber membrane.

[0100] For such a solution, the content of the alcoholic substance is preferably 70% by mass or more, more preferably 80% by mass or more, and more preferably 90% by mass or more, based on the total mass of the solution. After washing, drying is performed to further remove the solution containing the alcoholic substance. Such drying can be performed under heating and / or reduced pressure.

[0101] (Other steps)

[0102] In the present invention, in addition to the above treatments in the electrospinning step, other treatment steps may be used as required.

[0103] For example, the fiber membrane obtained by electrospinning can be cross-linked before or after the solvent removal step as needed to make the fiber membrane material at least partially cross-linked to provide the necessary mechanical properties. In addition, the degree of cross-linking can be adjusted to meet the requirements of the repair membrane service life for different traumas or clinical surgeries. It should be noted that such cross-linking should be controlled below a certain degree of cross-linking so as not to affect the degradability of the fiber membrane.

[0104] It should be noted that the cross-linking treatment or the use of a cross-linking agent in the present invention is not essential, but is merely a means or component that can be selected without affecting the technical effect of the present invention.

[0105] Regarding the cross-linking method, in some specific embodiments of the present invention, after the fiber membrane is obtained through the electrospinning film-forming step, the obtained fiber membrane can be directly heated and dried. Such a method is suitable for the case where the fiber raw material already contains or adds a cross-linking agent and / or an initiator. Usually in such a case, it is advantageous to perform the above-mentioned solvent removal step at the same time as the cross-linking treatment. This is to take into account that the cross-linking agent and / or the initiator may overflow due to the impregnation of alcohol substances in the solvent removal step.

[0106] In some other specific embodiments of the present invention, another method can also be used to complete the cross-linking treatment in the solvent removal step. In this case, the fiber membrane obtained by electrospinning can be immersed in the aforementioned solution containing medium and low boiling point (boiling point not exceeding 100°C, preferably not exceeding 90°C) alcohol substances (such as methanol or ethanol, etc.). In addition, such a solution also contains a cross-linking agent that can cause the fiber membrane to cross-link. Such a cross-linking agent can include one or a combination of more than two of carbodiimide, N-hydroxysuccinimide, genipin, and aldehyde compounds. Further, the cross-linking situation can be controlled by adjusting the reaction conditions of the cross-linking treatment and the amount of the cross-linking agent. For example, the cross-linking treatment temperature, the cross-linking treatment time, the mass ratio of the cross-linking agent to the fiber membrane, the mass ratio of the cross-linking agent to the mass of the above solution, etc. In the present invention, the reaction conditions in such a cross-linking step can be that the cross-linking treatment temperature is between 1 and 50°C, preferably between 4 and 30°C. The cross-linking treatment time is between 1 and 72h, preferably between 6 and 24h. The mass ratio of the chemical crosslinking agent to the fiber raw material in the fiber membrane (or the dry weight of the fiber membrane) is 0.1 to 3:1, preferably 0.5 to 2:1.

[0107] In the present invention, a (dried) fiber membrane is obtained by the method described above, wherein the average diameter of the fibers in the fiber membrane is 0.5 μm to 1.0 μm, preferably 0.6 μm to 1.0 μm.

[0108] Modification of fiber membrane

[0109] Furthermore, at least a portion of the structure of the fiber membrane is isomerized to obtain a modified layer and a matrix layer (hereinafter, for the convenience of description, the modified layer is sometimes represented by layer A and the matrix layer is sometimes represented by layer B). In the present invention, the matrix layer is the portion or layer of the fiber membrane that has not been isomerized.

[0110] In the present invention, for the isomerization treatment, in some specific embodiments, the isomerization treatment can make the fiber membrane modified layer and the substrate layer have at least one of the following conditions i to iv:

[0111] i) the apparent density of the modified layer is higher than the apparent density of the base layer;

[0112] ii) the degree of crosslinking of the modified layer is higher than that of the base layer;

[0113] iii) the mechanical strength of the modified layer is different from (i.e., higher or lower than) the mechanical strength of the base layer;

[0114] iv) The porosity of the modified layer is lower than that of the base layer.

[0115] The isomerization treatment of the present invention can be carried out by energy line irradiation. The energy line can include high energy rays, ultraviolet light or laser. Such energy line irradiation can cause at least part of the irradiated area in the modified layer to produce cladding, crosslinking and / or shrinkage.

