Magnesium removal agent for recycled aluminum, preparation method and use method thereof

By using magnesium removal agents prepared from raw materials such as sodium fluorosilicate, combined with ball mill stirring and granulation processes, the problem of excessive magnesium content in recycled aluminum is solved, achieving efficient magnesium removal, gas removal, and slag removal effects, and significantly reducing production costs. Hours and Usage.

CN114717426BActive Publication Date: 2024-10-29ZHEJIANG JINFEI KAIDA WHEEL
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210327977.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-30
Publication Date
2024-10-29
Estimated Expiration
2042-03-30

AI Technical Summary

Technical Problem

The impurity content in recycled aluminum is high and the magnesium content exceeds the standard. The existing magnesium removal agent is not effective and needs to be refined again, which increases production hours.

Method used

The magnesium removal agent is prepared using raw materials such as sodium fluorosilicate, aluminum fluoride, hexachloroethane, ammonium chloride, calcium chloride, and potassium chloride. Through drying, ball milling, stirring, and granulation screening processes, a high-density removal agent is formed. Magnesium agent is used to remove magnesium by powder spraying, control the temperature and gas pressure of the aluminum liquid, and ensure the effects of magnesium removal, gas removal and slag removal.

Benefits of technology

The magnesium removal effect is significantly improved, reaching one out of four to six, reducing usage and production hours, avoiding re-refining treatment, and significantly improving product quality and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114717426B_ABST
    Figure CN114717426B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of magnesium removal agent preparation, and specifically discloses a magnesium removal agent for recycled aluminum, a preparation method and a use method thereof, comprising 45-55% sodium fluorosilicate, 5-15% aluminum fluoride, 5-15% hexachloroethane, 3-12% ammonium chloride, 0-5% calcium fluoride, and the rest supplemented with potassium chloride to 100%. After drying and ball milling and stirring, each component is granulated into a granular flux. Fluoride salt and chloride salt react with magnesium, gas and inclusions in the melt at the same time, playing a good role in magnesium removal and refining. At the same time, the reaction products of calcium fluoride, potassium chloride and magnesium further improve the reaction effect and separation of the magnesium removal agent, and the aluminum slag is loose and non-sticky. At the same time, after granulation, the flux has a larger specific gravity, a longer floating time in the aluminum liquid, and a better reaction time and contact area in the aluminum liquid. The magnesium removal effect of the invention can reach four to six removals of one, and the amount of magnesium required for the same magnesium removal is reduced. At the same time, after using the same amount of magnesium removal agent, it is not necessary to spray powder and refine again, which effectively saves production time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of magnesium removal agent preparation, and in particular to a magnesium removal agent for recycled aluminum, a preparation method and a use method thereof. Background Art

[0002] Recycled aluminum is an aluminum alloy obtained by remelting, refining and purifying scrap aluminum and scrap aluminum alloy or aluminum-containing scrap. It is an important source of metallic aluminum. The sources of recycled aluminum raw materials are complex, mainly industrial depreciation scrap aluminum parts and scrap aluminum materials generated during aluminum processing, with high impurity content and complex composition. How to effectively remove impurities in recycled aluminum and effectively control its composition is the most critical point to determine the quality of recycled aluminum products.

[0003] The magnesium content in the die-cast aluminum alloys (ADC12, YZAlSi9Cu4, etc.) produced from recycled aluminum is required to be ≤0.3%, and the magnesium content in aluminum alloys such as ZL102 is ≤0.1%. As a zinc and iron-reducing material in recycled aluminum, cans have can lids and pull rings mainly made of 5 series aluminum alloys with high magnesium content, which can easily lead to excessive magnesium content in the aluminum liquid during use.

