A preparation method and application of conductive hydrogel
By introducing graphene oxide into acrylamide-acrylic acid copolymer to form a composite, the problem of insufficient mechanical properties and conductivity of conductive hydrogels is solved, the potential of high-sensitivity and flexible sensors is realized, and the stretchability of the material is significantly improved. magnification and conductivity.
Patent Information
- Application Number
- CN202210596041.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-05-30
AI Technical Summary
Existing conductive hydrogels have deficiencies in mechanical properties, conductivity, and sensing sensitivity, making it difficult to meet the flexibility and high-sensitivity needs of new electronic devices and medical equipment.
By introducing graphene oxide into the copolymer of acrylamide and acrylic acid, and through steps such as ultrasonic dispersion, heating reduction, and initiating free radical polymerization, a conductive hydrogel based on acrylamide-acrylic acid copolymer/graphene composite is formed, using hydrogen The bonding effect improves the mechanical properties and electrical conductivity of the material.
The mechanical properties and electrical conductivity of the material are significantly improved, and the sensing sensitivity is improved, making it suitable for the application of flexible sensors. It can maintain conductive properties under high stretch ratios and significantly improve the electrical conductivity.
Smart Images

Figure CN114773632B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a conductive hydrogel and a preparation method thereof, and belongs to the field of polymer materials. Background Art
[0002] Sensors have been used in all aspects of life and production, becoming an indispensable component in production and life. With the development of society and the advancement of science and technology, a wider range of application fields urgently need new sensors with stronger adaptability and more diverse functions. Among them, sensor materials used in new electronic equipment, medical equipment, etc. have high demands for their flexibility and high sensitivity.
[0003] Conductive hydrogel is a functional hydrogel. Due to its unique conductivity, high water content and flexibility, it has great application potential in medical patches, health monitoring materials, wearable electronics, sensors, actuators, etc.; but at present, it is still very challenging to construct hydrogels with good mechanical properties, high conductivity and high sensing sensitivity. Summary of the invention
[0004] The present invention provides a preparation method of a conductive hydrogel and application thereof, the purpose of which is to improve the mechanical properties and conductivity of the existing acrylamide and acrylic acid copolymer hydrogel.
[0005] The technical solution of the present invention is a method for preparing a conductive hydrogel, the method comprising:
[0006] (1) adding graphene oxide to water, dispersing it by ultrasonication, and then adding ascorbic acid to heat and reduce it under heating and stirring to obtain a uniformly dispersed reduced graphene oxide suspension;
[0007] (2) Add acrylamide and acrylic acid to the reduced graphene oxide suspension, add an initiator and a cross-linking agent after dissolution, and heat in an oven to initiate free radical polymerization to obtain a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite.
[0008] Furthermore, the mass ratio of the graphene oxide to water is (0.06-0.1):100, preferably (0.07-0.09):100; the mass ratio of ascorbic acid to graphene oxide is 3:1.
[0009] Furthermore, the heating reduction condition is 80°C~100°C for 2h-4h, preferably 88ºC~92ºC for 3h.
[0010] Furthermore, the mass ratio of the sum of the mass of acrylic acid and acrylamide to water is 0.6:1; the mass ratio of the added acrylic acid to acrylamide is (1.2-3.0):(3.0-4.8), and the mass ratio of acrylic acid to acrylamide is preferably 1:4.
[0011] Furthermore, the mass ratio of the sum of the mass of acrylamide and acrylic acid added to the crosslinker is (400-600):1, preferably 500:1; the mass ratio of the sum of the mass of acrylamide and acrylic acid added to the initiator is (50-70):1, preferably 60:1.
[0012] Furthermore, the oven heating condition is 50°C~60°C for reaction for 10 h~14 h, preferably 54ºC~57ºC for reaction for 12 h.
[0013] Furthermore, during the initiation of free radical polymerization, the amino and carboxyl groups of the acrylamide-acrylic acid copolymer and the groups on the reduced graphene oxide form a composite structure through hydrogen bonding.
[0014] Furthermore, the water is preferably ultrapure water.
[0015] Furthermore, the cross-linking agent is preferably MBA (N,N-methylenebisacrylamide).
[0016] Furthermore, the initiator is preferably ammonium persulfate.
[0017] Furthermore, the conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite is suitable for use as a flexible sensing material.
[0018] Beneficial effects of the present invention:
[0019] Compared with common polyacrylamide hydrogels, the conductive hydrogel material prepared by the present invention has obvious improvements in mechanical properties, conductivity and sensing sensitivity, and has the potential to be applied to new flexible sensors. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Attached Figure 1 The stretching ratio-stress curves of the conductive hydrogels based on acrylamide-acrylic acid copolymer / graphene composite prepared in Examples 1-4 when stretched to fracture are shown.