[0116] In addition, in each modified layer, based on the total area of ​​the layer, the area subjected to isomerization treatment or irradiated with energy rays is more than 20% of the total area, preferably more than 40%, and more preferably more than 50%; there is no particular restriction on the upper limit of the area subjected to isomerization treatment or irradiated with energy rays, but from the perspective of processability, usability, strength and degradability, it can be less than 80%, preferably less than 70%, and more preferably less than 60%.

[0117] In some specific embodiments of the present invention, the irradiation may be performed on at least one main surface of the fiber membrane, so that at least part of the main surface area of ​​the fiber membrane is isomerized and modified. The modified fiber membrane thus obtained has a structure of layer A / layer B. In addition, both main surfaces of the fiber membrane may be irradiated, so that the modified fiber membrane thus obtained has a structure of layer A / layer B / layer A.

[0118] In some other specific embodiments of the present invention, the A layer / (B layer / A layer) can also be formed in the fiber membrane by irradiation with energy lines. x / B layer / (A layer) y wherein x is an integer greater than 1, preferably 1 to 5, more preferably 1 to 3; and y is 0 or 1.

[0119] Typically, a structure of layer A / layer B / layer A / layer B or layer A / layer B / layer A / layer B / layer A can be formed. Such a method of embedding the modified layer A in the middle of layer B as a base layer can be obtained by processing through an auxiliary energy line irradiation device in the electrospinning film forming step described above.

[0120] Specifically, after the electrospinning reaches a certain set thickness, an energy line irradiation device can be used for irradiation, and the irradiated part is isomerized and modified, and then the electrospinning is continued. In such a process, the irradiation of the energy line is controlled to be as short as possible to avoid affecting the electrospinning process. Further, after the electrospinning film is formed and the subsequent treatment is completed to obtain a fiber membrane, at least one surface of the fiber membrane is irradiated with energy to isomerize at least part of the surface of the fiber membrane.

[0121] In addition, in the present invention, when a fiber membrane modified by isomerization has multiple modified layers A, the properties of these modified layers (at least one of the properties of the modified layers, such as apparent density, degree of crosslinking or mechanical strength) may be the same or different.

[0122] In some preferred embodiments of the present invention, when the modified fiber membrane has a structure of A layer / B layer / A layer, the two A layers have the same properties.

[0123] In some other preferred embodiments of the present invention, when the modified fiber membrane has A layer / (B layer / A layer) x / B layer / (A layer) y When the structure is formed, the layer A on the surface of the fiber membrane has different properties from the layer A inside the fiber membrane. More preferably, the layer A on the surface of the fiber membrane has a higher apparent density or cross-linking degree than the layer A inside the fiber membrane.

[0124] In addition, by irradiation with energy lines, a certain pattern can be formed on the irradiated surface of the fiber membrane. There is no particular limitation on such a pattern, which may include a grid, stripe, staggered or array dot pattern or a combination of these patterns. In some preferred embodiments of the present invention, the pattern includes straight lines staggered horizontally and vertically, and the spacing between two adjacent parallel straight lines is 0.2 mm to 1.0 mm. There is no particular limitation on other auxiliary methods for forming patterns, and a mask or lens may be used when necessary.

[0125] In the present invention, the energy line is preferably a laser for the convenience of operation and the reliability of processing. When the laser is used for irradiation, one or more laser light sources may be provided. The desired pattern is formed by scanning the laser light source, or the pattern may be formed by directly irradiating the arrangement or combination of multiple light sources.

[0126] There is no particular limitation on the laser equipment applicable to the present invention. In order to provide the modified layer with more reliable performance, the ratio between the laser power W and the laser scanning speed V can be controlled within the range of 0.15 to 0.25, preferably within the range of 0.18 to 0.23. If the ratio is too low, there is a concern that the degree of modification of the processed surface is insufficient, and if the ratio is too high, there is a concern that the processed surface may be damaged.

[0127] Further, regarding the thickness of the modified layer and the base layer, in some specific embodiments of the present invention, based on the average thickness of the fiber membrane containing the modified layer as 100%, the average thickness of each modified layer is 10% or less, preferably 8% or less, more preferably 5% or less, and more preferably 3% or less. In addition, the lower limit of the average thickness of each modified layer may be 0.5% or more, preferably 1% or more.