[0004] In order to solve the problem of high impurity content and excessive magnesium content in the recycled aluminum industry, the existing magnesium removal agents in the industry are usually made of a mixture of fluoride salt and chloride salt raw materials. The moisture control is not strictly prohibited, the product has a light specific gravity, and the bulk density is generally 1.1-1.2g / cm 3 The effect of use is basically ten divided by one (10kg of magnesium remover removes 1kg of magnesium), and the refining effect is poor. After magnesium removal, flux refining treatment must be carried out again, which increases production hours. Summary of the invention

[0005] The purpose of the present invention is to provide a magnesium removal agent for recycled aluminum, a preparation method and a method of using the same, which has the advantages of strong magnesium removal effect, small dosage, good degassing and slag removal effect, and at the same time, after using the same amount of magnesium removal agent, there is no need for powder spraying and refining again, which effectively saves production time.

[0006] In order to achieve the above object, the present invention adopts a magnesium removal agent for recycled aluminum, which is as follows according to the weight percentage of the formula:

[0007] Sodium fluorosilicate 45-55%; aluminum fluoride 5-15%; hexachloroethane 5-15%; ammonium chloride 3-12%; calcium fluoride 0-5%; the rest is supplemented with potassium chloride to 100%.

[0008] The present invention also proposes a method for preparing the above-mentioned magnesium removal agent for recycled aluminum, comprising the following steps:

[0009] The above raw materials are placed in a dryer and fully dried;

[0010] Then add the dried raw materials into the ball mill mixer according to the formula, and discharge the materials after being evenly milled;

[0011] Add the ball-milled material into the granulator for granulation, and select particles with a particle size of 0.5 to 2 mm;

[0012] The particles that are out of the required particle size will be re-entered into the granulator for granulation and screening;

[0013] The flux that meets the requirements is sealed and packaged.

[0014] The density of the qualified flux product is 1.28-1.35 g / cm 3 .

[0015] The present invention also provides a method for using a magnesium removal agent for recycled aluminum, using the above-mentioned magnesium removal agent for recycled aluminum, comprising the following steps:

[0016] Determine the excess magnesium content in the regenerated aluminum liquid and calculate the required weight of magnesium removal agent at a ratio of six to one;

[0017] Detect the temperature of aluminum liquid in the configuration furnace;

[0018] Turn on the refiner, add the required magnesium remover into the tank, and start powder spraying;

[0019] Spray the flux evenly to the middle and lower part of the melt. After powder spraying, let it stand and scrape off the slag, and check whether the composition is qualified.

[0020] Wherein, the temperature of the aluminum liquid when the flux is used is controlled at 700-750°C.

[0021] Among them, the inert gas pressure when starting powder spraying is controlled at 0.05-0.2MPa.

[0022] The powder spraying speed at the beginning of powder spraying is controlled at 1-2 kg / min.

[0023] Wherein, the inert gas is nitrogen or argon.

[0024] Wherein, in the step of uniformly spraying the flux to the lower middle part of the melt: the tumbling height of the aluminum liquid surface is controlled not to exceed 10 cm.

[0025] The magnesium removal agent for recycled aluminum of the present invention, the preparation method and the use method thereof, which uses fluoride salt, chloride salt and the like as raw materials, and is produced by drying, ball milling stirring, granulation screening and other processes, has a more uniform composition, a greater product density, a more intense reaction with aluminum liquid, a longer reaction time, and has good magnesium removal, degassing, and deslagging effects; at the same time, the present invention provides a method for using a magnesium removal agent suitable for recycled aluminum, giving full play to the advantages and effects of the product. The magnesium removal effect of the present invention can reach four to six removals of one (4 to 6 kg of magnesium removal agent for 1 kg of magnesium), which is about 40 to 60% higher than the existing products in the industry, significantly reducing the amount used by customers, and at the same time, the degassing and deslagging effects are significant, and after using the same amount of magnesium removal agent, it is not necessary to spray powder and refine again, effectively saving about 0.5 to 1 hour of production time. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 It is a flow chart of the method for preparing the magnesium removal agent for recycled aluminum of the present invention. DETAILED DESCRIPTION

[0028] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and are not to be construed as limitations of the present invention. In addition, in the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0029] See also Figure 1 The present invention provides a magnesium removal agent for recycled aluminum, which is as follows according to the weight percentage of the formula:

[0030] Sodium fluorosilicate 45-55%; aluminum fluoride 5-15%; hexachloroethane 5-15%; ammonium chloride 3-12%; calcium fluoride 0-5%; the rest is supplemented with potassium chloride to 100%.

