A catalyst for improving the yield of catalytic cracking gasoline and its preparation method

By simplifying the process and reducing costs, efficiently synthesizing small-grain Y-type molecular sieve catalysts has been solved, and the problems of complex processes and high costs in the prior art have been improved, and the yield of catalytic cracking gasoline is reduced.

CN114713267BActive Publication Date: 2024-11-01PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110015433.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-06
Publication Date
2024-11-01
Estimated Expiration
2041-01-06

AI Technical Summary

Technical Problem

In the process of improving the yield of catalytic cracking gasoline, the process is complex and the production cost is high, making it difficult to achieve industrial production of small crystal Y-shaped molecular sieves of kaolin microspheres.

Method used

Beat the kaolin, binder and deionized water, spray-drying to make kaolin microspheres, and then mix with the guide agent and alkali liquid after calcination, process at a specific temperature, add a silicon source for crystallization, and then filter it and perform "four two" after filtration The baking process reduces the sodium content and prepares a catalyst with small grain Y-shaped molecular sieve.

Benefits of technology

The external specific surface area of ​​the catalyst is increased, the accessibility of the active center is improved, and the rapid reaction of heavy oil macromolecules is reduced, excessive cracking is improved, gasoline yield is improved, and coke selectivity is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002885338310000061
    Figure BDA0002885338310000061
  • Figure BDA0002885338310000091
    Figure BDA0002885338310000091
Patent Text Reader

Abstract

A catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. The specific steps of the synthesis method of the invention include: slurrying kaolin, spray drying into microspheres, and then roasting at a certain temperature to obtain roasted kaolin microspheres; uniformly mixing a directing agent and part of the alkali solution at a certain temperature for a certain time, adding the directing agent and alkali solution, and an external silicon source to crystallize the roasted kaolin microspheres after alkali treatment at a certain temperature, filtering and washing, and obtaining crystallized microspheres containing small-grain Y-type molecular sieves. The method does not require the addition of organic matter, the process is simple, and the catalyst obtained after modification is used for catalytic cracking, the coke yield is reduced, and the gasoline yield is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof, and more specifically, to an in-situ crystallization catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. Background Art

[0002] Due to the adjustment of my country's oil consumption structure, the diesel-to-gasoline ratio reached a peak of 2.31 in 2005 and began to decline year by year. It has dropped to 1.64 in the first half of 2015 and is expected to drop to 1.06 in 2030. On the other hand, compared with diesel, the price difference of gasoline is higher than 1,000 yuan / ton. Reducing the diesel-to-gasoline ratio is an effective means for enterprises to improve quality and efficiency. Fluid catalytic cracking (FCC) is the main process for producing gasoline, providing about 70% of my country's gasoline pool. Improving the gasoline yield of FCC units is an important means to adjust the diesel-to-gasoline ratio of refineries. Catalytic cracking belongs to the catalytic process, and its core is the catalyst. The difference in catalyst performance will affect the conversion rate of the feedstock and the selectivity of the product. In order to improve the gasoline yield while taking into account the coke selectivity, people have conducted a lot of research on catalyst preparation.

[0003] Albemarle (NPRA, 2010AM-10-175) developed the GO-ULTRA catalyst by increasing the volume of medium and macropores and introducing aluminum atoms in a unique synergistic state. Compared with RUBY, it has a higher gasoline yield at the same catalyst-to-oil ratio and conversion rate. Patent CN1436835A improves the pore structure of the catalytic cracking catalyst by adding a medium and macroporous alumina, thereby improving the gasoline yield and coke selectivity. Patent CN1055301C uses macroporous pseudo-boehmite to improve the heavy oil conversion capacity, thereby improving the gasoline yield. Patent CN106179458A increases the content of mesopores in the catalytic cracking catalyst by adding a mesoporous active material, which is beneficial to the diffusion and cracking of heavy oil macromolecules and improves the gasoline yield. CN101733141A prepares a silicon-containing matrix by acidifying water glass, increases the pore volume of the catalyst, and improves the gasoline yield. CN102050434A uses a phosphorus-modified aluminum sol to improve the gasoline yield. Patent CN103506153A discloses a modified Y-type molecular sieve catalyst containing phosphorus and rare earth, which can reduce coking, improve heavy oil utilization, and improve gasoline selectivity. CN102019195A also invented a molecular sieve modified by phosphorus and rare earth to improve conversion capacity and gasoline yield. USP5312792 uses a phosphorus-containing molecular sieve as an active component to prepare a catalytic cracking catalyst with high gasoline yield and good thermal stability. CN1566270 uses an alkaline earth metal modified molecular sieve to improve gasoline yield.

