A method for preparing a nitrogen / graphene / carbon carrier composite material and a positive electrode material, a positive electrode and a lithium ion battery prepared therefrom
By using nitrogen/graphene/carbon carrier composite materials as sulfur carriers, the problems of low sulfur utilization and poor cycle stability in lithium-sulfur batteries are solved, achieving high specific energy density and excellent electrochemical performance, especially during cycling Performance and magnification performance have been significantly improved.
Patent Information
- Application Number
- CN202210571914.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-24
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-05-24
AI Technical Summary
The practical application of lithium-sulfur batteries faces problems such as low utilization of active material sulfur, poor cycle stability, low Coulombic efficiency, and safety needs to be evaluated. This is mainly due to the poor conductivity of sulfur elements and the shuttle effect caused by polysulfides being easily soluble in organic electrolytes. Electrode volume changes.
Nitrogen/graphene/carbon carrier composite materials are used as sulfur carriers, and graphene and nitrogen modified carbon carriers are used to construct high-specific surface area mesoporous materials, which provide loading space and adsorption sites, and reduce the shuttle of polysulfides, thus Improve the electrochemical performance of the battery.
The cycle performance and rate performance of lithium-ion batteries are significantly improved. The first discharge capacity is above 955mAh/g. The capacity retention rate exceeds 60% after 100 cycles, and the reduction in electrolyte volume is effectively avoided.
Smart Images

Figure CN114784254B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new energy battery materials, and specifically relates to a method for preparing a nitrogen / graphene / carbon carrier composite material and a positive electrode material, a positive electrode and a lithium ion battery prepared therefrom. Background Art
[0002] Lithium-ion batteries have become a battery system with better performance in modern commercial rechargeable batteries due to their inherent advantages. They mainly use lithium iron phosphate, lithium manganese phosphate and nickel-cobalt-manganese ternary complex as positive electrode materials, with a theoretical capacity of about 300mAh g -1 Therefore, this type of battery can no longer meet the energy needs of portable devices, especially car batteries. Therefore, cathode materials with high specific energy density are the research focus of various countries today. Lithium-sulfur batteries have attracted much attention due to their high energy density, and their specific capacity can reach 1675mAh·g -1 .
[0003] The active material of the positive electrode material of lithium-sulfur batteries is sulfur. Sulfur has the advantages of low cost and no pollution due to its high abundance in nature, environmental friendliness and non-toxicity. However, the practical application of lithium-sulfur batteries faces some obstacles, such as the poor conductivity of elemental sulfur (5×10 -30 S cm -1 ), the intermediate polysulfide in the charge and discharge reaction is easily soluble in the organic electrolyte, causing the shuttle effect, and the large change in electrode volume before and after the reaction (~80%). There are still many challenges in its commercialization, mainly the low utilization rate of active sulfur, poor cycle stability, low coulombic efficiency and safety to be evaluated. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a nitrogen / graphene / carbon carrier composite material, which utilizes graphene and introduces N elements to modify the carbon carrier, which has a high specific surface area and strong adsorption capacity, can provide loading space for sulfur and polysulfides and adsorb them, reduce polysulfide shuttling, and thus improve the electrochemical performance of the battery.
[0005] The present invention also aims to provide a nitrogen / graphene / carbon / sulfur composite positive electrode material and a preparation method thereof, in which sulfur is loaded in the pores of a nitrogen / graphene / carbon carrier composite material with a high specific surface area, thereby reducing polysulfide shuttling and improving the electrochemical performance of the battery.
[0006] The present invention also aims to provide a lithium-ion battery positive electrode and a lithium-ion battery, wherein the lithium-ion battery positive electrode is prepared using a nitrogen / graphene / carbon / sulfur composite positive electrode material as an active substance, and then assembled into a lithium-ion battery with excellent cycle performance and rate performance.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a nitrogen / graphene / carbon carrier composite material, the preparation method comprising the following steps:
[0009] (1) dissolving resorcinol in a mixed solution of anhydrous ethanol and ultrapure water, adding concentrated hydrochloric acid and urea, stirring and reacting for 1 to 1.5 hours, then adding formaldehyde solution dropwise thereto, and continuing to stir and react for 1 to 1.5 hours;
[0010] (2) adding the graphene suspension to step (1), stirring and reacting for 10 to 12 hours, transferring the resulting mixed solution into a closed reactor, and reacting at 65 to 75° C. for 10 to 12 hours to obtain an organic wet gel;
[0011] (3) The organic wet gel obtained in step (2) is dried, washed, dried again, and then carbonized in an inert atmosphere to obtain a nitrogen / graphene / carbon carrier composite material.
