A medium oil type hydrocracking catalyst, a sulfide type hydrocracking catalyst
By using small grain mesoporous modified Y molecular sieve and amorphous silica alumina in the hydrocracking catalyst, the problem of insufficient microporous structure of Y-type molecular sieve is solved, the liquid recovery and jet fuel yield of hydrocracking are improved, and the yield of jet fuel is reduced. The BMCI of the hydrogenated tail oil is added, which enhances the conversion capacity of the catalyst and the selectivity of the middle distillate.
Patent Information
- Application Number
- CN202110015517.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-01-06
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-01-06
AI Technical Summary
When existing hydrocracking catalysts treat heavy oil, due to the insufficient micropore structure of Y-type molecular sieves, they result in excessive cracking, low liquid yield and high light naphtha yield, and it is difficult to increase the yield of aviation kerosene.
Small grain mesoporous modified Y molecular sieve is used, treated with low concentration alkali solution to increase the mesoporous structure, combined with amorphous silica aluminum and active metals to form a medium oil hydrocracking catalyst, and improve the mesoporous index and micropores of the catalyst -Mesoporous connectivity.
It improves the liquid recovery and aviation fuel yield of hydrocracking, reduces the BMCI of hydrogenation tail oil, enhances the conversion ability of the catalyst and the selectivity of middle distillate oil, and reduces the reaction temperature.
Smart Images

Figure CN114713274B
Abstract
Description
Technical Field
[0001] The present invention relates to the field of hydrocracking catalysts, and more specifically, to a medium oil type hydrocracking catalyst and a sulfurized type hydrocracking catalyst containing a modified Y molecular sieve. Background Art
[0002] The trend of crude oil becoming heavier and of lower quality is becoming increasingly prominent. Hydrocracking process is a very effective means of converting heavy and inferior heavy oil into light and high-quality products. Compared with catalytic cracking, hydrocracking process has high adaptability to raw materials and has become the core process of modern oil refining enterprises.
[0003] The core of the hydrocracking process is the hydrocracking catalyst. A typical hydrocracking catalyst is a bifunctional catalyst, in which the hydrogenation function is provided by the active metal and the cracking function is provided by the acidic center. The hydrogenation function is mainly hydrogenation / dehydrogenation. The active metal often uses non-precious metal elements, such as Co, Ni, Mo, W, etc., and the sulfides of the above active metals play a role in the reaction process. The acidity is mainly provided by the carrier, which determines the cracking activity and selectivity of the catalyst to a considerable extent. The acidic components used in the early hydrocracking catalyst include amorphous silica-alumina, modified alumina, etc. With the deepening of the understanding of silica-alumina molecular sieves and the maturity of preparation technology, especially the Y-type molecular sieve has the advantages of unobstructed pores, large pore size, high acidity, and large modification space, it quickly became an important acidic component of the hydrocracking catalyst. By adjusting the matching degree of the hydrogenation function center and the acidic function center, the hydrogenation function is weaker and the acidic function is stronger, and a medium oil type hydrocracking catalyst that can produce more middle distillates and high-quality tail oil is obtained.
[0004] In order to meet the demand for increasing ethylene cracking raw materials and aviation kerosene, the selectivity of aviation kerosene should be improved and the BMCI of hydrogenated tail oil should be reduced. At the same time, the use of more active catalysts can reduce the reaction temperature and reduce production and operating costs. Hydrocracking feeds include fractions of 350℃ to 550℃ such as vacuum wax oil. The molecular microscopic size of heavy oil fractions is large. Since the Y-type molecular sieve is mainly composed of microporous structures and there are fewer larger mesoporous structures, it is difficult for heavy oil molecules to fully utilize the surface and acid sites of the Y-type molecular sieve, and the cracking products cannot be desorbed from the smaller micropores in time, resulting in excessive cracking, reducing the liquid yield, increasing the yield of light naphtha, and not utilizing the yield of aviation kerosene. Therefore, the catalyst needs to provide a large number of larger pore structures, such as mesoporous structures above 3 nanometers. Conventional methods can be achieved by using inorganic oxide components with large pore volume and large pore size in the carrier, such as alumina, amorphous silicon aluminum, etc.
[0005] ZL97121663.0 discloses a hydrocracking catalyst particularly suitable for producing middle distillate oil, comprising an amorphous silicon oxide-alumina component and a small-pore alumina binder, wherein the content of the amorphous silicon oxide-alumina is 30-60% by weight, at least one VIB group element and at least one VIII group element, the total content of active metal oxides is 20-35% by weight, and the balance is a small-pore alumina binder, characterized in that the catalyst has a specific surface area of 150-300m 2 / g, pore volume 0.25-0.50ml / g, 4-15 nanopore distribution 60-90%, infrared acidity 0.30-0.50mmol / g.