[0021] Attached Figure 2 This is a sensitivity calculation diagram of the conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite prepared in Example 1.
[0022] Attached Figure 3 This is a sensitivity calculation diagram of the conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite prepared in Example 4.
[0023] Attached Figure 4 This is a comparison chart of the calculated electrical conductivity of the conductive hydrogels based on acrylamide-acrylic acid copolymer / graphene composites prepared in Example 1 and Example 4.
[0024] Attached Figure 5 This is a schematic diagram of a flexible sensor made of the conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite prepared in Example 1 to verify its feasibility of flexible sensing. DETAILED DESCRIPTION
[0025] A method for preparing a conductive hydrogel, the method comprising the following steps:
[0026] (1) adding graphene oxide to ultrapure water and dispersing by ultrasonication to obtain a graphene oxide dispersion, then adding ascorbic acid to the graphene oxide dispersion and performing heating reduction under heating and stirring to obtain a uniformly dispersed reduced graphene oxide suspension;
[0027] (2) Acrylamide and acrylic acid are added to the reduced graphene oxide suspension in sequence under stirring. After dissolution, ammonium persulfate and MBA (N,N-methylenebisacrylamide) are added. The mixture is transferred to a mold and placed in an oven for heating to initiate free radical polymerization to obtain a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite.
[0028] In step (1), the mass ratio of the added graphene oxide to ultrapure water is (0.06-0.1):100, preferably (0.07-0.09):100; the mass ratio of the added ascorbic acid to graphene oxide is 3:1.
[0029] In the step (1), the heating reduction condition is 80°C~100°C for 2h-4h, preferably 88ºC~92ºC for 3h.
[0030] In the step (2), the reduced graphene oxide suspension is obtained after heating and reduction in the step (1).
[0031] In the step (2), the mass ratio of the sum of the mass of the added acrylic acid and acrylamide to the mass of ultrapure water is preferably 0.6:1; the mass ratio of the added acrylic acid to acrylamide is (1.2-3.0):(3.0-4.8), and the mass ratio of acrylic acid to acrylamide is preferably 1:4.
[0032] In the step (2), the mass ratio of the sum of the mass of acrylamide and acrylic acid added to MBA is (400-600):1, preferably 500:1; the mass ratio of the sum of the mass of acrylamide and acrylic acid added to ammonium persulfate is (50-70):1, preferably 60:1.
[0033] In the step (2), the heating condition in the oven is 50°C to 60°C for 10 h to 14 h, preferably 54°C to 57°C for 12 h.
[0034] The mold in step (2) can be selected according to actual conditions, and the conductive hydrogel of the acrylamide-acrylic acid copolymer / graphene composite can be prepared in different molds.
[0035] In the preparation method provided by the present invention, firstly, graphene oxide is reduced to obtain a reduced graphene oxide suspension, preferably under the condition of oil bath heating, acrylamide and acrylic acid are added as monomers to the reduced graphene oxide suspension, ammonium persulfate is added as an initiator, MBA is added as a cross-linking agent, and free radical polymerization is initiated under heating to obtain a conductive hydrogel of an acrylamide-acrylic acid copolymer / graphene composite; in the process of heating-initiated free radical polymerization, the amino and carboxyl groups of the acrylamide-acrylic acid copolymer and the groups on the flaky reduced graphene oxide form a composite structure through hydrogen bonding,
[0036] The amino and carboxyl groups of the acrylamide-acrylic acid copolymer in the conductive hydrogel composite material prepared by the present invention and the groups on the flaky reduced graphene oxide form a composite three-dimensional structure through hydrogen bonding, and the composite structure has good mechanical properties and conductivity.
[0037] The conductive hydrogel composite material prepared by the preparation method provided by the present invention is a conductive hydrogel material based on an acrylamide-acrylic acid copolymer / graphene composite; by adjusting the ratio of acrylamide and acrylic acid in the acrylamide-acrylic acid copolymer and introducing the hydrogen bonding effect between the reduced oxide graphene and the acrylamide-acrylic acid copolymer, the mechanical properties of the material are greatly superior to those of the hydrogel having only acrylamide and acrylic acid copolymer. Figure 1 As shown in Figure 1, a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite prepared in Example 1 of the present invention (the sample corresponding to curve 1) can be stretched to more than 20 times its original length without breaking, which is much better than the acrylamide-acrylic acid copolymer hydrogel without adding graphene (the sample corresponding to curve 4); at the same time, the unique sheet structure of graphene provides a good conductive path for the composite material. Figure 4 The conductivity of the conductive hydrogel material (sample 2) of the acrylamide-acrylic acid copolymer / graphene composite prepared in Example 1 was demonstrated and compared with the acrylamide and acrylic acid copolymer hydrogel (sample 1) without graphene. The conductivity was increased by nearly 3 times, which makes the material sensitive to resistance changes when subjected to stress, that is, it has good sensing sensitivity.