[0128] The final fiber membrane with a modified layer obtained according to the present invention has an average pore size of 0.5μm to 1.5μm, preferably 0.6μm to 1.2μm; the average porosity is less than 85%, preferably 40% to 80%; the average thickness is less than 0.5mm, preferably less than 0.4mm, and more preferably less than 0.35mm. In addition, there is no particular restriction on the lower limit of the average thickness, but from the perspective of repairability and usability when used as a repair membrane, it can be more than 0.05mm, preferably more than 0.1mm.

[0129] <Second Aspect>

[0130] A second aspect of the present invention provides a medical product for repairing human tissue.

[0131] In the present invention, the fiber membrane with the modified layer disclosed in the first aspect above can be directly used as a repair membrane. In addition, other active ingredients, medicinal ingredients, etc. can be compounded or loaded in the repair membrane according to any needs. There is no special limitation on these other ingredients, and they can be used according to actual needs.

[0132] In addition, in some specific embodiments of the present invention, the repair membrane of the present invention can also be compounded with a layer having a supporting function to obtain a laminate. Typically, a woven mesh can be used as a supporting layer. In such a case, the present invention can further provide a laminate, which includes a fiber membrane with a modified layer, a woven mesh and an adhesive layer, wherein the adhesive layer is located between the nanofiber membrane and the woven mesh. The adhesive material includes a hydrophilic substance, the fiber membrane and the woven mesh are combined through the adhesive layer, and the adhesive layer is at least partially embedded in the pores of the fiber membrane and the woven mesh. The hydrophilic substance includes: protein compounds and their derivatives modified by one or more of carbodiimide, carbodiimide / N-hydroxysuccinimide, genipin, and aldehyde compounds, cellulose compounds and their derivatives modified by aldehyde compounds, chitosan compounds and their derivatives modified by propylene glycol and water; the peel strength between the fiber membrane and the woven mesh is 20 to 75 cN / mm; the breaking strength of the composite tissue repair patch is 8 to 12.5 MPa; the distance between the nanofiber membrane and the woven mesh is 0.1 to 3 mm.

[0133] In some other specific embodiments of the present invention, the repair film of the present invention can also be compounded with a peelable layer to obtain a laminate. There is no particular limitation on the material of the peelable layer, and conventional thermoplastic resins, especially polyolefin resins and polyester resins, can be used. The peelable layer can be electrostatically bonded to the repair film of the present invention; in addition, an adhesive can be coated on the side where the peelable layer is bonded to the repair film of the present invention.

[0134] Example

[0135] The present invention will be further described below through specific embodiments.

[0136] Example 1

[0137] (1) dissolving gelatin and PLLA in a certain volume of hexafluoroisopropanol solvent at a mass ratio of 1:3, so that the total mass volume percentage concentration of gelatin and PLLA is 8 g / 100 mL;

[0138] (2) The polymer solution is loaded into an electrospinning syringe, the rate of the microinjection pump is adjusted to 5 ml / h, the voltage difference of the high-voltage generator is adjusted to 30 kV, and the receiving distance of the receiving device is adjusted to 20 cm. A fiber membrane with a tangled cross is prepared by electrospinning. When the thickness of the fiber membrane reaches 0.15 mm, the electrospinning is turned off and the fiber membrane is removed;

[0139] (3) The electrospun fiber membrane material was repeatedly soaked in a 95% ethanol solution to remove the hexafluoroisopropanol, and then dried. Figure 7 Sample before laser surface treatment.

[0140] (4) The dried film material is placed flat on the laser cutting equipment (Laser Tools & Technics Coporation, ILS IIINM-25W) platform for laser surface treatment. The laser power is set to 22%, the laser speed is 100%, that is, the ratio of laser power to laser scanning speed is 0.22, and the scanning CAD graphics is set to a horizontal and vertical staggered running track with a spacing of 0.5 mm. The laser surface treatment of the film surface is as follows Figure 7 The sample after laser surface treatment. The microscope picture of the sample is as follows Figure 1 to Figure 4 As shown, the SEM images are as follows Figure 5-Figure 6 As shown in the figure, the average pore size of the sample after laser surface treatment is 0.86 μm, the average fiber diameter is 0.74 μm, and the average porosity is 66.30%.