[0004] It can be seen from the above patents that the current research content for improving gasoline yield is mainly focused on semi-synthetic binder-type catalysts as the main research object, and the catalyst pore structure and performance are improved by adding medium and macroporous matrix materials and modified molecular sieves, but these methods will cause complex processes and increase production costs. In the 1960s, Engelhard Company of the United States successfully developed a technology for preparing in-situ crystallized FCC catalysts with kaolin. The kaolin slurry was first sprayed into microspheres suitable for fluidized catalytic cracking units. After calcination, a part of the microspheres was converted into Y-type molecular sieves under alkaline hydrothermal conditions, and the matrix and active components were obtained at the same time. Then, the in-situ crystallized catalyst was prepared into FCC catalysts after modification. Due to the unique synthesis process, compared with binder-type catalysts, the in-situ crystallized catalyst has unique advantages such as good pore structure, good activity stability, and strong heavy oil conversion ability. In addition, Al-Khattaf's research shows (Applied Catalysis A: General 231 (2002) 293-306) that when the conversion rate is fixed, the gasoline yield gradually increases as the unit cell size of the Y-type molecular sieve decreases. Al-Khattaf found (Ind. Eng. Chem. Res. 1999, 38, 1350-1356) that under the same conversion rate, the use of small-grain molecular sieves has a higher gasoline yield. After the molecular sieve crystals are reduced, their specific surface area increases and the pores are shortened, so that the catalyst active points can be relatively increased, the diffusion performance can be improved, the product molecules can diffuse out quickly, and the excessive cracking and hydrogen transfer reactions of the molecules are reduced, thereby reducing the formation of coke and increasing the gasoline yield. Therefore, the in-situ crystallization technology is used to synthesize small-grain Y-type molecular sieves on kaolin microspheres, and the modified catalytic cracking catalyst is prepared, which has good application prospects for improving gasoline yield and reducing coke yield.

[0005] At present, there are reports on the synthesis of small-grain Y-type molecular sieves from kaolin microspheres. Patent CN102019197A adds organic additives to synthesize small-grain Y-type molecular sieves during the crystallization process of kaolin microspheres. Patent CN1393402A adds sodium citrate to the directing agent to reduce the grain size of Y-type molecular sieves synthesized from kaolin microspheres. CN104556121A performs hydrothermal crystallization under the action of ultrasound to synthesize small-grain Y-type molecular sieves. Xiong Jiangxi (Petroleum Refining and Chemical Industry, 2009, 40(10): 8-12) mixes sodium silicate and metakaolin at 0-5°C, then adds sodium hydroxide and deionized water, stirs for a certain period of time, adds a certain amount of pre-prepared directing agent, stirs for another 5 hours, and then stands for aging at 0-5°C for 12 hours, then transfers the aged slurry to a reactor, and continues crystallization at 90-100°C to obtain a nano Y-type molecular sieve. As can be seen from the above report, the synthesis of small-grain Y-type molecular sieve by in-situ crystallization of kaolin microspheres is mainly achieved by adding organic additives, ultrasonic crystallization or harsh conditions aging, etc., although these can make the particle size of the molecular sieve smaller, the cost is high, the process is complicated, and it is difficult to achieve large-scale industrial production. The present invention does not add organic additives and the process is simple, which is conducive to the industrial production of synthesizing small-grain Y-type molecular sieves from kaolin microspheres. After the molecular sieve particle size is reduced, more active centers are exposed, the exposed orifices increase, the micropore channels are shortened, the cracking products are easier to strip and diffuse, and the secondary cracking of gasoline is reduced, so that the gasoline yield is improved and the coke yield is reduced. Summary of the invention

[0006] The purpose of the present invention is to provide a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. The catalyst is mainly used for improving the yield of gasoline in the catalytic cracking process.