[0031] The present invention also proposes a method for preparing the above-mentioned magnesium removal agent for recycled aluminum, comprising the following steps:

[0032] The above raw materials are placed in a dryer and fully dried; wherein, the dryer is used to first dry the raw materials, which can effectively remove the water remaining in the raw materials and prepare for subsequent ball milling;

[0033] Then, the dried raw materials are added to the ball mill mixer according to the formula, and the materials are discharged after being evenly mixed by ball milling. By mixing various raw materials and adding them to the ball mill, the raw materials can be evenly mixed while being ball milled by the ball mill, thus saving the raw material mixing step.

[0034] The ball-milled material is added to the granulator for granulation, and particles with a particle size of 0.5 to 2 mm are screened out; granulation is achieved in the granulator, and a 0.5 to 2 mm sieve plate is set for the particles to pass through, so as to unify the particle size and ensure the quality uniformity of the granular material.

[0035] Particles outside the particle size requirements are re-entered into the granulator for granulation and screening; this is conducive to recycling particles that do not meet the particle size requirements and preparing particles that meet the particle size requirements, thereby saving production costs.

[0036] The flux that meets the requirements is sealed and packaged. By sealing the flux, the air can be effectively isolated to prevent air from oxidizing the flux and affecting the efficacy and quality of the flux.

[0037] The density of the qualified flux product is 1.28-1.35 g / cm 3 After the flux is manufactured and before it needs to be sealed and packaged, the density of the product needs to be tested and the density needs to be controlled within 1.28-1.35 g / cm 3, This helps to ensure the effectiveness of the flux.

[0038] The present invention also provides a method for using a magnesium removal agent for recycled aluminum, using the above-mentioned magnesium removal agent for recycled aluminum, comprising the following steps:

[0039] Determine the excess magnesium content in the regenerated aluminum liquid and calculate the required weight of the magnesium remover at a ratio of six to one; determine the magnesium content in the regenerated aluminum liquid through testing, and then add the magnesium remover according to the ratio to prevent the addition of excess magnesium remover, which will cause waste of raw materials and increase costs.

[0040] Detect the temperature of aluminum liquid in the configuration furnace;

[0041] Turn on the refiner, add the required magnesium remover into the tank, and start powder spraying;

[0042] Spray the flux evenly to the middle and lower part of the melt. After powder spraying, let it stand and scrape off the slag, and check whether the composition is qualified.

[0043] When the flux is used, the temperature of the aluminum liquid is controlled at 700-750° C. By controlling the temperature of the aluminum liquid in the furnace within a range, and determining the range as the optimal range for controlling the aluminum liquid temperature after testing, it is beneficial to remove the magnesium content in the regenerated aluminum liquid.

[0044] The inert gas pressure at the start of powder spraying is controlled at 0.05-0.2 MPa. The powder spraying speed at the start of powder spraying is controlled at 1-2 kg / min. By controlling the inert gas pressure and the powder spraying speed, it can be ensured that the powder spraying adheres better to the middle and lower part of the melt.

[0045] The inert gas is nitrogen or argon.

[0046] In the step of uniformly spraying the flux to the middle and lower part of the melt: the tumbling height of the aluminum liquid is controlled to be no more than 10 cm. By controlling the tumbling height of the aluminum liquid, it is beneficial to control the powder spraying quality.

[0047] The above raw materials are placed in a dryer for thorough drying to ensure that the moisture content is ≤ 0.25%.

[0048] In the step of discharging the material after uniform stirring by ball milling: the ball milling time is 30 minutes.

[0049] In the step of standing still after powder spraying is completed: the standing time is 10 to 20 minutes.

[0050] Embodiment 1:

[0051] A magnesium removal agent for recycled aluminum and a method for using the same, wherein the composition ratio is: 52% sodium fluorosilicate; 10% aluminum fluoride; 10% hexachloroethane; 5% ammonium chloride; 3% calcium fluoride; and 20% potassium chloride.