[0006] CN102030351A discloses a macroporous alumina with a bimodal pore distribution, the pore volume of which is 0.6-3.0 ml / g and the specific surface area of which is 90-300 m 2 / g, wherein pores of 35 to 100 angstroms account for 20 to 55% of the total pore volume, and the most probable pore diameter is between 300 and 600 angstroms. The alumina is prepared by a two-step aging method.
[0007] CN107029779A discloses a multi-level pore hydrocracking catalyst containing Y molecular sieve, in which the pore volume of pores with a pore diameter less than 2 nanometers accounts for 2-50% of the total pore volume, the pore volume of pores with a pore diameter of 2-100 nanometers accounts for 20-85% of the total pore volume of the catalyst, and the pore volume of pores with a pore diameter greater than 100 nanometers accounts for 3-70% of the total pore volume of the catalyst.
[0008] In hydrocracking catalysts, including amorphous oxides, molecular sieves are key acidic cracking components. Improving the mesoporous degree of molecular sieves is also one of the important means to improve catalyst performance and enhance product selectivity and quality. The preparation of catalytic materials rich in mesoporous structures has become a research hotspot. Hydrocracking catalysts containing mesoporous molecular sieves show better performance.
[0009] Literature reports (Catalyst Design by NH4OH Treatment of USY Zeolite, Adv. Funct. Mater., 2015, 25, 7130-7144) use low concentration ammonia solution to treat Y molecular sieve with a silicon-aluminum ratio of 40 under the condition of a liquid-solid ratio of 80:1, and obtain a mesoporous Y molecular sieve without alkali metal ions. The Y molecular sieve obtained by this method has a high mesopore volume and specific surface area. Since this method will produce a large amount of dense hydrated ammonium silicate products (Hierarchization of USY Zeolite by NH4OH. A Postsynthetic Process Investigated by NMR and XRD, J. Phys. Chem. C 2014, 118, 22573-22582), the micropore volume is significantly reduced. Compared with other materials, the strong acidity, pore shape selectivity, selective ring opening and other special properties of Y molecular sieve come from the microporous properties brought by its regular crystal structure. Therefore, a relatively high microporous structure must be retained in order to fully utilize the mesopores brought by the modification on the basis of exerting the characteristics of the molecular sieve, realize efficient diffusion of micropores-mesopores, and enhance the performance of its catalytic macromolecules.
[0010] CN106669800A discloses a catalyst preparation method for producing low linear alkane content hydrocracking tail oil, which uses a modified Y-β composite molecular sieve treated with an organic alkali solution, and the modified composite molecular sieve has a relatively rich mesoporous structure. At the same conversion rate, the reaction temperature is reduced by 3 to 8 ° C, showing a higher hydrogenation ring-opening performance.
[0011] Chinese patent CN201711119061.X discloses a modified YY isomorphous molecular sieve and its preparation method, wherein the YY isomorphous molecular sieve is treated with an organic alkaline solution. The molecular sieve has a core-shell structure, wherein the shell structure is a nano Y molecular sieve; the total pore volume is 0.56-1.25 mL / g; the mesopore volume is 0.45-0.95 mL / g; the mesopore volume accounts for 40-80% of the total pore volume; the molar ratio of silicon oxide to aluminum oxide is 6-25; the specific surface area is 580-950 m 2 / g.
[0012] The literature reports the industrial application comparison analysis of the hydrocracking catalyst FC-76 using mesoporous Y molecular sieve and the FC-32 catalyst containing conventional USY molecular sieve (Comparative Analysis of Industrial Application of Hydrocracking Catalysts FC-76 and FC-32, Li Shiwei, Refining Technology and Engineering, Vol. 49, No. 6, 2019). The reaction temperature of the FC-76 catalyst was reduced by 6°C, the total space velocity was increased by 10%, the light hydrocarbon yield was reduced by 0.3 percentage points, the light naphtha was reduced by 2.4 percentage points, the intermediate distillate oil (jet kerosene + diesel) yield was reduced by 0.5 percentage points, and the hydrogenation tail oil BMCI was reduced by 1.9 units. The catalyst also strengthens the hydrogenation ring-opening reaction and hydrogenation isomerization reaction in the hydrocracking process, and can produce high-quality lubricant base oil products.
[0013] From the above, we can see that different types of molecular sieves can provide different reaction performances for catalysts. The use of some mesoporous molecular sieves with strong ring-opening ability can improve the properties of hydrocracking products and produce high-quality ethylene cracking raw materials while producing intermediate distillates. Summary of the invention
[0014] Based on the above, the purpose of the present invention is to provide a medium oil type hydrocracking catalyst, which adopts a mesoporous molecular sieve with strong ring-opening ability to improve the properties of its hydrocracking products. The hydrocracking catalyst is used in the hydrocracking process, and can increase the liquid yield and jet fuel yield of hydrocracking while producing intermediate distillate oil, and reduce the BMCI of hydrogenated tail oil.