[0012] The molar ratio of resorcinol to formaldehyde is 1:2-3; the concentration of the formaldehyde solution is 0.3-0.5 g / mL.
[0013] The molar ratio of urea to resorcinol is 1:5-20; the mass ratio of graphene to resorcinol is 1:30-150.
[0014] The preparation method of the graphene suspension is as follows: ultrasonically dispersing graphene in deionized water at a ratio of 1 g: 50-100 mL.
[0015] The volume ratio of the anhydrous ethanol to the ultrapure water is 1:1; the concentration of the resorcinol in the mixed solution is 0.05-0.5 g / mL.
[0016] The volume fraction of the concentrated hydrochloric acid is 37%; the volume ratio of the mixed solution formed by the concentrated hydrochloric acid, anhydrous ethanol and ultrapure water is 1:15-30.
[0017] In step (3), the carbonization reaction conditions are: in an argon atmosphere, at 3-8°C min -1 The heating rate is increased to 650-850℃ and kept at this temperature for 3-5h.
[0018] The invention provides a method for preparing a nitrogen / graphene / carbon / sulfur composite positive electrode material, comprising the following steps: mixing and grinding the nitrogen / graphene / carbon carrier composite material prepared by the preparation method with sulfur, placing the mixture in a closed reactor, keeping the mixture at 140-160° C. for 8-24 hours, then opening the upper cover of the reactor, keeping the mixture at 170-185° C. for 2-5 hours, and naturally cooling the mixture to obtain the nitrogen / graphene / carbon / sulfur composite positive electrode material.
[0019] The mass ratio of the nitrogen / graphene / carbon carrier composite material to sulfur is 1:1.5-3.
[0020] The present invention adopts a two-stage heating method to prepare a nitrogen / graphene / carbon / sulfur composite positive electrode material. During the first stage of heating, the sulfur molecules can be fully impregnated into the pores of the porous carbon material; the second stage of heating can remove excess sulfur molecules on the surface of the sulfur-carbon composite after impregnation, so as to ensure that in the first charge and discharge cycle of the battery sample, no sulfur molecules attached to the surface of the composite combine with the electrolyte to form polysulfides, thereby effectively avoiding a reduction in the amount of electrolyte.
[0021] The present invention also provides a nitrogen / graphene / carbon / sulfur composite positive electrode material prepared by the preparation method.
[0022] The present invention provides a lithium ion battery positive electrode, which is prepared using the nitrogen / graphene / carbon / sulfur composite positive electrode material as an active material.
[0023] The present invention provides a lithium ion battery, which is assembled using the lithium ion battery positive electrode as the positive electrode.
[0024] In the technical solution provided by the present invention, graphene and nitrogen are used to modify the carbon carrier. After the nitrogen modification, a basic conductive network can be constructed. The modification of graphene reduces the internal resistance of the battery, improves the battery efficiency and the voltage platform, and the modified nitrogen / graphene / carbon carrier composite material has a high specific surface area and a strong adsorption capacity. It is a mesoporous material with a pore size concentrated in 3-4nm and a specific surface area of more than 980㎡ / g. It can provide a loading space for sulfur and polysulfide and adsorb them, reduce the polysulfide shuttle, and thus improve the electrochemical performance of the battery. A lithium ion battery positive electrode is prepared using the nitrogen / graphene / carbon / sulfur composite positive electrode material of the present invention as an active material, and then assembled into a lithium ion battery with excellent cycle performance and rate performance. At a current density of 0.2C, the battery has an initial discharge capacity of more than 955mAh / g, and at a rate of 0.2C, after 100 cycles, its capacity retention rate is more than 60%. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a flow chart of the lithium-ion battery assembly in the present invention;
[0026] Figure 2 This is a curve diagram of the number of cycles and discharge capacity of the lithium-sulfur battery in Example 3. DETAILED DESCRIPTION
[0027] The present invention is described in detail below with reference to the embodiments.
[0028] In each embodiment: the volume ratio of anhydrous ethanol to ultrapure water is 1:1; the volume fraction of concentrated hydrochloric acid is 37%; the concentration of formaldehyde solution is 0.37 g / mL; the preparation method of graphene suspension is: ultrasonically disperse graphene in deionized water at a ratio of 1 g:50 mL.
