Circuit connection adhesive film
By incorporating two adhesive layers with different coefficients of linear expansion in the circuit connection adhesive film, the problem of increased connection resistance caused by substrate interface peeling is solved, achieving good connection reliability and strength under harsh environments.
Patent Information
- Application Number
- CN202210473838.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-04-29
AI Technical Summary
Existing circuit connection adhesive films are prone to peeling off from the substrate bonding interface, resulting in increased connection resistance, especially in high temperature and high humidity and thermal shock tests.
A two-layer adhesive structure is adopted, wherein the coefficient of linear expansion of the first adhesive layer is smaller than that of the second adhesive layer. The first adhesive layer is connected to the glass substrate, and the second adhesive layer is connected to the polyimide substrate. By setting adhesive layers with different coefficients of linear expansion, internal stress is reduced and connection reliability is improved.
It effectively prevents the adhesive interface from peeling off during high temperature, high humidity and thermal shock tests, maintains good connection reliability, reduces the risk of increased connection resistance, and improves the strength of circuit connections.
Smart Images

Figure CN114686125B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrical components, and in particular to a circuit connection adhesive film. Background Art
[0002] At present, for a circuit substrate having relative electrodes, an adhesive film in which conductive particles are dispersed is usually arranged between the two electrodes as a circuit connection adhesive film; for example, an adhesive film having anisotropic conductive function obtained by dispersing conductive particles in an epoxy adhesive or an acrylic adhesive is currently a representative circuit connection adhesive film.
[0003] The adhesive film having anisotropic conductive function is widely used for electrical connection between TCP (Tape Carrier Package) or COF (Chip On Flex) on which semiconductors for driving liquid crystal displays are mounted and LCD glass substrates.
[0004] After a polyimide substrate (generally referred to as TCP, COF, or FPC) is connected to an LCD glass substrate using an adhesive film having anisotropic conductive function, it is usually necessary to expose the product to various environments and perform multiple tests in order to confirm the reliability of the connection.
[0005] During the bonding process, due to the different linear expansion coefficients of the glass substrate and the polyimide substrate, internal stress occurs in the product; during the test process, especially in the high temperature and high humidity test (exposure to 85℃ / 85% environment for 500h to 1000h) and the thermal shock test (high temperature 100℃ to low temperature -40℃, repeated 500 to 1000 cycles), it is easy to peel off on one of the substrate sides or at the bonding interface of the two substrates, resulting in increased connection resistance.
[0006] As a conventional technology, in order to reduce the internal stress caused by the difference in thermal expansion coefficient after bonding, there is a technology of dispersing rubber particles in the adhesive. Although it has a certain effect on the interface peeling of polyimide substrates, it has no obvious improvement on the interface peeling of glass substrates.
[0007] In recent years, with the high-precision of LCD modules, the fine pitch of COF has been narrowed. The difference in linear expansion between the glass substrate and the COF substrate during connection causes a short circuit (short) problem between adjacent electrodes. As a countermeasure, a stacked structure of an anisotropic conductive adhesive layer with conductive particles dispersed and an insulating adhesive layer without conductive particles is adopted, and the thickness of the anisotropic conductive adhesive layer is 25.0-77.5% of the average particle size of the conductive particles. Therefore, compared with the previous circuit connection adhesive film, the capture efficiency of the conductive particles on the electrode has been significantly improved, and the connection reliability is also very good. However, although the polyimide interface of COF reduces the risk of short circuits, due to the peeling of the LCD glass interface, the increase in connection resistance has not been improved technically.
