A method for preparing a multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber
Through the coextruded composite material process and hierarchical structure design, the poor dyeing and adhesive residue of ultra-high molecular weight polyethylene fiber multi-layer composite boards are solved, which improves the sound insulation performance and safety of the boards and improves the health of the working environment. .
Patent Information
- Application Number
- CN202210386743.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-04-14
AI Technical Summary
The existing multi-layer composite sheets based on ultra-high molecular weight polyethylene fibers have poor dyeing properties and adhesive residual solvent problems, which affect the quality of the board and the health of the working environment.
By using the coextruded composite material process, by setting up a fiber-reinforced thermoplastic composite material layer and a polyurethane elastic layer, the ultra-high molecular weight polyethylene fiber reinforced resin layer is wrapped to form a box-shaped and honeycomb-shaped structure, reducing the use of adhesives, and improving the use of glass fiber layers. Deformation resistance and impact resistance.
It solves the problem of poor dyeing, avoids adhesive residue, improves the sound insulation performance and safety of composite boards, and improves the health of the working environment.
Smart Images

Figure CN114683624B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite plates, and in particular to a method for preparing a multi-layer composite plate based on ultra-high molecular weight polyethylene fibers. Background Art
[0002] Ultra-high molecular weight polyethylene fiber, referred to as UHMWPE fiber, is also called high-strength high-modulus polyethylene fiber. It is an unbranched linear polyethylene with a molecular weight of more than 1.5 million. It is collectively known as the "three major high-tech fibers in the world" with carbon fiber and aramid. It is a fiber made by spinning and high-multiple drafting of polyethylene with a molecular weight of more than 1 million. It has excellent mechanical properties. Its density is only two-thirds of aramid fiber and one-half of high-modulus carbon fiber. It also has excellent impact resistance, excellent chemical corrosion resistance and good electrical insulation. It is widely used in important departments such as aerospace and military industry. Composite sheets made of ultra-high molecular weight polyethylene fiber have been used in aircraft interiors, train exterior body covers, architectural decoration, furniture surface coatings, special packaging box shells, etc. in recent years. It is characterized by high strength, good toughness, environmental protection and recyclability, and has a wide range of application prospects in industrial and civil fields.
[0003] Composite sheets made of fiber-reinforced thermoplastic composite materials and ultra-high molecular weight polyethylene fibers have good molding properties, such as a Chinese invention with authorization announcement number CN108407421A, which proposes a lightweight, high-impact, high-modulus multi-layer composite sheet that is easy to heat-form and a preparation method thereof, including a composite sheet body; the composite sheet body is composed of a composite layer sheet of a two-layer or multi-layer structure; the present invention combines a lightweight, impact-resistant ultra-high molecular weight polyethylene layer with a high-modulus fiber-reinforced thermoplastic composite material, and can prepare large-sized sheet products by hot pressing; the composite sheet has both the high strength and high impact resistance of ultra-high molecular weight polyethylene and the lightweight and high modulus characteristics of rigid fiber-reinforced composite materials; at the same time, because the rigid fibers used are short-cut or long fibers, they have good molding properties under heating and pressurization conditions;
[0004] However, the existing multi-layer composite sheets based on ultra-high molecular weight polyethylene fibers still have the following problems:
[0005] There is no dye gene on the ultra-high molecular weight polyethylene fiber, and its wettability is poor. It is difficult for the dye to penetrate into the fiber, resulting in poor dyeability. The ultra-high molecular weight polyethylene fiber layer in most composite boards is exposed to the outside, making the ultra-high molecular weight polyethylene fiber layer inconsistent with other layers in color, affecting the quality of the board;
[0006] When making multi-layer composite boards, adhesives need to be set in each layer. The use of adhesives results in residual solvents when the boards are made, and there is odor in the working environment, which affects the health of the workers. Therefore, we propose a preparation method for a multi-layer composite board based on ultra-high molecular weight polyethylene fiber to solve the above problems. Summary of the invention
[0007] The object of the present invention is to provide a method for preparing a multi-layer composite sheet material based on ultra-high molecular weight polyethylene fiber, so as to solve the problem of the existing multi-layer composite sheet material based on ultra-high molecular weight polyethylene fiber proposed in the above-mentioned background technology, that there is no dye gene on the ultra-high molecular weight polyethylene fiber, and its wettability is poor, and it is difficult for the dye to penetrate into the fiber, resulting in poor dyeability. The ultra-high molecular weight polyethylene fiber layer in most composite sheets is exposed to the outside world, so that the color of the ultra-high molecular weight polyethylene fiber layer is inconsistent with that of other layers, affecting the quality of the sheet material. When making the multi-layer composite sheet material, it is necessary to set an adhesive in each layer. The use of the adhesive causes residual solvent to exist when the sheet material is made, and there is odor in the working environment, which affects the health of the staff.