[0015] To this end, the present invention provides a medium oil type hydrocracking catalyst, which, based on the weight of the catalyst, comprises: 10-20wt% modified Y molecular sieve, 30-70wt% amorphous silicon aluminum, 20-50wt% binder and 25-35wt% active metal;
[0016] The modified Y molecular sieve is a small-grain mesoporous modified Y molecular sieve, wherein the molar ratio of silicon oxide to aluminum oxide in the framework is 15-60, the sodium oxide content is less than 0.1wt%, the unit cell parameter is 2.430-2.438nm, the relative crystallinity is 60-100%, the crystal particle size is normally distributed with d as the center, wherein d is less than 500nm, the mesoporous index M is 1.7-5.0, wherein M=(S ext / S micro )*(V meso / V micro ), S ext is the external specific surface area in the t-plot method in nitrogen adsorption and desorption determination, S micro is the micropore specific surface area in the t-plot method in nitrogen adsorption and desorption determination, V micro is the micropore volume in the t-plot method in nitrogen adsorption-desorption determination, V mesoIt is the total pore volume of the single point adsorption method in nitrogen adsorption-desorption measurement minus V micro The difference.
[0017] In the hydrocracking catalyst of the present invention, preferably, the micropore volume of the modified Y molecular sieve is not less than 0.20 ml / g.
[0018] In the hydrocracking catalyst of the present invention, preferably, the mesoporous index M is 2.0 to 5.0, and more preferably 3.0 to 5.0.
[0019] In the hydrocracking catalyst of the present invention, preferably, the d is less than 450 nm, and more preferably less than 350 nm.
[0020] The hydrocracking catalyst of the present invention is preferably prepared by the following method:
[0021] (1) placing the Y molecular sieve in a vacuum heating container for pretreatment until the gas pressure in the container is reduced to less than 0.1 atmosphere;
[0022] (2) preparing a mixed alkaline solution, wherein the concentration of ammonia is 0.01 to 0.50 mol / L, and the concentration of another alkali is 0.05 to 0.5 mol / L, and more preferably, the concentration of the organic base in the mixed alkaline solution is 0.1 to 0.5 mol / L;
[0023] (3) adding the mixed alkali solution prepared in step (2) into the vacuum heating container in step (1), reacting at 40-95° C. for 10 minutes to 5 hours, then filtering, washing, drying and calcining to obtain a modified Y molecular sieve;
[0024] Wherein, the other base is selected from at least one of methylamine, ethylamine, ethylenediamine, 1-propylamine and isopropylamine, and the mass ratio of the mixed alkaline solution to the Y molecular sieve is 3 to 50:1.
[0025] The preparation method of the modified Y molecular sieve provided by the present invention has the advantages of short preparation time and simple operation, and adopts a base without metal ions as a modification agent, and combines a weak base ammonia with an organic small molecule base to achieve the purpose of improving the mesoporous properties, thereby improving the activity and selectivity of the hydrogenation conversion catalyst. Compared with alkali metal salts and / or bases, the above-mentioned base without metal ions is partially ionized in an aqueous solution, and a part of the base still exists in the form of molecules. After the silicon oxide of the molecular sieve reacts with the base, this part of the unionized base is gradually ionized, which plays a role of pH buffering, so that the pH value of the solution remains stable, and no strong dissolution process occurs, thereby causing the collapse of the molecular sieve pores. Compared with complex directing agents containing quaternary ammonium ions such as tetrapropylammonium hydroxide and hexadecyl-trimethylammonium bromide, the present invention adopts a mixed alkaline solution of small molecule ammonia and small molecule simple organic base as a buffer solution, which can penetrate into the micropores or mesoporous cavities inside the molecular sieve crystal to cause acid-base neutralization reaction, so that the internal silicon oxide is removed, the connectivity of the micropores / mesoporous cavities is improved, and the internal mesoporous structure is increased.
[0026] It should be noted that the mixed alkaline solution used in the present invention does not play the role of a directing agent and / or a template agent. Due to the moderate alkalinity of the buffer solution, the solution is affected by the diffusion of the molecular sieve surface and pores, and the reaction occurs preferentially on the outer surface of the molecular sieve crystal, which reduces the particle size of the crystal particles, further increases the surface area, and shortens the diffusion distance within the crystal.