[0008] There is currently a technology for forming a circuit connection adhesive film having insulating properties between adjacent circuit electrodes and conductive properties between opposite circuit electrodes and having good film-forming properties (see Japanese Patent Invention No. 2016-110141). It is characterized by being filled with high concentrations of silica fillers and organic fillers, with the content of silica fillers being greater than 10% by mass and less than 80%, or greater than 5% by volume and less than 40%. However, at the same time, it is a necessary condition that the mass fraction of the organic filler is 5 to 20%, or the volume fraction is 5 to 20%. When a silica filler with a mass fraction of more than 10% is filled, there is no problem if it is a paste-like connection material, but in the case where the connection material is in the form of a film, the viscosity of the adhesive is significantly increased, and for fine pitch substrates below 50μm, the adhesive between the opposite terminals cannot be eliminated, which will lead to poor connection. Summary of the invention
[0009] The technical problem to be solved by the present invention is: in order to solve the problem in the prior art that the circuit connection adhesive film is easy to peel off at the bonding interface with the substrate, resulting in increased connection resistance, the present invention provides a circuit connection adhesive film, which reduces the internal stress of the workpiece to improve the bonding reliability by setting two layers of bonding base layers with different linear expansion coefficients, thereby solving the problem that the bonding interface is easy to peel off and cause increased resistance.
[0010] The technical solution adopted by the present invention to solve its technical problem is:
[0011] A circuit connection adhesive film comprises a first adhesive layer and a second adhesive layer which are stacked; wherein:
[0012] The first adhesive layer is used to connect with the glass substrate; the first adhesive layer includes a first adhesive layer and conductive particles dispersed in the first adhesive layer;
[0013] The second bonding layer is used to connect with the polyimide substrate; the second bonding layer includes a second adhesive layer;
[0014] The linear expansion coefficient of the first adhesive layer is smaller than the linear expansion coefficient of the second adhesive layer.
[0015] Optionally, the thickness of the first adhesive layer is 1 to 2 times the particle size of the conductive particles.
[0016] Optionally, the first bonding layer further comprises inorganic nanoparticles dispersed in the first adhesive layer.
[0017] Optionally, the mass fraction of the inorganic nanoparticles in the first adhesive layer is in a range of 2% to 15%.
[0018] Optionally, the inorganic nanoparticles include inorganic silica particles.
[0019] Optionally, the surface of the inorganic silica particles is hydrophobically treated with at least one of dimethylsiloxane, trimethylsilyl and octylsilane.
[0020] Optionally, the second adhesive layer further includes core-shell type organic powder dispersed in the second adhesive layer.
[0021] Optionally, the mass fraction of the core-shell type organic powder in the second adhesive layer is in the range of 5% to 20%.
[0022] Optionally, the core-shell organic powder includes a core layer and a shell layer coated on the outside of the core layer; the core layer is at least one of a (meth)acrylic polymer and a butadiene polymer; and the shell layer is a monomer of methyl methacrylate or a copolymer thereof.
[0023] Optionally, the core layer is selected from at least one of poly(meth)acrylate rubber, polybutylene rubber, polyisoprene rubber, and styrene-butadiene rubber.
[0024] The beneficial effect of the present invention is that the circuit connection adhesive film provided by the present invention is configured as a two-layer adhesive layer structure with different linear expansion coefficients. When connecting a glass substrate and a polyimide substrate, the second adhesive layer with a larger linear expansion coefficient is connected to the polyimide substrate with a larger thermal expansion, and the first adhesive layer with a smaller linear expansion coefficient is connected to the glass substrate with a smaller thermal expansion. This can reduce the internal stress caused by the different thermal expansion amounts of the polyimide substrate and the glass substrate during the test, avoid peeling of the bonding interface between the circuit connection adhesive film and the glass substrate or the polyimide substrate, thereby avoiding an increase in connection resistance, and at the same time improve the connection strength of the circuit connection adhesive film. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0026] Figure 1 It is a schematic structural diagram of the circuit connection adhesive film of the present invention;
[0027] Figure 2 The present invention is a schematic diagram of assembling the circuit connection adhesive film with the glass substrate and the polyimide substrate. DETAILED DESCRIPTION
[0028] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.
[0029] In the description of the present invention, it should be understood that the terms "first" and "second" are only used to simplify the description, and should not be understood as indicating or implying relative importance, or implicitly indicating the number of the indicated technical features. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0030] As LCD modules are gradually moving towards high precision and lightweight development, the corresponding glass substrates and polyimide substrates are gradually becoming thinner, and the spacing between the two is gradually becoming finer; in order to reduce components, it is usually necessary to increase the width of the glass substrate and the polyimide substrate to facilitate the mounting of more components; as the width of the glass substrate and the polyimide substrate increases, the problems caused by the difference in thermal expansion become more obvious.