[0007] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof, characterized in that the preparation method comprises the following steps: (1) kaolin, a binder and deionized water are mixed and slurried, the solid content of the slurry is 30-50%, and spray-dried to prepare kaolin microspheres; (2) the kaolin microspheres are roasted at 700-1000°C for 1-3 hours to prepare roasted kaolin microspheres; (3) the directing agent and part of the alkali solution are mixed evenly, and the mixture is treated at 40-80°C for 1-3 hours; and then the mixture is added into the mixture. (2) calcining kaolin microspheres with alkali solution and treating at 90-95° C. for 1-3 hours; (4) adding a silicon source and uniformly mixing it with the solution in step (3), crystallizing it at 90-95° C. for 12-16 hours, filtering and washing with water to obtain crystallized microspheres containing small-grain Y-type molecular sieve; (5) exchanging the crystallized microspheres with ammonium and rare earth according to the "four cross-exchange and two roasting" process and roasting them between the exchanges to reduce the sodium content to Na2O < 0.5%, and drying to obtain a catalytic cracking catalyst for improving gasoline yield.

[0008] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. In the step (1), the kaolin comprises soft kaolin, hard kaolin and coal gangue, wherein the particle size is 2.5 to 3.5 μm, the crystalline kaolinite content is higher than 80%, the iron oxide content is lower than 1.7%, and the sum of sodium oxide and potassium oxide is lower than 0.5%.

[0009] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. In the step (1), the binder is one or more of water glass, silica sol and aluminum sol, and the added amount is 2-10% of the mass of kaolin.

[0010] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. The molar ratio of the directing agent in the step (3) is: (14-16) SiO2: (0.7-1.3) Al2O3: (14-16) Na2O: (300-330) H2O. The amount of the directing agent added is 1%-10% of the weight of the synthetic material, and the synthetic material refers to the sum of all raw materials used for the synthesis of the small-grain Y-type molecular sieve composite material.

[0011] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof, wherein the alkali solution in the steps (3) and (4) is selected from one of sodium hydroxide or potassium hydroxide solutions or a mixture thereof, and the total amount of the sodium hydroxide or potassium hydroxide solution or the mixture thereof is 1% to 6% of the weight of the synthetic material, preferably 2% to 4%. The amount of the calcined kaolin microspheres added on a dry basis is 8% to 35% of the weight of the synthetic material.

[0012] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. In the step (3), the calcined kaolin microspheres are dry basis: alkali solution OH - The mass ratio is 15-20:1.

[0013] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. In the step (4), the added silicon source is selected from water glass or silica sol, and the added amount is 5% to 30% of the weight of the synthetic material in terms of SiO2 content.

[0014] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. The modification method comprises exchanging ammonium and rare earth according to a "four cross-linking and two roasting" process and roasting between the exchanges to reduce the sodium content to Na2O < 0.5%, for example, according to the "four cross-linking and two roasting" in Example 9 of CN101250428A.

[0015] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. In step (4), the crystallized microspheres containing small-grain Y-type molecular sieve have a crystallinity of 20-50%, a silicon-aluminum ratio greater than 4.7, and a particle size less than 400nm.

[0016] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. The external specific surface area of ​​the prepared catalytic cracking catalyst is greater than 150m 2 / g, good activity and high gasoline yield.