[0038] The conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite prepared by the present invention is a black opaque hydrogel that can be stretched to more than 15 times its original length (such as the attached Figure 1 As shown in the figure), the sensor sensitivity (GF)>2 in the stretching range of 100%-400% (as shown in the figure) Figure 2 as shown).
[0039] The present invention uses acrylamide as a substrate and forms a copolymer by free radical polymerization with a certain proportion of acrylic acid. At the same time, highly conductive reduced oxide graphene is introduced into the synthesis process to be compounded with the high molecular polymer chain. The presence of graphene effectively improves the conductivity and sensing sensitivity of the hydrogel.
[0040] The conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite is suitable for use as a flexible sensing material.
[0041] The present invention is described in detail below in conjunction with the embodiments and the accompanying drawings.
[0042] Example 1
[0043] A method for preparing a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite comprises the following steps:
[0044] 1) Graphene oxide reduction process: 0.008 g of graphene oxide was added to 10 ml of ultrapure water, and ultrasonically dispersed in an ultrasonic instrument for 2 h to obtain a graphene oxide dispersion. Then, 0.024 g of ascorbic acid was added and heated and stirred at 90°C in an oil bath for 3 h to obtain a reduced graphene oxide suspension. After heating, the mixture was naturally cooled to room temperature.
[0045] 2) Synthesis process of composite hydrogel: 4.8 g acrylamide and 1.2 g acrylic acid are added to the reduced graphene oxide suspension obtained in step 1) under stirring and dissolved, and then 0.1 g ammonium persulfate and 0.012 g MBA are added. After stirring and dissolving, the mixed solution is transferred to a mold and placed in an oven and heated at 55°C for 12 hours to obtain a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite.
[0046] Attached Figure 1 Curve 1 in the figure is the elongation ratio-stress curve of the conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite synthesized in Example 1 when stretched to fracture. The hydrogel prepared in Example 1 can be stretched to more than 2000% of the original length without fracture, which is much better than the acrylamide-acrylic acid copolymer hydrogel without adding graphene (as shown in curve 4). Figure 2 The sensing sensitivity of the conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite was demonstrated when it was stretched to 400% of its original length. Figure 3The sensing sensitivity of the acrylamide-acrylic acid copolymer prepared in Example 4 when stretched to 400% of the original length is compared with that in Example 1. The sensing sensitivity (GF) of the conductive hydrogel of the acrylamide-acrylic acid copolymer / graphene composite is much higher than that of the acrylamide-acrylic acid copolymer hydrogel without adding graphene. Figure 4 Sample 1 is the conductivity of the hydrogel prepared in Example 4, and sample 2 is the conductivity of the hydrogel prepared in Example 1. By comparison, it can be found that the addition of graphene increases the conductivity by nearly 3 times.
[0047] Example 2
[0048] A method for preparing a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite comprises the following steps:
[0049] 1) Graphene oxide reduction process: 0.006 g of graphene oxide was added to 10 ml of ultrapure water, and ultrasonically dispersed in an ultrasonic instrument for 2 h to obtain a graphene oxide dispersion. Then, 0.018 g of ascorbic acid was added and heated and stirred at 85°C in an oil bath for 2.5 h to obtain a reduced graphene oxide suspension. After heating, the mixture was naturally cooled to room temperature.
[0050] 2) Synthesis process of composite hydrogel: 4.0 g acrylamide and 2.0 g acrylic acid are added to the reduced graphene oxide suspension obtained in step 1) under stirring and dissolved, and then 0.088 g ammonium persulfate and 0.01 g MBA are added. After stirring and dissolving, the mixed solution is sucked into a syringe mold and placed in an oven and heated at 50°C for 14 hours to obtain a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite.
[0051] Attached Figure 1 Curve 2 in FIG. 1 is the elongation ratio-stress curve of the hydrogel synthesized in Example 2 when stretched to break.
[0052] Example 3
[0053] A method for preparing a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite comprises the following steps:
[0054] 1) Graphene oxide reduction process: 0.010 g of graphene oxide was added to 10 ml of ultrapure water, and ultrasonically dispersed in an ultrasonic instrument for 2 h to obtain a graphene oxide dispersion. Then, 0.030 g of ascorbic acid was added and heated and stirred at 95°C in an oil bath for 3.4 h to obtain a reduced graphene oxide suspension. After heating, the mixture was naturally cooled to room temperature.
[0055] 2) Synthesis process of composite hydrogel: 3 g acrylamide and 3 g acrylic acid are added to the reduced graphene oxide suspension obtained in step 1) under stirring and dissolved, and then 0.12 g ammonium persulfate and 0.015 g MBA are added. After stirring and dissolving, the mixed solution is sucked into a syringe mold and placed in an oven and heated at 60°C for 10 hours to obtain a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite.