[0031] In order to solve the problem in the prior art that the circuit connection adhesive film is easy to peel off from the bonding interface with the substrate, resulting in increased connection resistance, the present invention provides a circuit connection adhesive film, see Figure 1As shown, the circuit connection adhesive film includes a first adhesive layer and a second adhesive layer which are stacked; wherein the first adhesive layer is used to connect with the glass substrate; the first adhesive layer includes a first adhesive layer, and conductive particles dispersed in the first adhesive layer, so as to achieve electrical connection in the pressurized direction; the second adhesive layer is used to connect with the polyimide substrate; the second adhesive layer includes a second adhesive layer; in the present invention, preferably, the first adhesive layer and the second adhesive layer are both epoxy adhesive layers or acrylic adhesive layers; the specific materials of the first adhesive layer and the second adhesive layer can be the same or different; in order to reduce the internal stress of the product obtained after connecting the glass substrate and the polyimide substrate through the circuit connection adhesive film, in the present invention, preferably, the linear expansion coefficient of the first adhesive layer is smaller than the linear expansion coefficient of the second adhesive layer.
[0032] It should be noted that, in order to facilitate the description of the structure of the circuit connection adhesive film, the circuit connection adhesive film is divided into a first adhesive layer and a second adhesive layer; but in actual use, the first adhesive layer and the second adhesive layer are an integral structure bonded to each other, that is, the circuit connection adhesive film provided by the present invention does not have any stratification phenomenon during use.
[0033] The circuit connection adhesive film provided by the present invention is configured as a structure of two adhesive layers with different linear expansion coefficients. When connecting a glass substrate and a polyimide substrate, the second adhesive layer with a larger linear expansion coefficient is connected to the polyimide substrate with a larger thermal expansion, and the first adhesive layer with a smaller linear expansion coefficient is connected to the glass substrate with a smaller thermal expansion. This can reduce the internal stress caused by the different thermal expansion amounts of the polyimide substrate and the glass substrate during the test, reduce deformation, and avoid peeling of the bonding interface between the circuit connection adhesive film and the glass substrate or the polyimide substrate. Even after the test is carried out in a harsh environment, the circuit connection adhesive film can maintain good connection reliability, thereby avoiding the increase of connection resistance. At the same time, the connection strength of the circuit connection adhesive film can also be improved by the conductive particles dispersed in the first adhesive layer.
[0034] The conductive particles can be conductive metal particles such as Au, Ag, Cu, Ni, etc., or conductive particles obtained by coating conductive metal on the outside of non-conductive glass, ceramic, plastic and other particles; the particle size of the conductive particles can be determined according to the wiring spacing and electrode height of the polyimide substrate; for conductive particles with resin particles as cores, if the particle size is less than 2μm, it is difficult to exert the elasticity and recovery function of the core material; if the particle size of the conductive particles is greater than 20μm, it is not conducive to the refinement of the distance between the two substrates; in view of this, the particle size range of the conductive particles of the present invention and the preferred conductive particles is 2 to 20μm.
[0035] The conductive particles are preferably dispersed in the surface layer in a certain direction that is biased towards the thicker layer of the adhesive film. In order to ensure the connection strength between the metal electrode of the polyimide substrate and the glass substrate and improve the capture efficiency of the conductive particles on the electrode, refer to Figure 1 As shown, the thickness of the first adhesive layer of the present invention is preferably 1 to 2 times the particle size of the conductive particles, so as to maintain a sufficient low linear expansion adhesive layer between the metal electrode of the polyimide substrate and the glass substrate, thereby achieving high connection reliability.