[0008] To achieve the above-mentioned object, the present invention provides the following technical scheme: a method for preparing a multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber, wherein the multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber comprises a multi-layer composite sheet body, wherein the multi-layer composite sheet body comprises a first outer layer, an inner layer, a second outer layer, a glass fiber layer and a polyurethane elastic layer, wherein the first outer layer and the second outer layer are both fiber-reinforced thermoplastic composite material layers, and the inner layer is an ultra-high molecular weight polyethylene fiber-reinforced resin layer;
[0009] The preparation method of the multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber is as follows:
[0010] Step 1: Place the sheet metal mold on the processing platform and use a level to check the flatness of the mold.
[0011] Step 2: Put the fiber reinforced thermoplastic composite material, the processing aid and the dye into a mixer and stir them so that the fiber reinforced thermoplastic composite material, the processing aid and the dye are fully mixed, and then put the mixed material into a melting device to form a molten state, and then put the molten fiber reinforced thermoplastic composite material into an extruder;
[0012] Step 3: Put the ultra-high molecular weight polyethylene raw material, the internal modified organic nano-phosphate and the antioxidant into a mixer and mix them thoroughly, then add them into a twin-screw extruder for mixing and granulation to obtain a modified masterbatch;
[0013] Step 4: The modified masterbatch ultra-high molecular weight polyethylene and the external modifier fluoroelastomer are fully mixed in a high-speed mixer, and then added to a twin-screw extruder for melt spinning, and the nascent fibers are obtained by cooling in a water bath, and then the nascent fibers are stretched, and the stretched ultra-high molecular weight polyethylene fibers are put into a melting device to form a molten state, and then the molten ultra-high molecular weight polyethylene fibers are put into an extruder;
[0014] Step 5: Put the glass fiber raw material into the melting equipment for heating, and then put it into the extruder;
[0015] Step 6: Put the polyurethane elastic raw material into the melting device for heating, and then put it into the extruder;
[0016] Step 7: The molten fiber-reinforced thermoplastic composite material is put into the mold through an extruder. After the amount of the fiber-reinforced thermoplastic composite material put into the mold reaches the requirement, the first outer layer of the box-shaped structure is formed;
[0017] Step 8: Putting molten glass fiber into the first outer layer through an extruder, then putting molten polyurethane elastic material, and then putting molten ultra-high molecular weight polyethylene fiber into the fiber-reinforced thermoplastic composite material with a box-shaped structure through an extruder to form an inner layer with a honeycomb structure, and then putting molten polyurethane elastic material and molten glass fiber in sequence;
[0018] Step 9: Then, a molten fiber-reinforced thermoplastic composite material is placed on the outside of the glass fiber, and the fiber-reinforced thermoplastic composite material is laid on the glass fiber to form a second outer layer;
[0019] Step 10: Turn off the heating function of the mold, and then cool the mold through a cooling device to form a multi-layer composite board body consisting of the first outer layer, the inner layer, the second outer layer, the glass fiber layer and the polyurethane elastic layer.
[0020] Preferably, the first outer layer is in a box-shaped structure, and the outer side surface of the inner layer is in contact with the inner side surface of the first outer layer.
[0021] Preferably, the length and width of the first outer layer are equal to the length and width of the second outer layer.
[0022] Preferably, when the first outer layer, the inner layer, the second outer layer, the glass fiber layer and the polyurethane elastic layer are placed in the mold, a vibration device is arranged outside the mold, and the vibration device slightly vibrates the mold to shake out the air in the material.