[0027] In the above method, in order to further improve the mesoporous properties of modified Y molecular sieve, in its preparation step, first vacuum heating pretreatment is carried out to unmodified Y molecular sieve, and the gas filled in the molecular sieve micropores and mesoporous channels is removed as much as possible, because this part of the gas is limited in the channel, causing alkaline solution to be difficult to enter the mesopores and micropores with smaller pore size, and the generation efficiency of mesoporous structure is relatively low, thereby affecting the improvement of mesoporous properties. Therefore, the present invention is preferentially pretreated to unmodified Y molecular sieve before mixed alkali solution treatment, and the air pressure of the environment in the container is reduced to less than 0.1 atmosphere, and gas is excluded as much as possible. After adding mixed alkali solution, the solution can be promoted to enter the mesopores and microporous structures with smaller pore size, and in the process of treatment, the mesopore generation efficiency and mesoporation index are significantly improved, which is very beneficial to the improvement of catalytic performance.
[0028] Since the entire alkali treatment process does not introduce metal elements, especially alkali metal elements, and ammonium / amine treatment and / or exchange are further performed during the modification process, so that the metal ion content is further reduced, the metal content of the modified Y molecular sieve is extremely low, and it can be directly used as an acidic component of a hydrocracking / conversion catalyst; the modified Y molecular sieve prepared by the present invention also has significantly enhanced mesoporous properties, while retaining a microporous structure, and the preparation method has the characteristics of low pollution, low cost, simple process, and low cost. The modified Y molecular sieve prepared by this method can be directly used as an acidic component of a cracking catalyst, and has excellent conversion capacity and higher middle distillate selectivity when used for heavy oil hydrocracking, and low light hydrocarbon component yield.
[0029] The hydrocracking catalyst of the present invention is preferably such that the SiO2 / Al2O3 molar ratio of the Y molecular sieve framework is 18-60.
[0030] Specifically, the silicon-aluminum ratio of the Y molecular sieve framework used in the present invention is 15 to 60, and the protective effect of aluminum atoms on silicon atoms is further weakened as the silicon-aluminum ratio of the molecular sieve increases. The use of organic small molecule bases can increase the pH value of the solution, which can overcome the weakened protective effect of aluminum atoms, thereby achieving the purpose of improving the mesoporous properties of the alkali treatment modification process.
[0031] The hydrocracking catalyst of the present invention is preferably such that, in step (3), the mass ratio of the mixed alkaline solution to the Y molecular sieve is 5 to 30:1, more preferably 5 to 10:1.
[0032] The hydrocracking catalyst of the present invention is preferably such that, in step (3), the reaction time is 15 minutes to 4 hours.
[0033] The hydrocracking catalyst of the present invention is preferably such that, in step (1), the pretreatment temperature is 35-400°C.
[0034] The hydrocracking catalyst of the present invention is preferably such that the original vacuum degree in the vacuum heating container is maintained during the process of adding the mixed alkali solution in step (3), and after the mixed alkali solution is added, air or nitrogen is filled into the vacuum heating container to restore the internal pressure to normal.
[0035] The hydrocracking catalyst of the present invention is preferably such that in step (3), the conditions of the drying and the calcining are: drying at 110-160° C. for 5-12 hours and calcining at 400-600° C. for 2-5 hours.
[0036] When the hydrocracking catalyst of the present invention is used to treat VGO, the reaction conditions are: in the presence of hydrogen, the hydrogen partial pressure is 10-20MPa, the reaction temperature is 350-420°C, the hydrogen-oil volume ratio is 800-1600, and the liquid hourly space velocity is 0.5-3.0h -1 .
[0037] The hydrocracking catalyst of the present invention is preferably that the Y molecular sieve is a USY molecular sieve obtained by hydrothermal treatment twice or more, or a Y molecular sieve obtained by dealumination and siliconization, or a Y molecular sieve obtained by hydrothermal treatment and dealumination and siliconization.
[0038] In the hydrocracking catalyst of the present invention, it is preferred that the active component is a metal of Group VIB and / or Group VIII, the Group VIB metal is at least one of molybdenum and tungsten, and the Group VIII metal is nickel.
[0039] The hydrocracking catalyst of the present invention preferably has a content of 13-28% of the Group VIB metal in oxide form and a content of 5-10% of the Group VIII metal in oxide form, based on the weight of the catalyst.
[0040] To this end, the present invention also provides a sulfided hydrocracking catalyst, which is prepared by the following steps: contacting the above hydrocracking catalyst with a sulfur-containing compound and / or a nitrogen-containing compound to prepare a sulfided hydrocracking catalyst.
[0041] The beneficial effects of the present invention are as follows:
[0042] The medium-oil type hydrocracking catalyst provided by the present invention adopts a mesoporous molecular sieve with strong ring-opening ability, namely a modified molecular sieve, to improve the properties of the hydrocracking product, produce high-quality ethylene cracking raw materials while producing intermediate distillate oil, reduce the BMCI of hydrogenation tail oil, and improve the liquid yield and jet fuel yield of hydrocracking. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1A This is the XRD diffraction spectrum of the unmodified molecular sieve Y-1 in Example 1.