[0036] Specifically, Figure 1 Where D is the thickness of the first bonding layer, F OR is the first bonding layer, F IN is the second adhesive layer; wherein the linear expansion coefficient of the first adhesive layer is less than the linear expansion coefficient of the second adhesive layer; after the circuit connection adhesive film is connected to the glass substrate and the polyimide substrate, see Figure 2 As shown, Figure 2 Wherein, P is a polyimide substrate, and G is a glass substrate; since the first adhesive layer is connected to the glass substrate in the presence of conductive particles, it is not easy to peel off at the interface of the glass substrate; and, if the thickness of the first adhesive layer is less than 1 times the diameter of the conductive particles, the low linear expansion adhesive layer between the metal electrode of the polyimide substrate and the glass substrate is insufficiently filled, resulting in poor connection reliability, and peeling is likely to occur at the interface of the glass substrate, resulting in increased connection resistance; on the contrary, if the thickness of the first adhesive layer is greater than 2 times the diameter of the conductive particles, the high linear expansion adhesive layer that should exist on the polyimide interface side is insufficiently filled, and it becomes difficult to relax the stress caused by the thermal expansion of the polyimide, thereby affecting the connection reliability, and peeling is likely to occur at the interface of the polyimide substrate, which is not desirable; therefore, the present invention preferably has a thickness of the first adhesive layer that is 1 to 2 times the particle size of the conductive particles.
[0037] The wiring part that actually makes the electrical connection is as follows Figure 2 As shown, the conductive particles are biased toward the glass substrate side, so by laminating the layer on the conductive particle side to the glass substrate for use, the adhesive layer with a low linear expansion coefficient fixes the wiring material, and electrical connection can be made through the conductive particles. Therefore, the presence of conductive particles in the adhesive with a low linear expansion coefficient on the glass substrate side can improve the connection reliability. On the contrary, by laminating an adhesive layer with a high linear expansion coefficient on the polyimide substrate side with large thermal expansion and contraction, not only the deviation (internal stress) caused by thermal expansion and contraction during connection is alleviated, but also the bonding strength is greatly improved.
[0038] In order to further reduce the linear expansion coefficient of the first adhesive layer, the present invention preferably includes inorganic nanoparticles dispersed in the first adhesive layer, so as to make the linear expansion coefficient of the first adhesive layer closer to the linear expansion coefficient of glass, alleviate the stress near the glass interface, and improve the reliability of the connection.
[0039] In order to ensure that the specific surface area of the inorganic nanoparticles meets the requirements, the particle size of the inorganic nanoparticles in the present invention is preferably in the range of 1 to 500 nm, and more preferably in the range of 1 to 200 nm.
[0040] As the content of inorganic nanoparticles increases, the linear expansion coefficient of the first adhesive layer decreases, but at the same time the bonding strength also tends to decrease; in order to take into account both the linear expansion coefficient and the connection strength of the first adhesive layer, the present invention preferably has a mass fraction range of 2% to 15% of inorganic nanoparticles in the first adhesive layer.
[0041] The inorganic nanoparticles may be nano-TiO2 or inorganic silicon dioxide particles; in the present invention, the inorganic nanoparticles are preferably inorganic silicon dioxide particles.
[0042] In order to improve the hydrophobicity of the inorganic silica particles and improve the reliability of connection after environmental testing, the surface of the inorganic silica particles is preferably treated with hydrophobicity by at least one of dimethylsiloxane, trimethylsilyl and octylsilane.
[0043] The inorganic silica particles with hydrophobic surface treatment can be prepared according to the existing technology or purchased directly, such as the inorganic silica particles produced by EVONIC, the product name is AEROSILR202, which are treated with dimethyl silicone and have a primary particle diameter of 14nm; the inorganic silica particles produced by EVONIC, the product name is AEROSILR805, which are treated with octylsilane and have a primary particle diameter of 12nm; the inorganic silica particles produced by EVONIC, the product name is AEROSILR812, which are treated with trimethylsilyl and have a primary particle diameter of 7nm.
[0044] In the present invention, the inorganic nanoparticles are preferably kneaded by a three-roll polisher (model DS50, manufactured by Longxin Intelligent Equipment Co., Ltd.) and then dispersed into the resin.