[0017] The present invention discloses a catalyst for improving the yield of catalytic cracking gasoline and a preparation method thereof. The catalyst improves the activity of the crystal nucleus and increases the relative number of effective crystal seeds by mixing alkali liquid and a guiding agent in the crystallization stage. At the same time, the kaolin microspheres are alkali-treated and roasted to generate activated silicon oxide and aluminum oxide, so that the nucleation rate of the crystal nucleus is accelerated during the crystallization process, thereby reducing the particle size of the molecular sieve. The small-grain Y-type molecular sieve is synthesized on the kaolin microspheres by using this technology, wherein the crystallinity is 20-50%, the silicon-aluminum ratio is greater than 4.7, and the particle size is less than 400nm. The catalytic cracking catalyst is obtained by modification. Compared with the conventional in-situ crystallization catalyst, the molecular sieve particle size is reduced, the external specific surface area of ​​the catalyst is increased, the accessibility of the active center is improved, the heavy oil macromolecules quickly approach the active center for reaction, and the product molecules quickly diffuse out, reducing over-cracking, improving the gasoline yield, and having good coke selectivity. DETAILED DESCRIPTION

[0018] The present invention will be further described below with reference to specific embodiments, but the present invention is not limited by the following specific embodiments.

[0019] Source of raw materials

[0020] Kaolin: Produced by China Kaolin Company, with a medium particle size of 3.2μm, kaolinite content of 82%, iron oxide content of 0.74%, and the sum of potassium oxide and sodium oxide content of 0.35%.

[0021] Water glass: SiO2 250.3g / L, Na2O 87.4g / L, produced by Lanzhou Petrochemical Company

[0022] Alkali solution: NaOH 14m%, produced by Lanzhou Petrochemical Company

[0023] Hydrochloric acid: HCl 36-37m% Tianjin Kemiou Chemical Reagent Co., Ltd.

[0024] Potassium hydroxide: KOH 99m% Tianjin Yongda Chemical Reagent Co., Ltd.

[0025] Silica sol: SiO2 25m%, pH 8.5-10, produced by Lanzhou Petrochemical Company

[0026] Alumina sol: Al2O3 26m%, produced by Lanzhou Petrochemical Company

[0027] Guiding agent: Prepared according to the guiding agent composition in Example 1 of CN1232862A

[0028] Rare earth nitrate: RE2O3 230.5g / L, produced by Lanzhou Petrochemical Company

[0029] Ammonium chloride: NH4Cl 99m% Produced by Tianjin Yongda Chemical Reagent Co., Ltd.

[0030] Analytical methods

[0031] The sodium oxide and rare earth of the catalytic cracking catalyst were determined by X-ray fluorescence, the crystallinity and silicon-aluminum ratio of the Y-type molecular sieve were determined by X-ray powder diffraction, the photos of the Y-type molecular sieve morphology were tested by scanning electron microscopy, the catalyst surface area was determined by nitrogen adsorption-desorption method, and the catalyst activity was determined by a fixed bed micro-reactor. (For the analysis method, see "Petrochemical Analysis Method (RIPP Experimental Method)", edited by Yang Cuiding et al., Science Press, published in 1990). The catalyst reaction performance was evaluated by ACE device (Advanced Cracking Evaluation, Kayser, R+MultiMode reactor), and the evaluation conditions were: the catalyst was aged at 800°C and 100% steam for 17h, the reaction temperature was 530°C, the catalyst-oil ratio was 5, the raw oil was Xinjiang vacuum wide-fraction wax oil and Xinjiang vacuum residue oil, and the residue blending ratio was 30%. The properties of the raw oil are shown in Table 1.

[0032] Table 1 Properties of crude oil*

[0033]

[0034] *: The above results are determined by PetroChina Lanzhou Lubricant R&D Center

[0035] Example 1

[0036] 3000g kaolin (dry basis), 210g silica sol and deionized water were mixed and slurried to a solid content of 40%, and spray dried to form microspheres. The kaolin microspheres were calcined at 780°C for 2.8h to obtain calcined kaolin microspheres, 340g of directing agent and 540g of alkali solution were mixed evenly, and treated at 40°C for 2.9h; 880g of calcined kaolin microspheres were mixed evenly with 980g of alkali solution and treated at 92°C for 2.5h, and then the treated directing agent and alkali solution, as well as 546g of water glass were added, mixed evenly, and crystallization was continued for 13 hours, filtered, washed with water, and dried to obtain crystallized microspheres containing small-grain Y-type molecular sieves, wherein the Y-type molecular sieve had a crystallinity of 33%, a silicon-aluminum ratio of 4.91, and an average grain size of 343nm. The above-mentioned crystallized microspheres were modified and reduced in sodium according to the "four cross-linking and two baking" method, and finally dried to obtain catalyst 1.