[0044] Figure 1B This is the XRD diffraction spectrum of the modified molecular sieve MY-1 in Example 1.
[0045] Figure 2A This is the XRD diffraction spectrum of the unmodified molecular sieve Y-2 in Example 2.
[0046] Figure 2B This is the XRD diffraction spectrum of the modified molecular sieve MY-2 in Example 2.
[0047] Figure 3AThis is the XRD diffraction spectrum of the unmodified molecular sieve Y-3 in Example 3.
[0048] Figure 3B This is the XRD diffraction spectrum of the modified molecular sieve MY-3 in Example 3. DETAILED DESCRIPTION
[0049] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0050] Example 1
[0051] (1) Add 10.0 g of raw material Y-1 molecular sieve into a vacuum reactor, reduce the pressure in the reactor to 0.1 atmosphere and maintain it at 50°C; prepare 200 mL of an aqueous solution containing 0.05 mol / L ethylenediamine and 0.5 mol / L ammonia, add the aqueous solution into the reactor while maintaining the vacuum degree at 0.1 atmosphere, continue stirring for 10 minutes after the addition is completed, and then introduce air to restore the normal pressure state. Then, stir at 90°C for 5 hours, filter, dry, and calcine to obtain a modified Y molecular sieve free of metal ions, numbered MY-1.
[0052] The specific properties of Y-1 and MY-1 are shown in Table 1 and Figure 1A and Figure 1B As shown. Figure 1A and Figure 1B From the comparison, it can be seen that the positions of the diffraction peaks in the XRD spectrum after modification remain almost unchanged, the degree of reduction of the diffraction peaks is relatively low, and the relative crystallinity is 61%.
[0053] (2) 10 g of the MY-1 molecular sieve obtained in step (1) was mixed with 85.7 g of amorphous silica-alumina dry glue powder (dry basis 70%) and 30 g of a binder, and then shaped, dried and calcined to prepare 100 g of a carrier MZT-1;
[0054] (3) A metal impregnation solution containing 32 g of nickel nitrate hexahydrate and 49.3 g of ammonium metatungstate was prepared, and the support obtained in step (2) was fully contacted with the metal impregnation solution for impregnation, dried at 110° C. for 20 hours, and then calcined at 500° C. for 2 hours to obtain a hydrocracking catalyst MC-1, the composition of which is shown in Table 2.
[0055] Example 2
[0056] (1) Add 10.0 g of raw material Y-2 molecular sieve into a vacuum reactor, reduce the pressure in the reactor to 0.09 atmosphere and maintain it at 400°C; prepare 500 mL of an aqueous solution containing 0.5 mol / L 1-propylamine and 0.01 mol / L ammonia, add the aqueous solution into the reactor while maintaining the vacuum degree at 0.1 atmosphere, continue stirring for 15 minutes after the addition is completed, and then introduce air to restore the normal pressure state. Then, stir at 60°C for 3 hours, filter, dry, and calcine to obtain a modified Y molecular sieve free of metal ions, numbered MY-2.
[0057] The specific properties of Y-2 and MY-2 are shown in Table 1 and Figure 2A and Figure 2B As shown. Figure 2A and Figure 2B From the comparison, it can be seen that the positions of the diffraction peaks in the XRD spectrum after modification remain almost unchanged, the degree of reduction of the diffraction peaks is relatively low, and the relative crystallinity is 73%.
[0058] (2) 3 g of the MY-2 molecular sieve obtained in step (1) was mixed with 88.6 g of amorphous silica-alumina dry rubber powder (dry basis 70%) and 35 g of a binder, and then shaped, dried and calcined to prepare 100 g of a carrier MZT-2;
[0059] (3) A metal impregnation solution containing 26 g of nickel nitrate hexahydrate and 31 g of ammonium metatungstate was prepared, and the support obtained in step (2) was fully contacted and impregnated with the metal impregnation solution, dried at 140° C. for 8 hours, and then calcined at 350° C. for 6 hours to obtain a hydrocracking catalyst MC-2, the composition of which is shown in Table 2.
[0060] Example 3
[0061] (1) Add 33.0 g of raw material Y-3 molecular sieve into a vacuum reactor, reduce the pressure in the reactor to 0.05 atmosphere and maintain it at 200°C; prepare 100 mL of an aqueous solution containing 0.3 mol / L isopropylamine and 0.20 mol / L ammonia, add the aqueous solution into the reactor while maintaining the vacuum degree at 0.09 atmosphere, continue stirring for 5 minutes after the addition is completed, and then introduce air to restore the normal pressure state. Then, stir at 80°C for 10 minutes, filter, dry, and calcine to obtain a modified Y molecular sieve, numbered MY-3.