[0045] In order to alleviate the stress during the curing process, the second adhesive layer of the present invention preferably further includes core-shell organic powder dispersed in the second adhesive layer; by adding the core-shell organic powder to the second adhesive layer, the stress during the curing process is alleviated without significantly reducing the linear expansion coefficient of the second adhesive layer. By adding the core-shell organic powder to the adhesive film layer on the polyimide substrate side, it has a higher linear expansion coefficient than glass, which can reduce the stress from the polyimide substrate and improve the bonding strength.
[0046] The preferred particle size range of the core-shell organic powder of the present invention is 50-1000 nm; the mass fraction range of the core-shell organic powder in the second adhesive layer is 5%-20%.
[0047] The core-shell organic powder is a microparticle with propylene polymer or butadiene polymer as the main component, which is a polymer of unsaturated monomers with a core layer forming a rubber-like polymer, and the shell layer is a monomer or a copolymer of methyl methacrylate; specifically, the core-shell organic powder includes a core layer and a shell layer coated on the outside of the core layer; the core layer is at least one of a (meth)acrylic polymer and a butadiene polymer; the shell layer is a monomer or a copolymer of methyl methacrylate.
[0048] The core layer of the present invention is preferably selected from unsaturated monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate and lauryl (nitrogen-containing) (meth)acrylate, (meth)acrylonitrile, (meth)acrylamide; aromatic compounds such as styrene, α-methylstyrene and vinyltoluene; hydroxyl-containing unsaturated monomers such as hydroxyethyl (meth)acrylate and hydroxymethyl (meth)acrylamide; (Meta)unsaturated acids, such as acrylic acid. Examples thereof include at least one of butylamine and isoprene. Typical examples of polymers include poly (meth)acrylate rubber, polybutene rubber, polyisoprene rubber, polyvinyl chloride, styrene-butene rubber, styrene-butene-styrene rubber and styrene-isoprene-styrene rubber; examples thereof include styrene-butene rubber, styrene-ethylene rubber and ethylene-propylene rubber; among them, at least one of poly (meth)acrylate rubber, polybutene rubber, polyisoprene rubber and styrene-butadiene rubber is particularly preferred.
[0049] The methyl methacrylate polymer forming the shell layer is obtained by polymerizing methyl methacrylate monomer and other lower alkyl methacrylates (such as ethyl methacrylate, butyl methacrylate, styrene or a mixture thereof).
[0050] The core-shell organic powder can be prepared by oneself or purchased directly; for example, one can choose (core) butyl acrylate / (shell) methacrylate organic particles produced by DOW, the product name is PARALOID EXL-2313, with an average particle size of 500nm; (core) butadiene-styrene / (shell) methacrylate organic particles produced by DOW, the product name is PARALOID EXL-2655, with an average particle size of 200nm; (core) butadiene-styrene / (shell) methacrylate-styrene organic particles produced by KANEKA, the product name is KANE ACE M-732, with an average particle size of 180nm; (core) butyl acrylate / (shell) polystyrene organic particles produced by AICA, the product name is STAFILOID AC-3355, with an average particle size of 500nm.