[0037] Example 2

[0038] 3102g kaolin (dry basis), 200g water glass, 120g silica sol and deionized water were mixed and slurried to a solid content of 39%, and spray dried to form microspheres. The kaolin microspheres were calcined at 980°C for 1.2h to obtain calcined kaolin microspheres, 1500g of directing agent and 1024g of alkali solution were mixed evenly, and treated at 78°C for 1.3h; 580g of calcined kaolin microspheres were mixed evenly with 487 alkali solution and treated at 91°C for 2.9h, and then the directed agent and alkali solution after the above treatment, as well as 920g of water glass, were added, and after mixing evenly, crystallization was continued for 15 hours, filtered, washed with water, and dried to obtain crystallized microspheres containing small-grain Y-type molecular sieves, wherein the Y-type molecular sieve had a crystallinity of 46%, a silicon-aluminum ratio of 4.83, and an average grain size of 316nm. The above-mentioned crystallized microspheres were modified and reduced in sodium according to the "four cross-linking and two baking" method, and finally dried to obtain catalyst 2.

[0039] Example 3

[0040] 2928g kaolin (dry basis), 270g water glass and deionized water were mixed and slurried to a slurry solid content of 43%, and spray dried to form microspheres. The kaolin microspheres were calcined at 870°C for 2.2h to obtain calcined kaolin microspheres, 440g of directing agent and 201g of 10 wt% potassium hydroxide solution were mixed evenly, and treated at 70°C for 1.7h; 1160g of calcined kaolin microspheres were mixed evenly with 1516g of % potassium hydroxide solution and treated at 90°C for 2.5h, and then the above-treated directing agent and alkali solution, as well as 4000g of silica sol were added, mixed evenly, and crystallized for 16 hours, filtered, washed with water, and dried to obtain crystallized microspheres containing small-grain Y-type molecular sieves, wherein the Y-type molecular sieve has a crystallinity of 35%, a silicon-aluminum ratio of 4.87, and an average grain size of 350nm. The above-mentioned crystallized microspheres were modified and reduced in sodium according to the "four cross-linking and two baking" method, and finally dried to obtain catalyst 3.

[0041] Example 4

[0042] 3421g kaolin (dry basis), 250g water glass and deionized water were mixed and slurried to a solid content of 35%, and spray dried to form microspheres. The kaolin microspheres were calcined at 960°C for 2.5h to obtain calcined kaolin microspheres, 460g of directing agent and 81g of alkali solution were mixed evenly, and treated at 60°C for 2.2h; 520g of calcined kaolin microspheres were mixed evenly with 499g of alkali solution and treated at 95°C for 1.5h, and the above-treated directing agent and alkali solution, as well as 2060g of water glass, were added, and crystallization was continued for 12 hours, filtered, washed with water, and dried to obtain crystallized microspheres containing small-grain Y-type molecular sieves, wherein the Y-type molecular sieve has a crystallinity of 28%, a silicon-aluminum ratio of 5.07, and an average grain size of 376nm. The above-mentioned crystallized microspheres were modified and reduced in sodium according to the "four cross-linking and two baking" method, and finally dried to obtain catalyst 4.

[0043] Example 5

[0044] 3200g kaolin (dry basis), 336g water glass and deionized water were mixed and slurried to a solid content of 47%, and spray dried to form microspheres. The kaolin microspheres were calcined at 920°C for 1.8h to obtain calcined kaolin microspheres, 1160g of directing agent and 433g of alkali solution were mixed evenly and treated at 45°C for 1.7h; 2000g of calcined kaolin microspheres were mixed evenly with 1867g of alkali solution and treated at 93°C for 2.6h, and the above-treated directing agent and alkali solution, as well as 1280g of silica sol were added, mixed evenly, and crystallized for 14 hours, filtered, washed with water, and dried to obtain crystallized microspheres containing small-grain Y-type molecular sieves, wherein the Y-type molecular sieve has a crystallinity of 41%, a silicon-aluminum ratio of 4.81, and an average grain size of 301nm. The above-mentioned crystallized microspheres were modified and reduced in sodium according to the "four cross-linking and two baking" method, and finally dried to obtain catalyst 5.