[0056] Attached Figure 1 Curve 3 in FIG. 3 is the elongation ratio-stress curve of the hydrogel synthesized in Example 3 when stretched to break.
[0057] Example 4
[0058] The preparation method of acrylamide-acrylic acid copolymer hydrogel comprises the following steps:
[0059] 1) Hydrogel synthesis process: 4.8 g acrylamide and 1.2 g acrylic acid were added to 10 ml ultrapure water under stirring, and after dissolution, 0.1 g ammonium persulfate and 0.012 g MBA were added respectively, and after stirring and dissolving, the mixed solution was sucked into a syringe mold, and placed in an oven and heated at 55°C for 12 hours to obtain acrylamide-acrylic acid copolymer hydrogel.
[0060] Attached Figure 2 Curve 4 in FIG. 4 is the elongation ratio-stress curve of the hydrogel synthesized in Example 4 when stretched to break.
[0061] Attached Figure 3 The sensor sensitivity calculation diagram of the hydrogel prepared in Example 4 is shown in FIG. Figure 4 Sample 1 is the conductivity of the hydrogel prepared in Example 4, Figure 4 Sample 2 is the conductivity of the acrylamide-acrylic acid copolymer / graphene composite hydrogel prepared in Example 1.
[0062] Example 5
[0063] The conductive hydrogel materials based on acrylamide-acrylic acid copolymer / graphene composite were tested for mechanics, sensing sensitivity and conductivity.
[0064] The hydrogel materials prepared in Examples 1-4 were tested for their mechanical properties on a stretching machine (Instason-5967). The specific test method was as follows: clamp the two ends of the hydrogel with the clamps on the stretching machine, stretch the hydrogel vertically at a rate of 100 cm / min until it breaks, and record the curve of the hydrogel stretching ratio-vertical stress. The results are shown in the attached figure. Figure 1 As shown:
[0065] The stretching machine was connected with a Tonghui bridge (TH2830), and the sensing sensitivity of the material was calculated by measuring the change in the relative resistance of the hydrogel materials prepared in Example 1 and Example 4 during the stretching process. The calculation formula is:
[0066] GF = ΔR / R0 / ΔL;
[0067] Where ΔR is the change in hydrogel resistance during stretching, R0 is the initial resistance of the hydrogel before stretching, and ΔR / R0 is the relative resistance of the hydrogel during stretching. Figure 2 , Attachment Figure 3 The ordinate in the figure is ΔL, which is the change in the relative resistance (ΔR / R0) during the stretching process of the hydrogel, corresponding to the change in the stretching ratio. Figure 2 , Attachment Figure 3 The horizontal axis in .
[0068] The conductivity of the hydrogel materials prepared in Example 1 and Example 4 was measured using an electrochemical workstation (AutolabPGSTAT302N), and the calculation formula was:
[0069] σ = L / (R×S);
[0070] Where L is the height of the hydrogel, S is the cross-sectional area, and R is the measured hydrogel resistance; the test results are shown in the attached Figure 4 As shown, the conductivity of the conductive hydrogel material (sample 2) of the acrylamide-acrylic acid copolymer / graphene composite prepared in Example 1 is nearly 3 times higher than that of the acrylamide and acrylic acid copolymer hydrogel (sample 1) without graphene.
[0071] Example 6
[0072] The conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite prepared in Example 1 was attached to the joints of a dummy as a flexible sensor material to conduct a verification test on the feasibility of flexible sensing. Figure 5 The conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite is applied to the back of a dummy's neck, and the resistance curve of the conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite as the neck bends is shown; it can be seen that as the neck bends back and forth, the resistance of the conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite fluctuates significantly, which can indicate that the conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite has good motion sensing performance and is fully suitable for use as a flexible sensing material.
Claims
1. A conductive hydrogel is used as a flexible sensing material, characterized in that The preparation method of the conductive hydrogel comprises: Step 1) Reduction process of graphene oxide: 0.008 g of graphene oxide was added to 10 ml of ultrapure water, and ultrasonically dispersed in an ultrasonic instrument for 2 hours to obtain a graphene oxide dispersion, and then 0.024 g of ascorbic acid was added and heated and stirred at 90° C. in an oil bath for 3 hours to obtain a reduced graphene oxide suspension. After heating, the suspension was naturally cooled to room temperature; Step 2) Synthesis process of composite hydrogel: 4.8 g acrylamide and 1.2 g acrylic acid are added to the reduced graphene oxide suspension obtained in step 1) under stirring and dissolved, and then 0.1 g ammonium persulfate and 0.012 g MBA are added. After stirring and dissolving, the mixed solution is transferred to a mold and placed in an oven and heated at 55°C for 12 hours to obtain a conductive hydrogel based on acrylamide-acrylic acid copolymer / graphene composite.