[0141] The hydrophilicity and hydrophobicity of the membrane surface after surface treatment have changed significantly, such as Figure 7As shown. It can significantly slow down the swelling effect of liquid.

[0142] (5) The samples before and after laser surface treatment were irradiated and sterilized, and then used to repair the mandibular defect animal model after tooth extraction.

[0143] That is, the beagle dogs were fasted for 12 hours before the operation, and anesthetized with 3% sodium pentobarbital at 1 ml / kg intravenous injection. After anesthesia, the hair around the mandibular operation site was removed. The inside of the mouth and the surrounding skin were disinfected with iodine and covered with a towel. The gingival flaps around the 1st, 2nd, 3rd, and 4th premolars were separated to ensure the integrity of the periosteum, and the 1st, 2nd, 3rd, and 4th premolars on both sides of the mandible were removed. Then the gingival flaps were re-sutured, and the animals were returned to the breeding room for observation and feeding after they woke up. The animals were injected with antibiotics 3 days after the operation to prevent infection.

[0144] To prevent gingival cracking at the suture site, the animals were fed liquid food for the first 15 days after surgery, and healing assessments were performed weekly until complete healing. Three months after tooth extraction, an animal model of mandibular defect was made. The specific operation was as follows: incise from the lateral side of the mandible, and use a gingival separator to separate the buccal gingiva at the extraction site to the alveolar ridge to ensure the integrity of the periosteum. Use a dental drill to create two three-wall box-shaped defects at the left and right extraction sites (cooling with a large amount of saline while grinding). The two defects are 5 mm apart. The inferior alveolar nerve and blood vessels are not damaged during the operation. The length, width, and height of the defect are 9 mm × 5 mm × 7 mm. Place bone powder mixed with autologous blood in the extraction socket and squeeze it appropriately so that the height of the bone powder is flush with the defect surface. Cover the laser surface treated repair membrane sample on top of the bone powder and fix it with bone screws at the four corners. Then suture the gums, such as Figure 8 After 14 days of postoperative anatomy, the material did not swell, fall off or shift. Soft tissue growth was visible on the membrane and the gums began to heal. Fig. 9 As shown in the figure. However, the sample before laser treatment showed swelling, displacement and exposure of the membrane material on the 4th day after implantation, as shown in the figure. Fig.10 shown.

[0145] Example 2

[0146] (1) dissolving gelatin and PLLA in a certain volume of hexafluoroisopropanol solvent at a mass ratio of 7:3, so that the total mass volume percentage concentration of gelatin and PLLA is 8 g / 100 mL;

[0147] (2) The polymer solution is loaded into an electrospinning syringe, the rate of the microinjection pump is adjusted to 6 ml / h, the voltage difference of the high-voltage generator is adjusted to 30 kV, and the receiving distance of the receiving device is adjusted to 22 cm. A fiber membrane with a tangled cross is prepared by electrospinning. When the thickness of the fiber membrane reaches 0.2 mm, the electrospinning is turned off and the fiber membrane is removed;

[0148] (3) The electrospun fiber membrane material is repeatedly immersed in a 95% ethanol solution to remove the hexafluoroisopropanol, and then dried to prepare a sample before laser surface treatment.

[0149] (4) Place the dried membrane material flat on the laser cutting equipment (Laser Tools & Technics Coporation, ILS IIINM-25W) platform for laser surface treatment. Set the laser power to 18% and the laser speed to 100%, that is, the ratio of laser power to laser speed is 0.18: Set the scanning CAD graphics to a horizontal and vertical staggered running track with a spacing of 0.2 mm. Perform laser surface treatment on the surface of the membrane material to obtain the sample after laser surface treatment. The average pore size of the sample after laser surface treatment is tested to be 0.63μm, the average fiber diameter is 0.61μm, and the average porosity is 73.1%

[0150] (5) The samples before and after laser surface treatment were irradiated and sterilized, and then used to repair the mandibular defect animal model after tooth extraction.