[0045] Example 6

[0046] 2735g kaolin (dry basis), 176g aluminum sol and deionized water were mixed and slurried to a solid content of 32%, and spray dried to form microspheres. The kaolin microspheres were calcined at 800°C for 2.8h to obtain calcined kaolin microspheres, 940g of directing agent and 1060g of alkali solution were mixed evenly, and treated at 65°C for 1.4h; 1820g of calcined kaolin microspheres were mixed evenly with 1999g of alkali solution and treated at 94.5°C for 2.3h, and then the directed agent and alkali solution after the above treatment, as well as 1240g of water glass, were added, and after mixing evenly, crystallization was continued for 12.5 hours, filtered, washed with water, and dried to obtain crystallized microspheres containing small-grain Y-type molecular sieves, wherein the Y-type molecular sieve has a crystallinity of 31%, a silicon-aluminum ratio of 4.93, and an average grain size of 345nm. The above-mentioned crystallized microspheres were modified and reduced in sodium according to the "four cross-linking and two baking" method, and finally dried to obtain catalyst 6.

[0047] Comparative Example 1

[0048] The preparation scheme of kaolin microspheres is the same as that of Example 1. The kaolin microspheres are calcined at 780°C for 2.8h to obtain calcined kaolin microspheres. 340g of directing agent, 1520g of alkali solution, 880g of calcined kaolin microspheres and 546g of water glass are mixed evenly, crystallized at 92°C for 13 hours, filtered, washed with water, and dried to obtain crystallized microspheres containing Y-type molecular sieve, wherein the Y-type molecular sieve has a crystallinity of 32%, a silicon-aluminum ratio of 4.93, and an average grain size of 865nm. The above-mentioned crystallized microspheres are modified and reduced in sodium according to the "four cross-linking and two baking" method, and finally dried to obtain contrast agent 1.

[0049] Comparative Example 2

[0050] The preparation scheme of kaolin microspheres is the same as that of Example 2. The kaolin microspheres are calcined at 980°C for 1.2h to obtain calcined kaolin microspheres. 1500g of directing agent, 1520g of alkali solution, 1024g of calcined kaolin microspheres and 920g of water glass are mixed evenly, crystallized at 91°C for 15 hours, filtered, washed with water, and dried to obtain crystallized microspheres containing Y-type molecular sieve, wherein the Y-type molecular sieve has a crystallinity of 47%, a silicon-aluminum ratio of 4.81, and an average grain size of 773nm. The above-mentioned crystallized microspheres are modified and reduced in sodium according to the "four cross-linking and two baking" method, and finally dried to obtain contrast agent 2.

[0051] Comparative Example 3

[0052] The preparation scheme of kaolin microspheres is the same as that of Example 3. The kaolin microspheres are calcined at 870°C for 2.2h to obtain calcined kaolin microspheres. 440g of directing agent, 1480g of 10% potassium hydroxide solution, 1160g of calcined kaolin microspheres and 4000g of silica sol are mixed evenly, crystallized at 90°C for 16 hours, filtered, washed with water, and dried to obtain crystallized microspheres containing Y-type molecular sieve, wherein the Y-type molecular sieve has a crystallinity of 35%, a silicon-aluminum ratio of 4.84, and an average grain size of 907nm. The above-mentioned crystallized microspheres are modified and reduced in sodium according to the "four cross-linking and two baking" method, and finally dried to obtain contrast agent 3.

[0053] Table 2 lists the physicochemical properties and reaction performance of catalysts 1, 2 and 3 and comparative agents 1, 2 and 3.