[0023] Compared with the prior art, the invention has the following beneficial effects: the method for preparing the multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber solves the problem that the inner layer composed of ultra-high molecular weight polyethylene fiber reinforced resin has poor dyeability and the inner layer is not colored, and is manufactured by the process of co-extrusion composite materials. No adhesive is required between the layers of the multi-layer composite sheet, so there is no residual solvent and no odor;
[0024] 1. A first outer layer and a second outer layer are provided, both of which are fiber-reinforced thermoplastic composite material layers, and the fiber-reinforced thermoplastic composite material is mixed with a dye to produce the required color. The first outer layer and the second outer layer of the box-shaped structure wrap the inner layer, so as to solve the problem of poor dyeability of the inner layer composed of ultra-high molecular weight polyethylene fiber-reinforced resin;
[0025] 2. A first outer layer, an inner layer and a second outer layer are provided. When the first outer layer, the inner layer and the second outer layer are manufactured, the first outer layer, the inner layer and the second outer layer are manufactured by using a co-extrusion composite material process. A fiber-reinforced thermoplastic composite material, an ultra-high molecular weight polyethylene fiber-reinforced resin and a fiber-reinforced thermoplastic composite material are sequentially fed into a mold by an extruder, and the molded material is formed after cooling, so that no adhesive is required between layers of the multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber, so there is no residual solvent and no odor, and the ultra-high molecular weight polyethylene fiber of the inner layer has a honeycomb structure, thereby improving the sound insulation performance of the composite sheet;
[0026] 3. A glass fiber layer and a polyurethane elastic layer are provided, and the glass fiber layer and the polyurethane elastic layer are provided above and below the inner layer, and the glass fiber layer and the polyurethane elastic layer are located on the inner side of the first outer layer and the second outer layer. The glass fiber layer is used to improve the deformation resistance of the composite board, and the polyurethane elastic layer is used to increase the impact resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the overall structure of the present invention;
[0028] Figure 2 It is a schematic diagram of the front view cutaway structure of the present invention;
[0029] Figure 3 It is a schematic diagram of the overall structure of the inner layer and the first outer layer connected to each other in the present invention.
[0030] In the figure: 1. multi-layer composite board body; 2. first outer layer; 3. inner layer; 4. second outer layer; 5. glass fiber layer; 6. polyurethane elastic layer. DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] See also Figure 1-3 The present invention provides a technical solution: a method for preparing a multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber, wherein the multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber comprises a multi-layer composite sheet body 1, wherein the multi-layer composite sheet body 1 is composed of a first outer layer 2, an inner layer 3, a second outer layer 4, a glass fiber layer 5 and a polyurethane elastic layer 6, wherein the first outer layer 2 and the second outer layer 4 are both fiber-reinforced thermoplastic composite material layers, and the inner layer 3 is an ultra-high molecular weight polyethylene fiber-reinforced resin layer;
[0033] The preparation method of the multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber is as follows:
[0034] Step 1: Place the sheet metal mold on the processing platform and use a level to check the flatness of the mold.
[0035] Step 2: Put the fiber reinforced thermoplastic composite material, the processing aid and the dye into a mixer and stir them so that the fiber reinforced thermoplastic composite material, the processing aid and the dye are fully mixed, and then put the mixed material into a melting device to form a molten state, and then put the molten fiber reinforced thermoplastic composite material into an extruder;
[0036] Step 3: Put the ultra-high molecular weight polyethylene raw material, the internal modified organic nano-phosphate and the antioxidant into a mixer and mix them thoroughly, then add them into a twin-screw extruder for mixing and granulation to obtain a modified masterbatch;
[0037] Step 4: The modified masterbatch ultra-high molecular weight polyethylene and the external modifier fluoroelastomer are fully mixed in a high-speed mixer, and then added to a twin-screw extruder for melt spinning, and the nascent fibers are obtained by cooling in a water bath, and then the nascent fibers are stretched, and the stretched ultra-high molecular weight polyethylene fibers are put into a melting device to form a molten state, and then the molten ultra-high molecular weight polyethylene fibers are put into an extruder;
[0038] Step 5: Put the glass fiber raw material into the melting equipment for heating, and then put it into the extruder;
[0039] Step 6: Put the polyurethane elastic raw material into the melting device for heating, and then put it into the extruder;