[0051] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0052] Example 1
[0053] S1: 40 wt% of polyurethane resin (Desmocoll406, produced by Covestro), 15 wt% of fluorene acrylate (TR-FR-301, produced by TRONLY), 35 wt% of polyurethane acrylate (SartomerCN9782, produced by ARKEMA), 1 wt% of phosphoric acid acrylate (SartomerSR9050, produced by ARKEMA), 1 wt% of acrylic silane coupling agent (A-171, produced by MOMENTIVE), 3 wt% of organic peroxide (LUPEROX331, produced by ARKEMA), 3 wt% of conductive particles (AUL704, produced by Sekisui Chemical Industry Co., Ltd.), 2 wt% of inorganic silica particles (AEROSIL R805: octylsilane treated silica particles, primary particle size 12 nm, produced by EVONIC) were mixed and stirred with a self-rotating stirrer, and then coated on a PET film (25E-DG3, produced by ZACROS) using a coating machine (BEVS1818, produced by BEVS) to a thickness of 4 μm, and dried in a drying oven at 60°C for 5 minutes to obtain a first adhesive layer;
[0054] S2: 40wt% polyurethane resin (Desmocoll406, produced by Covestro), 15wt% fluorene acrylate (TR-FR-301, produced by TRONLY), 35wt% polyurethane (SartomerCN9782, produced by ARKEMA), 1wt% phosphoric acid acrylate (Sartomer SR9050, produced by ARKEMA), 1wt% acrylic silane coupling agent (A-171, produced by MOMENTIVE), 3wt% organic peroxide (LUPEROX331, produced by ARKEMA), 5wt% core-shell organic powder (PARALOID EXL2313: average particle size 500nm, produced by DOW) was mixed, stirred with a self-rotating stirrer, and then coated on a PET film (50E-8811ASCHK, produced by ZACROS) using a coating machine (BEVS1818, produced by BEVS) to a thickness of 11μm, and dried at 60°C for 5 minutes to obtain a second adhesive layer;
[0055] S3: Paste the first adhesive layer and the second adhesive layer together to obtain a circuit connection adhesive film with a thickness of 15 μm.
[0056] Example 2
[0057] The difference between this embodiment and embodiment 1 is that 10 wt % of inorganic silica particles (AEROSIL R805: octylsilane-treated silica particles, primary particle size 12 nm, produced by EVONIC) are added in step S1; 20 wt % of core-shell organic powder (PARALOID EXL2313: average particle size 500 nm, produced by DOW) are added in step S2; the thickness of the first adhesive layer 1 is 8 μm, and the thickness of the second adhesive layer 2 is 7 μm.
[0058] Example 3
[0059] The difference between this embodiment and embodiment 1 is that 2 wt % of inorganic silica particles (AEROSILR805: octylsilane-treated silica particles, primary particle size 12 nm, produced by EVONIC) are added in step S1; and 20 wt % of core-shell organic powder (PARALOID EXL2313: average particle size 500 nm, produced by DOW) are added in step S2.
[0060] Example 4
[0061] The difference between this embodiment and embodiment 1 is that 10 wt % of inorganic silica particles (AEROSILR805: octylsilane treated silica particles, primary particle size 12 nm, produced by EVONIC) are added in step S1; and 5 wt % of core-shell type organic powder (PARALOID EXL2313: average particle size 500 nm, produced by DOW) are added in step S2.
[0062] Comparative Example 1
[0063] The difference between this comparative example and Example 1 is that no inorganic silicon dioxide particles are added in step S1, and no core-shell organic powder is added in step S2; the thickness of the first adhesive layer 1 is 2 μm, and the thickness of the second adhesive layer 2 is 13 μm.
[0064] Comparative Example 2
[0065] The difference between this comparative example and Example 1 is that 15 wt% of inorganic silica particles (AEROSIL R805: octylsilane-treated silica particles, primary particle size 12 nm, produced by EVONIC) are added in step S1; 30 wt% of core-shell organic powder (PARALOID EXL2313: average particle size 500 nm, produced by DOW) are added in step S2; the thickness of the first adhesive layer 1 is 10 μm, and the thickness of the second adhesive layer 2 is 5 μm.
[0066] The performance test of the circuit connection adhesive films prepared in the above embodiments and comparative examples was carried out, and the specific test method is as follows:
[0067] 1. Measurement of linear expansion coefficient
[0068] After the first adhesive layer 1 and the second adhesive layer 2 prepared above are overlapped separately to a thickness of 30 to 33 μm, they are placed in an oven at 200°C for 3 hours for heat curing. The heat-cured film is peeled off from the separator and cut into 2mm×30mm size as a sample for measurement. Using a TMA device (model TMA450, produced by TAInstruments), a thermomechanical analysis is performed in the tensile test mode under the load conditions of 20mm between chucks, a measurement temperature range of 50 to 200°C, a heating rate of 5°C / min, and a cross-sectional pressure of 0.5MPa, and the linear expansion coefficient is obtained. The results are shown in Table 1.