[0151] That is, the beagle dogs were fasted for 12 hours before the operation, and anesthetized with 3% sodium pentobarbital at 1 ml / kg intravenous injection. After anesthesia, the hair around the mandibular operation site was removed. The inside of the mouth and the surrounding skin were disinfected with iodine and covered with a towel. The gingival flaps around the 1st, 2nd, 3rd, and 4th premolars were separated to ensure the integrity of the periosteum, and the 1st, 2nd, 3rd, and 4th premolars on both sides of the mandible were removed. Then the gingival flaps were re-sutured, and the animals were returned to the breeding room for observation and feeding after they woke up. The animals were injected with antibiotics 3 days after the operation to prevent infection.

[0152] To prevent gingival cracking at the suture site, the animals were fed with liquid food for the first 15 days after surgery, and healing assessments were performed weekly until complete healing. Three months after tooth extraction, an animal model of mandibular defect was made. The specific operation was as follows: incision was made from the lateral side of the mandible, and a gingival separator was used to separate the buccal gingiva at the extraction site to the alveolar ridge to ensure the integrity of the periosteum. Two three-wall box-shaped defects were made at the left and right extraction sites using a dental drill (cooled with a large amount of saline while grinding). The two defects were 5 mm apart. The inferior alveolar nerve and blood vessels were not damaged during the operation. The length, width, and height of the defect were 9 mm × 5 mm × 7 mm. Bone powder mixed with autologous blood was placed in the extraction socket, and it was squeezed appropriately to make the height of the bone powder flush with the defect surface. The laser surface-treated repair membrane sample was covered on top of the bone powder, and bone screws were nailed on the four corners to fix it. Then the gingiva was sutured. The sutures were removed 7 days after surgery to observe that there was no exposure, shedding, or displacement of the material, and the gingiva healed well. See, Fig.12 .

[0153] Example 3

[0154] (1) dissolving gelatin and PLLA in a certain volume of hexafluoroisopropanol solvent at a mass ratio of 2:5, so that the total mass volume percentage concentration of gelatin and PLLA is 8 g / 100 mL;

[0155] (2) The polymer solution is loaded into an electrospinning syringe, the rate of the microinjection pump is adjusted to 6 ml / h, the voltage difference of the high-voltage generator is adjusted to 30 kV, and the receiving distance of the receiving device is adjusted to 22 cm. A fiber membrane with a tangled cross is prepared by electrospinning. When the thickness of the fiber membrane reaches 0.3 mm, the electrospinning is turned off and the fiber membrane is removed;

[0156] (3) The electrospun fiber membrane material was repeatedly immersed in a 95% ethanol solution to remove the hexafluoroisopropanol, and then dried to prepare a sample before laser surface treatment.

[0157] (4) Place the dried membrane material flat on the laser cutting equipment (Laser Tools & Technics Coporation, ILS IIINM-25W) platform for laser surface treatment. Set the laser power to 20% and the laser speed to 100%, that is, the ratio of laser power to laser speed is 0.20: Set the scanning CAD graphics to a horizontal and vertical staggered running track with a spacing of 0.3mm. Perform laser surface treatment on the surface of the membrane material to obtain the sample after laser surface treatment. The average pore size of the sample after laser surface treatment is tested to be 0.75μm, the average fiber diameter is 0.68μm, and the average porosity is 75.3%

[0158] (5) The samples before and after laser surface treatment were irradiated and sterilized, and then used to repair the mandibular defect animal model after tooth extraction.

[0159] That is, the beagle dogs were fasted for 12 hours before the operation, and anesthetized with 3% sodium pentobarbital at 1 ml / kg intravenous injection. After anesthesia, the hair around the mandibular operation site was removed. The inside of the mouth and the surrounding skin were disinfected with iodine and covered with a towel. The gingival flaps around the 1st, 2nd, 3rd, and 4th premolars were separated to ensure the integrity of the periosteum, and the 1st, 2nd, 3rd, and 4th premolars on both sides of the mandible were removed. Then the gingival flaps were re-sutured, and the animals were returned to the breeding room for observation and feeding after they woke up. The animals were injected with antibiotics 3 days after the operation to prevent infection.