[0052] The preparation process mainly includes:

[0053] S1: Place the raw materials in a dryer and fully dry them to ensure that the moisture content is ≤ 0.25%;

[0054] S2: Add the dried raw materials into the ball mill according to the formula requirements, and discharge the materials after 30 minutes of ball milling and stirring;

[0055] S3: Add the ball-milled material into a granulator for granulation, set the upper screen to 2 mm, the lower screen to 0.5 mm, and screen out particles that meet the particle size requirements;

[0056] S4: Particles outside the particle size requirement are re-entered into the granulator for granulation and screening;

[0057] S5: The product density is 1.31g / cm 3 , the flux that meets the requirements is sealed and packaged, with a net weight of 1kg per package.

[0058] It is used in ZL102 aluminum liquid (magnesium content is required to be ≤0.1%) in a 600kg crucible furnace with recycled aluminum. The specific method of use is as follows:

[0059] The composition of the aluminum liquid after batching was measured. The actual weight of the aluminum liquid was about 570kg, and its magnesium content was 0.216%. Theoretically, more than 0.66kg of magnesium needed to be removed, so 3kg of magnesium removal agent was prepared;

[0060] The aluminum liquid temperature in the detection configuration furnace is 738℃;

[0061] Turn on the refiner, add the required magnesium removal agent into the tank, start powder spraying, and control the powder spraying pressure at 0.05MPa;

[0062] Spray the flux evenly to the middle and lower part of the melt, control the liquid level to not exceed 10cm, and spray for 3 minutes;

[0063] After the powder spraying is completed, let it stand for 20 minutes before removing the slag. Take a sample from 1 / 2 of the bottom of the crucible center for testing.

[0064] The pinhole degree of the ingot casting test before the furnace reached level 1, the magnesium content was 0.095%, the actual magnesium removal was 0.69 kg, and the magnesium removal efficiency was 4.34 kg of magnesium removal agent to remove 1 kg of magnesium. After meeting the requirements, water was taken to cast the ingot.

[0065] This solves the problem of high impurity content and excessive magnesium content in the recycled aluminum industry. The existing magnesium removal agents in the industry are usually mixed with fluoride salt and chloride salt raw materials. The moisture control is not strictly prohibited. The product has a light specific gravity and the bulk density is generally 1.1-1.2g / cm 3 The effect of use is basically ten divided by one (10kg of magnesium remover removes 1kg of magnesium), and the refining effect is poor. After magnesium removal, flux refining treatment must be carried out again, which increases the production time.

[0066] Embodiment 2:

[0067] A magnesium removal agent for recycled aluminum and a use method thereof, wherein the composition ratio is: 55% sodium fluorosilicate; 10% aluminum fluoride; 10% hexachloroethane; 5% ammonium chloride; 5% calcium fluoride; and 15% potassium chloride.

[0068] The preparation process mainly includes:

[0069] S1: Place the raw materials in a dryer and fully dry them to ensure that the moisture content is ≤ 0.25%;

[0070] S2: Add the dried raw materials into the ball mill according to the formula requirements, and discharge the materials after 30 minutes of ball milling and stirring;

[0071] S3: Add the ball-milled material into a granulator for granulation, set the upper screen to 2 mm, the lower screen to 0.5 mm, and screen out particles that meet the particle size requirements;

[0072] S4: Particles outside the particle size requirement are re-entered into the granulator for granulation and screening;

[0073] S5: The product density is 1.32g / cm 3 , the flux that meets the requirements is sealed and packaged, with a net weight of 5kg per package.

[0074] It is used in a 25-ton recycled aluminum configuration furnace. The specific usage is as follows:

[0075] Determine the composition of the aluminum liquid after batching (ADC12, magnesium content required ≤ 0.3%). The actual weight of the aluminum liquid is about 25 tons, and its magnesium content is 0.332%. Theoretically, more than 7.7 kg of magnesium needs to be removed, and 60 kg of magnesium removal agent is prepared;

[0076] The aluminum liquid temperature in the detection configuration furnace is 716℃;

[0077] Turn on the refiner, add the required magnesium removal agent into the tank, start powder spraying, and control the powder spraying pressure at 0.14MPa;