[0054] Table 2 Physicochemical properties and reaction performance of catalysts and comparison agents

[0055]

[0056] It can be seen from Table 2 that the catalytic cracking catalyst prepared by the technology of the present invention has good heavy oil conversion ability, and the gasoline yield is significantly improved while the coke yield is reduced.

[0057] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a catalyst for improving the yield of catalytic cracking gasoline, It is characterized in that The preparation method comprises the following steps: (1) kaolin, a binder and deionized water are mixed and slurried to obtain a slurry with a solid content of 30-50%, and spray-dried to obtain kaolin microspheres; (2) calcining the kaolin microspheres at 700-1000° C. for 1-3 hours to obtain calcined kaolin microspheres; (3) uniformly mixing a directing agent and a portion of an alkali solution, and treating the mixture at 40-80° C. for 1-3 hours; then adding the calcined kaolin microspheres in step (2) and the remaining alkali solution to mix the mixture, and treating the mixture at 90-95° C. for 1-3 hours; (4) uniformly mixing an external silicon source with the solution in step (3), crystallizing the mixture at 90-95° C. for 12-16 hours, filtering and washing the mixture with water to obtain crystallized microspheres containing small-grain Y-type molecular sieves; and (5) exchanging the crystallized microspheres with ammonium and rare earth according to a "four cross-exchange and two roasting" process, and roasting the crystallized microspheres between the exchanges to reduce the sodium content to Na 2 O<0.5%, drying obtains the catalyst which improves the yield of catalytic cracking gasoline.

2. The preparation method according to claim 1, It is characterized in that In step (1), the kaolin is selected from at least one of soft kaolin and hard kaolin, wherein the kaolin particle size is 2.5-3.5 μm, the crystalline kaolinite content is higher than 80%, the iron oxide content is lower than 1.7%, and the sum of the sodium oxide and potassium oxide contents is lower than 0.5%.

3. The preparation method according to claim 1, It is characterized in that In step (1), the binder is selected from one or more of water glass, silica sol and alumina sol, and the amount added is 2-10% of the mass of kaolin.

4. The preparation method according to claim 1, It is characterized in that The molar ratio of the directing agent in step (3) is: (14-16) SiO 2 :(0.7~1.3)Al 2 O 3 :(14~16)Na 2 O:(300~330)H 2 O, the amount of the directing agent added is 1%-10% of the weight of the synthetic material, and the synthetic material refers to the sum of all raw materials used for synthesizing the crystallized microspheres containing small-grain Y-type molecular sieve.

5. The preparation method according to claim 1, It is characterized in that In step (3), part of the alkali solution and the remaining alkali solution are both selected from sodium hydroxide or potassium hydroxide solution or a mixture thereof, and the total amount of alkali solution added accounts for 1% to 6% of the weight of the synthetic material, and the synthetic material refers to the sum of all raw materials used for synthesizing crystallized microspheres containing small-grain Y-type molecular sieve.

6. The preparation method according to claim 5, It is characterized in that The total amount of alkali solution added in step (3) accounts for 2% to 4% of the weight of the synthetic material.

7. The preparation method according to claim 1, It is characterized in that In step (4), the added silicon source is selected from water glass or silica sol, and the added amount is SiO 2 The content accounts for 5% to 30% of the weight of the synthetic material, and the synthetic material refers to the sum of all raw materials used for synthesizing crystallized microspheres containing small-grain Y-type molecular sieve.

8. The preparation method according to claim 1, It is characterized in that In step (3), the dry amount of calcined kaolin microspheres added is 8% to 35% of the weight of the synthetic material, and the synthetic material refers to the sum of all raw materials used to synthesize crystallized microspheres containing small-grain Y-type molecular sieve.

9. The preparation method according to any one of claims 1 to 8, It is characterized in that The crystallized microspheres containing small-grain Y-type molecular sieve in step (4) have a crystallinity of 20-50%, a silicon-aluminum ratio greater than 4.7, and a particle size less than 400 nm.

10. The preparation method according to any one of claims 1 to 8, It is characterized in that The external specific surface area of ​​the prepared catalyst is greater than 150m 2 / g.