[0160] To prevent gingival cracking at the suture site, the animals were fed with liquid food for the first 15 days after surgery, and healing assessment was performed weekly until complete healing. Three months after tooth extraction, an animal model of mandibular defect was made. The specific operation was as follows: incision was made from the outer side of the mandible, and the buccal gingiva at the extraction site was separated to the alveolar ridge with a gingival separator to ensure the integrity of the periosteum. Two three-wall box-shaped defects were made at the left and right extraction sites with a dental drill (cooled with a large amount of saline while grinding). The two defects were 5 mm apart. The inferior alveolar nerve and blood vessels were not damaged during the operation. The length, width and height of the defect were 9 mm × 5 mm × 7 mm. Bone powder mixed with autologous blood was placed in the extraction socket, and it was squeezed appropriately to make the height of the bone powder flush with the defect surface. The laser surface treated repair membrane sample was covered on the bone powder, and bone screws were fixed on the four corners. Then the gingiva was sutured. The sutures were removed 14 days after surgery to observe that there was no exposure, shedding or displacement of the material, and the gingiva healed well.

[0161] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present disclosure should not be limited thereto.

[0162] The embodiments of the present disclosure have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

[0163] Industrial Applicability

[0164] The fiber membrane-based tissue repair membrane provided by the present invention can be prepared and used industrially as a medical repair product.

Claims

1. A tissue repair membrane, characterized in that: The repair membrane is a fiber membrane. The fiber membrane comprises a matrix layer and at least one modified layer, wherein the modified layer is obtained by isomerizing at least a part of the structure of the fiber membrane, the layer in the fiber membrane that has not been isomerized is the matrix layer, and the isomerization modification treatment is performed by energy line irradiation; Wherein, at least a part of the modified layer is irradiated with energy rays to produce cladding, cross-linking and / or shrinkage, and the modified layer is formed into a certain pattern in the region irradiated with energy rays; The fiber membrane includes fibers derived from a composition containing natural hydrophilic materials, and the composition containing natural hydrophilic materials also includes artificial synthetic materials. The natural hydrophilic materials are selected from one or more of hydrophilic colloids, proteins, and polysaccharides.

2. The repair film according to claim 1, characterized in that The modified layer is present in at least one main surface of the fiber membrane or the modified layer forms at least one main surface of the fiber membrane.

3. The repair film according to claim 1 or 2, characterized in that: Based on 100% of the average thickness of the fiber membrane, the average thickness of each modified layer is less than 10%.

4. The repair film according to claim 1 or 2, characterized in that: A stripe-shaped, staggered or array dot-shaped pattern or a combination of these patterns is formed in the area of ​​the modified layer of the fiber membrane that is irradiated by the energy line.

5. The repair film according to claim 1 or 2, characterized in that: The energy line includes a flow of energy particles.

6. The repair film according to claim 1 or 2, characterized in that: The energy line is a laser, and the ratio between the laser power W and the laser scanning speed V is 0.15 to 0.

25.

7. The repair film according to claim 1 or 2, characterized in that: The average thickness of the fiber membrane is less than 0.5 mm.

8. The repair film according to claim 1 or 2, characterized in that: The average thickness of the fiber membrane is 0.1 mm to 0.3 mm.

9. The repair film according to claim 1 or 2, characterized in that: The average porosity of the fiber membrane is less than 85%.

10. The repair film according to claim 1 or 2, characterized in that: The average porosity of the fiber membrane is 40% to 80%.

11. The repair film according to claim 1, characterized in that: The natural hydrophilic material in the composition containing natural hydrophilic materials is selected from one or more of gelatin, collagen and polysaccharides, and the artificial synthetic material includes one or more of polyester materials.

12. The repair film according to claim 1, characterized in that: The mass ratio between the artificial synthetic material and the natural hydrophilic material is (20%:80%) to (80%:20%).

13. A laminate for tissue repair, characterized in that: At least one layer in the laminate includes the tissue repair membrane according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Fiber membranes for tissue repair, their preparation methods and applications, and products for tissue repair

    CN106492272B

  • Chitosan-based nerve fiber membrane, preparation method, nerve conduit and application

    CN111632193A

  • Pelvic floor repairing sheet

    CN103800942A

  • Functional guidance muscle tissue repair membrane and preparation method and application thereof

    CN110404117A

  • Soft tissue repair patch and preparation method thereof, and tension-free hanging belt system

    WO2016107522A1