[0062] The specific properties of Y-3 and MY-3 are shown in Table 1 and Figure 3A and Figure 3B As shown. Figure 3A and Figure 3B From the comparison, it can be seen that the positions of the diffraction peaks in the XRD spectrum after modification remain almost unchanged, the degree of reduction of the diffraction peaks is relatively low, and the relative crystallinity is 85%.
[0063] (2) 20 g of the MY-3 molecular sieve obtained in step (1) was mixed with 42.8 g of amorphous silica-alumina dry rubber powder (dry basis 70%) and 50 g of a binder, and then shaped, dried and calcined to prepare 100 g of a carrier MZT-3;
[0064] (3) A metal impregnation solution containing 24.3 g of nickel nitrate hexahydrate and 21.8 g of ammonium heptamolybdate was prepared, and the support obtained in step (2) was fully contacted with the metal impregnation solution for impregnation, dried at 160° C. for 5 hours, and then calcined at 450° C. for 3 hours to obtain a hydrocracking catalyst MC-3, the composition of which is shown in Table 2.
[0065] Comparative Example 1
[0066] (1) Y-1 molecular sieve was treated according to the literature report (Catalyst Design by NH4OH Treatment of USY Zeolite, Adv. Funct. Mater., 2015, 25, 7130-7144).
[0067] Take 2.5g of Y-1 molecular sieve and add it to 200mL of ammonia solution with a concentration of 0.02mol / L. Stir at 250 rpm for 0.25 hours at room temperature, filter and wash 3 times, and then dry at 100℃. Calcination conditions: heat from room temperature to 200℃ at a rate of 2℃ / min and keep for 30min; then heat to 450℃ at a rate of 3℃ / min and keep for 30min. DY-1 molecular sieve is obtained. This condition is the best condition for the micropore volume of the modified molecular sieve in the literature.
[0068] (2) 0.5 g of DY-1 molecular sieve was mixed with 85.7 g of amorphous silica-alumina dry glue powder (dry basis 70%) and 39.5 g of a binder, and then shaped, dried and calcined to prepare a carrier ZT-1;
[0069] (3) A metal impregnation solution containing 32 g of nickel nitrate hexahydrate and 49.3 g of ammonium metatungstate was prepared, and the support obtained in step (2) was fully contacted with the metal impregnation solution for impregnation, dried at 110° C. for 20 hours, and then calcined at 500° C. for 2 hours to obtain a hydrocracking catalyst C-1.
[0070] Comparative Example 2
[0071] (1) Treating Y-2 molecular sieve by the method of Chinese patent CN201711119061.X, under stirring conditions, H-type USY molecular sieve and tetrapropylammonium hydroxide solution are mixed in a high-pressure reactor, nitrogen is introduced to control the system pressure at 0.5MPa, and then the temperature is raised to 60°C, and constant temperature stirring is continued for 2 hours, the pressure is released, cooled, and filtered until the pH value is less than 9, dried at 120°C for 13 hours, and calcined at 520°C for 3 hours to obtain a modified Y molecular sieve, numbered DY-3. The concentration of the tetrapropylammonium hydroxide solution is 0.12mol / L, and the mass ratio of the H-type USY molecular sieve to the water in the solution is 1:9. Modified Y molecular sieve DY-2 is obtained.
[0072] (2) 3 g of DY-2 molecular sieve was mixed with 88.6 g of amorphous silica-alumina dry glue powder (dry basis 70%) and 35 g of a binder, and then shaped, dried and calcined to prepare a carrier ZT-2;
[0073] (3) A metal impregnation solution containing 26 g of nickel nitrate hexahydrate and 31 g of ammonium metatungstate was prepared, and the support obtained in step (2) was fully contacted with the metal impregnation solution for impregnation, dried at 140° C. for 8 hours, and then calcined at 350° C. for 6 hours to obtain a hydrocracking catalyst C-2, the composition of which is shown in Table 2.
[0074] Comparative Example 3
[0075] (1) Modified Y molecular sieve was prepared by the method of Example 1 of CN104760973A.
[0076] Weigh 40 grams of NaY molecular sieve into a quartz reaction tube and introduce nitrogen. Set the nitrogen purge rate to 50 mL / min, and heat from room temperature to 500°C and maintain for 2 hours (heating time 100 minutes). Stop heating, cool naturally to 270°C, introduce nitrogen containing saturated SiCl4, and heat to 430°C at a heating rate of 4°C / min in 40 minutes, then stop introducing nitrogen containing saturated SiCl4, purge with high-purity nitrogen alone for 2 hours, then stop heating and cool naturally;
[0077] Take out the sample, wash and dry it to obtain the dealuminated silicon-filled molecular sieve;
[0078] Take 40g of dealuminated silicon-filled molecular sieve, add it into 400g of 0.5mol / L hydrochloric acid solution, heat it in a water bath at 80°C, stir it rapidly for 1 hour, filter it and wash it until the pH is close to neutral.