[0029] Example 1
[0030] A method for preparing a nitrogen / graphene / carbon carrier composite material comprises the following steps:
[0031] (1) 11 g of resorcinol was dissolved in a mixed solution of 100 mL of anhydrous ethanol and ultrapure water, 5 mL of concentrated hydrochloric acid and 0.5 g of urea were added, and the mixture was stirred in a sealed manner at room temperature for 1 h. Then 15 mL of formaldehyde solution was added dropwise, and the mixture was stirred and reacted for 1 h under the same conditions;
[0032] (2) adding 5 mL of graphene suspension to step (1), stirring and reacting for 12 h, transferring the resulting mixed solution into a closed reactor, and reacting at 70 ° C. for 12 h to obtain an organic wet gel;
[0033] (3) The organic wet gel obtained in step (2) was dried and cooled to room temperature, washed with water and centrifuged three times, and dried in a forced air drying oven at 80°C for 12 h. The obtained material was then placed in a tube furnace and incubated at 5°C min-1 in an argon atmosphere. -1 The heating rate is increased to 750°C and carbonized for 5 hours to obtain the nitrogen / graphene / carbon carrier composite material.
[0034] The nitrogen / graphene / carbon carrier composite material prepared in this example and sublimated S were mixed in a mass ratio of 4:6, placed in a mortar and fully ground, then placed in a 50 ml closed reactor, and kept warm in a forced air drying oven at a temperature of 155° C. for 16 h. Then, the upper cover of the reactor was opened, heated to 180° C. and kept warm for 3 h, and naturally cooled to obtain a nitrogen / graphene / carbon / sulfur composite positive electrode material.
[0035] The nitrogen / graphene / carbon / sulfur composite positive electrode material, acetylene black, and PVDF prepared in this embodiment are mixed in a mass ratio of 8:1:1, and after being evenly ground, N-methylpyrrolidone (NMP) is added, and the mixture is stirred for 15 hours to form a slurry, and then evenly coated on a glass plate with aluminum foil, placed in a vacuum drying oven at 65°C and dried for 15 hours, and the dried electrode pieces are cut into a size of 1cm×1cm, and the electrode pieces are placed under a device with a pressure of 30MPa to obtain electrode pieces. The positive electrode shell, positive electrode sheet, diaphragm, 40μL electrolyte, lithium sheet, gasket, shrapnel, and negative electrode shell are placed in a glove box, and finally the battery is placed under a positive pressure of 500Pa, and the battery is placed in a positive pressure with the positive electrode facing downward and the negative electrode facing upward, and the assembly is completed by standing for 12 hours. The assembly process is as follows: Figure 1 shown.
[0036] The battery was tested for electrochemical properties such as charge and discharge using an electrochemical workstation. The electrochemical test results showed that the battery performance was significantly improved. At a current density of 0.2C, the first discharge capacity of the lithium-sulfur battery was 955mAh / g. At a rate of 0.2C, the capacity retention rate was 80.5% after 100 cycles.
[0037] Example 2
[0038] A method for preparing a nitrogen / graphene / carbon carrier composite material comprises the following steps:
[0039] (1) 11 g of resorcinol was dissolved in a mixed solution of 100 mL of anhydrous ethanol and ultrapure water, 5 mL of concentrated hydrochloric acid and 0.6 g of urea were added, and the mixture was stirred in a sealed manner at room temperature for 1 h. Then 15 mL of formaldehyde solution was added dropwise, and the mixture was stirred and reacted for 1 h under the same conditions;
[0040] (2) adding 10 mL of graphene suspension to step (1), stirring and reacting for 12 h, transferring the resulting mixed solution into a closed reactor, and reacting at 75 ° C. for 10 h to obtain an organic wet gel;
[0041] (3) The organic wet gel obtained in step (2) was dried and cooled to room temperature, washed with water and centrifuged three times, and dried in a forced air drying oven at 80°C for 12 h. The obtained material was then placed in a tube furnace and incubated at 5°C min-1 in an argon atmosphere. -1 The heating rate is increased to 750°C and carbonized for 5 hours to obtain the nitrogen / graphene / carbon carrier composite material.
[0042] The nitrogen / graphene / carbon carrier composite material prepared in this example was used to prepare a nitrogen / graphene / carbon / sulfur composite positive electrode material in the same manner as in Example 1. A positive electrode sheet was prepared in the same manner as in Example 1 and assembled into a lithium-sulfur battery.
[0043] The battery was tested for electrochemical properties such as charge and discharge using an electrochemical workstation. The electrochemical test results showed that the battery performance was significantly improved. At a current density of 0.2C, the first discharge capacity of the lithium-sulfur battery was 985mAh / g. At a rate of 0.2C, the capacity retention rate was 81.6% after 100 cycles.