[0078] Spray the flux evenly to the middle and lower part of the melt, control the liquid level to not exceed 10cm, and spray powder for 30 minutes;

[0079] After the powder spraying is completed, let it stand for 15 minutes before removing the slag, and take samples from the middle of the melt at 1 / 2 radius inward from the center of the furnace door for testing;

[0080] The pinhole degree of the ingot casting test before the furnace reached the second level, the magnesium content was 0.290%, the actual magnesium removal was 10.53kg, and the magnesium removal efficiency was 5.7kg of magnesium removal agent to remove 1kg of magnesium. After meeting the requirements, water was added to cast the ingot.

[0081] In summary, the magnesium removal agent produced by drying, ball milling, granulation and screening with fluoride salts and chloride salts as raw materials has a more uniform composition, a larger product density, a more intense reaction with aluminum liquid, a longer reaction time, and good magnesium removal, degassing, and deslagging effects; at the same time, the present invention provides a method for using a magnesium removal agent suitable for recycled aluminum, giving full play to the advantages and effects of this product. The magnesium removal effect of the present invention can reach four to six removals of one (4 to 6 kg of magnesium removal agent for 1 kg of magnesium), which is about 40 to 60% higher than the existing products in the industry, significantly reducing the amount used by customers, and at the same time, the degassing and deslagging effects are significant. After using the same amount of magnesium removal agent, there is no need to spray powder and refine again, which effectively saves about 0.5 to 1 hour of production time.

[0082] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A method for using a magnesium removal agent for recycled aluminum, characterized in that: The preparation method of the magnesium removal agent for recycled aluminum comprises the following steps: The weight percentage of the formula is: 45-55% sodium fluorosilicate; 5-15% aluminum fluoride; 5-15% hexachloroethane; 3-12% ammonium chloride; 0-5% calcium fluoride; the rest is supplemented with potassium chloride to 100%; The above raw materials are placed in a dryer and fully dried to ensure that the moisture content is ≤ 0.25%; Then add the dried raw materials into the ball mill according to the formula, and discharge the materials after ball milling and stirring evenly. The ball milling time is 30 minutes; The ball-milled material is added to the granulator for granulation, and particles with a particle size of 0.5 to 2 mm are screened out; The particles that are out of the required particle size will be re-entered into the granulator for granulation and screening; Test the density of the flux and control the density between 1.28 and 1.35 g / cm 3, Seal and package the flux that meets the requirements; The method for using the magnesium removal agent for recycled aluminum comprises the following steps: Determine the excess magnesium content in the regenerated aluminum liquid and calculate the required weight of magnesium removal agent at a ratio of six to one; Detect the temperature of aluminum liquid in the configuration furnace; Turn on the refiner, add the required magnesium remover into the tank, and start powder spraying; Spray the flux evenly to the middle and lower part of the melt. After spraying, let it stand for 10 to 20 minutes and remove the slag, and check whether the composition is qualified. In the step of uniformly spraying the flux to the lower middle part of the melt: the tumbling height of the aluminum liquid surface is controlled not to exceed 10 cm.

2. The method for using the magnesium removal agent for recycled aluminum according to claim 1, characterized in that: The temperature of the aluminum liquid is controlled at 700-750°C when the flux is used.

3. The method for using the magnesium removal agent for recycled aluminum according to claim 2, characterized in that: The inert gas pressure at the beginning of powder spraying is controlled at 0.05-0.2Mpa.

4. The method for using the magnesium removal agent for recycled aluminum according to claim 3, characterized in that: When starting to spray powder, the spraying speed is controlled at 1-2 kg / min.

5. The method for using the magnesium removal agent for recycled aluminum according to claim 4, characterized in that: The inert gas is nitrogen or argon.

Citation Information

Patent Citations

  • Powder spraying, refining and calcium removing method used for aluminium alloy material

    CN102912169A

  • Slag remover for refining Al or Al alloy

    CN1073486A

  • Fluoride-free chlorine-free environment-friendly granular refining agent for aluminum alloy as well as preparation and application of fluoride-free chlorine-free environment-friendly granular refining agent

    CN112048634A