[0069] 2. Make the circuit connection structure
[0070] The circuit connection adhesive film obtained by pasting the first adhesive layer 1 and the second adhesive layer 2 is cut into a size of 1.5mm×50mm, and is laminated on an ITO patterned glass substrate (40umP, Line / Space=1 / 1, 0.8mm thick) using a pasting device (model LD-02, produced by Ohashi Manufacturing Co., Ltd.) at 70°C / 1MP / 2sec; after peeling off the PET, the COF polyimide substrate (40umP, Line / Space=1 / 1, S'perflex substrate) is aligned and temporarily fixed in position, and is connected using a hot pressing device (model BD-01, produced by Ohashi Manufacturing Co., Ltd.) at 170°C / 3MPa / 10sec to obtain a circuit connection structure.
[0071] 3. Determination of connection resistance before environmental testing
[0072] The connection resistance value of the circuit connection structure was measured using a 4-terminal method when the current between the terminals was 1 mA, and the connection resistance before the environmental test was obtained. The test data is shown in Table 2.
[0073] 4. Determination of connection resistance after environmental testing
[0074] The circuit connection structure was placed in a high temperature and high humidity environment of 85°C / 85% for 500 hours and then taken out. After returning to room temperature, the connection resistance was measured to obtain the connection resistance after the environmental test. The test data is shown in Table 2.
[0075] In the present invention, a connection resistance of 3Ω or more is judged as NG.
[0076]
[0077] Table 1 Table 2
[0078]
[0079] It can be seen from the data in the above table that the circuit connection adhesive film provided by the present invention will not peel off at the substrate interface when connecting a glass substrate and a polyimide substrate under heating and pressurization conditions, and can maintain good connection reliability even after testing in a harsh environment.
[0080] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A circuit connection adhesive film, characterized in that: It comprises a first adhesive layer and a second adhesive layer which are stacked; wherein, The first adhesive layer is used to connect with the glass substrate; the first adhesive layer includes a first adhesive layer and conductive particles dispersed in the first adhesive layer; The second bonding layer is used to connect with the polyimide substrate; the second bonding layer includes a second adhesive layer; The linear expansion coefficient of the first adhesive layer is smaller than the linear expansion coefficient of the second adhesive layer; The thickness of the first adhesive layer is 1 to 2 times the particle size of the conductive particles; The first adhesive layer further includes inorganic nanoparticles dispersed in the first adhesive layer; The inorganic nanoparticles include inorganic silica particles; The surfaces of the inorganic silica particles are hydrophobically treated with at least one of dimethylsiloxane, trimethylsilyl and octylsilane; The circuit connection adhesive film is prepared according to the following method: S1: 40wt% of polyurethane resin, 15wt% of fluorene acrylate, 35wt% of polyurethane acrylate, 1wt% of phosphate acrylate, 1wt% of acrylic silane coupling agent, 3wt% of organic peroxide, 3wt% of conductive particles, and 2wt% of inorganic silica particles are mixed, stirred with a self-rotating stirrer, coated on a PET film to a thickness of 4μm, and dried in a drying oven at 60°C for 5 minutes to obtain a first adhesive layer; S2: 40wt% of polyurethane resin, 15wt% of fluorene acrylate, 35wt% of polyurethane acrylate, 1wt% of phosphate acrylate, 1wt% of acrylic silane coupling agent, 3wt% of organic peroxide, and 5wt% of core-shell organic powder were mixed, stirred with a self-rotating stirrer, coated on a PET film to a thickness of 11μm, and dried at 60°C for 5 minutes to obtain a second adhesive layer; S3: Paste the first adhesive layer and the second adhesive layer together to obtain a circuit connection adhesive film with a thickness of 15 μm.
2. The circuit connection adhesive film according to claim 1, characterized in that: The core-shell organic powder comprises a core layer and a shell layer coated outside the core layer; the core layer is at least one of a (meth)acrylic polymer and a butadiene polymer; the shell layer is a monomer of methyl methacrylate or a copolymer thereof.
3. The circuit connection adhesive film according to claim 2, characterized in that: The core layer is selected from at least one of poly(meth)acrylate rubber and styrene-butadiene rubber.