[0040] Step 7: The molten fiber-reinforced thermoplastic composite material is put into the mold through an extruder. After the amount of the fiber-reinforced thermoplastic composite material put into the mold reaches the requirement, a first outer layer 2 of the box-shaped structure is formed;
[0041] Step 8: Put the molten glass fiber into the first outer layer 2 through an extruder, then put the molten polyurethane elastic material, and then put the molten ultra-high molecular weight polyethylene fiber into the fiber-reinforced thermoplastic composite material with a box-shaped structure through an extruder to form an inner layer 3 with a honeycomb structure inside, and then put the molten polyurethane elastic material and the molten glass fiber in sequence;
[0042] Step nine: Then, a molten fiber-reinforced thermoplastic composite material is placed on the outside of the glass fiber, and the fiber-reinforced thermoplastic composite material is laid on the glass fiber to form a second outer layer 4;
[0043] Step 10: Turn off the heating function of the mold, and then cool the mold by a cooling device, so that the multi-layer composite board body 1 composed of the first outer layer 2, the inner layer 3, the second outer layer 4, the glass fiber layer 5 and the polyurethane elastic layer 6 is formed;
[0044] The first outer layer 2 is a box-shaped structure, and the outer side of the inner layer 3 is in contact with the inner side of the first outer layer 2. The first outer layer 2 and the second outer layer 4 are used to wrap the material. The length and width of the first outer layer 2 are equal to the length and width of the second outer layer 4. When the first outer layer 2, the inner layer 3, the second outer layer 4, the glass fiber layer 5 and the polyurethane elastic layer 6 are placed in the mold, a vibration device is arranged outside the mold. The vibration device slightly vibrates the mold to shake out the air in the material, thereby improving the quality of the board.
[0045] During processing, place the sheet metal mold on the processing platform and use a level to check the flatness of the mold.
[0046] The fiber-reinforced thermoplastic composite material, the processing aid and the dye are put into a mixer and stirred to fully mix the fiber-reinforced thermoplastic composite material, the processing aid and the dye, and then the mixed material is put into a melting device to form a molten state, and then the molten fiber-reinforced thermoplastic composite material is put into an extruder;
[0047] The ultra-high molecular weight polyethylene raw material, the internal modified organic nano-phosphate and the antioxidant are put into a mixer and fully mixed, and then added into a twin-screw extruder for mixing and granulation to obtain a modified masterbatch;
[0048] The modified master batch ultra-high molecular weight polyethylene and the external modifier fluoroelastomer are fully mixed in a high-speed mixer, and then added into a twin-screw extruder for melt spinning, and the nascent fibers are obtained by cooling in a water bath, and then the nascent fibers are stretched, and the stretched ultra-high molecular weight polyethylene fibers are put into a melting device to form a molten state, and then the molten ultra-high molecular weight polyethylene fibers are put into an extruder;
[0049] The glass fiber raw material is put into a melting device for heating, and then put into an extruder, and the polyurethane elastic raw material is put into a melting device for heating, and then put into an extruder;
[0050] The molten fiber-reinforced thermoplastic composite material is fed into the mold by an extruder, and after the amount of the fiber-reinforced thermoplastic composite material fed into the mold reaches the requirement, a first outer layer 2 of the box-shaped structure is formed;
[0051] The molten glass fiber is put into the first outer layer 2 through an extruder, and then the molten polyurethane elastic material is put, and then the molten ultra-high molecular weight polyethylene fiber is put into the fiber-reinforced thermoplastic composite material with a box-shaped structure through an extruder to form an inner layer 3 with a honeycomb structure inside, and then the molten polyurethane elastic material and the molten glass fiber are put in sequence, and then the molten fiber-reinforced thermoplastic composite material is put on the outer side of the glass fiber, and the fiber-reinforced thermoplastic composite material is laid on the glass fiber to form a second outer layer 4. When putting, the vibration structure on the side is opened to vibrate the mold to shake out the gas in the material;
[0052] Then turn off the heating function of the mold, and then cool the mold through a cooling device to form a multilayer composite board body 1 composed of a first outer layer 2, an inner layer 3, a second outer layer 4, a glass fiber layer 5 and a polyurethane elastic layer 6. The above completes a series of operations of the preparation method of the multilayer composite board based on ultra-high molecular weight polyethylene fiber. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0053] The standard parts used in the present invention can all be purchased from the market, and special-shaped parts can be customized according to the instructions and the drawings. The specific connection methods of each part adopt conventional means such as mature bolts, rivets, welding, etc. in the prior art. Machinery, parts and equipment all adopt conventional models in the prior art, and the circuit connection adopts the conventional connection method in the prior art, which will not be described in detail here.