[0079] The filtered sample was directly added into 800 g of 0.2 mol / L sodium hydroxide solution, heated in a water bath at 70°C, stirred rapidly for 1 hour, filtered and washed until the pH value was close to neutral, and dried at 120°C overnight to obtain a Y-type molecular sieve with ultra-high mesoporous content, numbered DY-3.
[0080] (2) 20 g of DY-3 molecular sieve was mixed with 42.8 g of amorphous silica-alumina dry glue powder (dry basis 70%) and 50 g of a binder, and then shaped, dried and calcined to prepare a carrier ZT-3;
[0081] (3) A metal impregnation solution containing 24.3 g of nickel nitrate hexahydrate and 21.8 g of ammonium heptamolybdate was prepared, and the support obtained in step (2) was fully contacted with the metal impregnation solution for impregnation, dried at 160° C. for 5 hours, and then calcined at 450° C. for 3 hours to obtain a hydrocracking catalyst C-3, the composition of which is shown in Table 2.
[0082] Example 4
[0083] Evaluation of hydrocracking performance.
[0084] The evaluation device uses a 100mL small hydrogenation device. The catalyst is pre-sulfurized before the activity evaluation. Under a pressure of 15.0Mpa, the reaction temperature rises from room temperature to 140°C in 2 hours; when the reaction temperature reaches 140°C, sulfurized oil (2% DMDS) is introduced, and the temperature is increased after 4 hours of constant temperature. Then the temperature is increased to 220°C at a rate of 20°C / h, and the temperature is kept constant at 220°C for 8 hours. The temperature is continued to rise to 320°C at 20°C / h, and the temperature is kept constant at 320°C for 12 hours, and the sulfurization is completed. Subsequently, sulfurized oil is continued to be introduced, and after the temperature is increased to the set temperature at a rate of 30°C / h, the evaluation raw materials are switched and the evaluation is carried out.
[0085] The properties of the feedstock oil and the reaction process conditions used to evaluate the catalyst activity are shown in Tables 3 and 4, and the catalyst reaction performance comparison is shown in Table 5. When evaluating the catalyst, the feedstock oil first passes through the hydrofining catalyst bed and then directly enters the hydrocracking catalyst bed. When passing through the hydrofining catalyst bed, the organic nitrogen content in the feedstock oil is controlled to be less than 30 ppm.
[0086] Table 1 Properties of Y molecular sieves in the embodiments of the present invention and the comparative examples
[0087]
[0088]
[0089] Table 2 Catalyst composition
[0090] C-1 C-2 C-3 MC-1 MC-2 MC-3 Molecular sieve content in carrier, weight % 10 3 20 10 3 20 Amorphous silicon-aluminum content in the carrier, weight % 70 62 30 70 62 30 Binder content in carrier, weight % 20 35 50 20 35 50 NiO content in catalyst, weight % 6 5 5 6 5 5 WO3 content in catalyst, weight % 28 20 - 28 20 - MoO3 content in catalyst, weight % - - 15 - - 15
[0091] Table 3 Process conditions
[0092] Reaction pressure 15MPa Hydrogen to oil volume ratio 1200∶1 airspeed <![CDATA[1.5h -1 ]]>
[0093] Table 4 Raw material properties
[0094] project Analyze the results <![CDATA[Density (20 °C), g / cm 3 > 0.9205 Distillation range, ℃ 314-539 S, μg / g 10100 N, μg / g 1920 Carbon residue, wt% 0.18 Pour point, ℃ 33
[0095] Table 5 Catalyst reaction performance
[0096]
[0097]
[0098] The hydrocracking reaction results shown in Table 5 show that compared with the comparative catalyst, the catalyst of the present invention has lower reaction temperature, increased liquid yield, lower light naphtha yield, improved middle distillate selectivity, and greater improvement in tail oil BMCI when the conversion rate is the same, indicating that the hydrocracking catalyst prepared by the method of the present invention has better catalytic performance.
[0099] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.
Claims
1. A medium oil type hydrocracking catalyst, characterized in that: Taking the weight of the catalyst as 100wt%, the composition includes: 10-20wt% of modified Y molecular sieve, 30-70wt% of amorphous silicon-aluminum, 20-50wt% of binder and 25-35wt% of active metal, wherein the content of the active metal is calculated as its oxide; the total content of each component in the catalyst composition is 100wt%; The modified Y molecular sieve is a mesoporous modified Y molecular sieve, wherein the molar ratio of silicon oxide to aluminum oxide in the modified Y molecular sieve framework is 15-60, the sodium oxide content is less than 0.1wt%, the unit cell parameter is 2.430-2.438nm, the relative crystallinity is 60-100%, the crystal particle size is normally distributed with d as the center, wherein d is less than 500nm, and the mesoporous index M is 1.7-5.0, wherein M=(S ext / S micro )*(V meso / V micro ), S ext is the external specific surface area in the t-plot method in nitrogen adsorption and desorption determination, S micro is the micropore specific surface area in the t-plot method in nitrogen adsorption and desorption determination, V micro is the micropore volume in the t-plot method in nitrogen adsorption-desorption determination, V meso It is the total pore volume of the single point adsorption method in nitrogen adsorption-desorption measurement minus V micro The difference between The preparation method of the modified Y molecular sieve is as follows: (1) placing the Y molecular sieve in a vacuum heating container for pretreatment until the gas pressure in the container is reduced to less than 0.1 atmosphere; (2) preparing a mixed alkaline solution, wherein the concentration of the weak base ammonia is 0.01-0.50 mol / L and the concentration of another organic base is 0.05-0.5 mol / L; (3) adding the mixed alkali solution prepared in step (2) into the vacuum heating container in step (1), reacting at 40-95° C. for 10 minutes-5 hours, then filtering, washing, drying and calcining to obtain a modified Y molecular sieve; Wherein, the organic base is selected from at least one of methylamine, ethylamine, ethylenediamine, 1-propylamine, and isopropylamine, and the mass ratio of the mixed alkali solution to the Y molecular sieve is (3~50):
1.
2. The hydrocracking catalyst according to claim 1, characterized in that The micropore volume of the modified Y molecular sieve is ≥0.20 mL / g.
3. The hydrocracking catalyst according to claim 1, characterized in that The mesoporation index M is 2.0-5.
0.
4. The hydrocracking catalyst according to claim 3, characterized in that The mesoporation index M is 3.0-5.
0.
5. The hydrocracking catalyst according to claim 1, characterized in that The d is less than 450 nm.
6. The hydrocracking catalyst according to claim 5, characterized in that The d is less than 350 nm.
7. The hydrocracking catalyst according to claim 1, characterized in that The concentration of the organic base in the mixed alkaline solution is 0.1-0.5 mol / L.
8. The hydrocracking catalyst according to claim 1, characterized in that The SiO2 / Al2O3 molar ratio of the Y molecular sieve framework is 18-60.
9. The hydrocracking catalyst according to claim 1, characterized in that In step (3), the mass ratio of the mixed alkaline solution to the Y molecular sieve is (5-30):
1.
10. The hydrocracking catalyst according to claim 9, characterized in that In step (3), the mass ratio of the mixed alkaline solution to the Y molecular sieve is (5-10):
1.
11. The hydrocracking catalyst according to claim 1, characterized in that In step (3), the reaction time is 15 minutes to 4 hours.
12. The hydrocracking catalyst according to claim 1, characterized in that In step (1), the pretreatment temperature is 35-400°C.
13. The hydrocracking catalyst according to claim 1, characterized in that During the process of adding the mixed alkali solution in step (3), the original vacuum degree in the vacuum heating container is maintained. After the mixed alkali solution is added, air or nitrogen is filled into the vacuum heating container to restore the internal pressure to normal.
14. The hydrocracking catalyst according to claim 1, characterized in that The Y molecular sieve is a USY molecular sieve obtained through more than two hydrothermal treatments, or a Y molecular sieve obtained through dealumination and siliconization, or a Y molecular sieve obtained through hydrothermal treatment and dealumination and siliconization.
15. The hydrocracking catalyst according to claim 1, characterized in that The drying temperature is 110-160° C., and the drying time is 5-12 hours; the calcining temperature is 400-600° C., and the calcining time is 2-5 hours.
16. The hydrocracking catalyst according to claim 1, characterized in that The active metal is a metal of Group VIB and / or Group VIII, the Group VIB metal is at least one of molybdenum and tungsten, and the Group VIII metal is nickel.
17. The hydrocracking catalyst according to claim 16, characterized in that Based on 100 wt% of the weight of the catalyst, the content of the VIB Group metal in the form of oxide is 13-28%.
18. The hydrocracking catalyst according to claim 16, characterized in that Based on 100 wt% of the weight of the catalyst, the content of the Group VIII metal in the form of oxide is 5-10%.
19. A sulfided hydrocracking catalyst, characterized in that: The catalyst is prepared by the following steps: contacting the hydrocracking catalyst described in any one of claims 1 to 18 with a sulfur-containing compound, or with a sulfur-containing compound and a nitrogen-containing compound to prepare a sulfurized hydrocracking catalyst.