[0054] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber, characterized in that: The multi-layer composite sheet based on ultra-high molecular weight polyethylene fibers comprises a multi-layer composite sheet body (1), wherein the multi-layer composite sheet body (1) is composed of a first outer layer (2), an inner layer (3), a second outer layer (4), a glass fiber layer (5) and a polyurethane elastic layer (6), wherein the first outer layer (2) and the second outer layer (4) are both fiber-reinforced thermoplastic composite material layers, and the inner layer (3) is an ultra-high molecular weight polyethylene fiber-reinforced resin layer; The preparation method of the multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber is as follows: Step 1: Place the sheet metal mold on the processing platform and use a level to check the flatness of the mold. Step 2: Put the fiber reinforced thermoplastic composite material, the processing aid and the dye into a mixer and stir them so that the fiber reinforced thermoplastic composite material, the processing aid and the dye are fully mixed, and then put the mixed material into a melting device to form a molten state, and then put the molten fiber reinforced thermoplastic composite material into an extruder; Step 3: Put the ultra-high molecular weight polyethylene raw material, the internal modified organic nano-phosphate and the antioxidant into a mixer and mix them thoroughly, then add them into a twin-screw extruder for mixing and granulation to obtain a modified masterbatch; Step 4: The modified masterbatch ultra-high molecular weight polyethylene and the external modifier fluoroelastomer are fully mixed in a high-speed mixer, and then added to a twin-screw extruder for melt spinning, and the nascent fibers are obtained by cooling in a water bath, and then the nascent fibers are stretched, and the stretched ultra-high molecular weight polyethylene fibers are put into a melting device to form a molten state, and then the molten ultra-high molecular weight polyethylene fibers are put into an extruder; Step 5: Put the glass fiber raw material into the melting equipment for heating, and then put it into the extruder; Step 6: Put the polyurethane elastic raw material into the melting device for heating, and then put it into the extruder; Step 7: injecting the molten fiber-reinforced thermoplastic composite material into the mold through an extruder, and after the amount of the fiber-reinforced thermoplastic composite material injected into the mold reaches the required amount, a first outer layer (2) of the box-shaped structure is formed; Step 8: injecting molten glass fibers into the first outer layer (2) through an extruder, and then injecting molten polyurethane elastic material, and then injecting molten ultra-high molecular weight polyethylene fibers into the fiber-reinforced thermoplastic composite material with a box-shaped structure through an extruder to form an inner layer (3) with a honeycomb structure, and then injecting molten polyurethane elastic material and molten glass fibers in sequence; Step 9: Then, a molten fiber-reinforced thermoplastic composite material is placed on the outside of the glass fiber, and the fiber-reinforced thermoplastic composite material is laid on the glass fiber to form a second outer layer (4); Step 10: Turn off the heating function of the mold, and then cool the mold through a cooling device, so that the multi-layer composite board body (1) composed of the first outer layer (2), the inner layer (3), the second outer layer (4), the glass fiber layer (5) and the polyurethane elastic layer (6) is formed.
2. The method for preparing a multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: The first outer layer (2) is in a box-shaped structure, and the outer side surface of the inner layer (3) is in contact with the inner side surface of the first outer layer (2).
3. The method for preparing a multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: The length and width of the first outer layer (2) are equal to the length and width of the second outer layer (4).
4. The method for preparing a multi-layer composite sheet based on ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that: When the first outer layer (2), the inner layer (3), the second outer layer (4), the glass fiber layer (5) and the polyurethane elastic layer (6) are placed in the mold, a vibration device is arranged outside the mold, and the vibration device lightly vibrates the mold to shake out the air in the material.
Citation Information
Patent Citations
Lightweight high-impact-resistance high-modulus multilayer composite board easy in thermal forming and preparation method thereof
CN108407421A
Ultrahigh molecular weight polyethylene / continuous fiber reinforced thermoplastic plastic composite board, and preparation method thereof
CN105328954A
Lightweight high-strength travel luggage shell body structure and manufacturing technology thereof
CN108656666A
Shellproof panel of ultra high molecular weight polyethylene
CN206291788U