[0044] Example 3
[0045] A method for preparing a nitrogen / graphene / carbon carrier composite material comprises the following steps:
[0046] (1) 11 g of resorcinol was dissolved in a mixed solution of 100 mL of anhydrous ethanol and ultrapure water, 5 mL of concentrated hydrochloric acid and 0.5 g of urea were added, and the mixture was stirred in a sealed manner at room temperature for 1 h. Then 15 mL of formaldehyde solution was added dropwise, and the mixture was stirred and reacted for 1 h under the same conditions;
[0047] (2) adding 7.5 mL of graphene suspension to step (1), stirring and reacting for 12 h, transferring the resulting mixed solution into a closed reactor, and reacting at 75 ° C. for 10 h to obtain an organic wet gel;
[0048] (3) The organic wet gel obtained in step (2) was dried and cooled to room temperature, washed with water and centrifuged three times, and dried in a forced air drying oven at 80°C for 12 h. The obtained material was then placed in a tube furnace and incubated at 5°C min-1 in an argon atmosphere. -1 The heating rate is increased to 750°C and carbonized for 5 hours to obtain the nitrogen / graphene / carbon carrier composite material.
[0049] The nitrogen / graphene / carbon carrier composite material prepared in this example was used to prepare a nitrogen / graphene / carbon / sulfur composite positive electrode material in the same manner as in Example 1. A positive electrode sheet was prepared in the same manner as in Example 1 and assembled into a lithium-sulfur battery.
[0050] The electrochemical performance test of the battery, such as charge and discharge, was carried out using an electrochemical workstation. The electrochemical test results showed that the battery performance was significantly improved. At a current density of 0.2C, the first discharge capacity of the lithium-sulfur battery was 1086mAh / g. At a rate of 0.2C, the capacity retention rate was 87.9% after 100 cycles. Figure 2 shown.
[0051] Example 4
[0052] A method for preparing a nitrogen / graphene / carbon carrier composite material comprises the following steps:
[0053] (1) 11 g of resorcinol was dissolved in a mixed solution of 100 mL of anhydrous ethanol and ultrapure water, 5 mL of concentrated hydrochloric acid and 0.7 g of urea were added, and the mixture was stirred in a sealed manner at room temperature for 1 h. Then 15 mL of formaldehyde solution was added dropwise, and the mixture was stirred and reacted for 1 h under the same conditions;
[0054] (2) adding 15 mL of graphene suspension to step (1), stirring and reacting for 12 h, transferring the resulting mixed solution into a closed reactor, and reacting at 75 ° C. for 10 h to obtain an organic wet gel;
[0055] (3) The organic wet gel obtained in step (2) was dried and cooled to room temperature, washed with water and centrifuged three times, and dried in a forced air drying oven at 80°C for 12 h. The obtained material was then placed in a tube furnace and incubated at 5°C min-1 in an argon atmosphere. -1 The heating rate is increased to 750°C and carbonized for 5 hours to obtain the nitrogen / graphene / carbon carrier composite material.
[0056] The nitrogen / graphene / carbon carrier composite material prepared in this example was used to prepare a nitrogen / graphene / carbon / sulfur composite positive electrode material in the same manner as in Example 1. A positive electrode sheet was prepared in the same manner as in Example 1 and assembled into a lithium-sulfur battery.
[0057] The battery was tested for electrochemical properties such as charge and discharge using an electrochemical workstation. The electrochemical test results showed that the battery performance was significantly improved. At a current density of 0.2C, the first discharge capacity of the lithium-sulfur battery was 1023mAh / g. At a rate of 0.2C, the capacity retention rate was 83.6% after 100 cycles.
[0058] Comparative Example 1
[0059] A method for preparing a carbon / sulfur composite positive electrode material comprises the following steps:
[0060] (1) 11 g of resorcinol was dissolved in a mixed solution of 100 mL of anhydrous ethanol and ultrapure water, 5 mL of concentrated hydrochloric acid was added, and the mixture was stirred in a sealed container at room temperature for 1 h. Then 15 mL of formaldehyde solution was added dropwise thereto, and the mixture was stirred and reacted for 1 h under the same conditions;
[0061] (2) transferring the solution in step (1) into a closed reactor and reacting at 70° C. for 12 h to obtain an organic wet gel;
[0062] (3) The organic wet gel obtained in step (2) was dried and cooled to room temperature, washed with water and centrifuged three times, and dried in a forced air drying oven at 80°C for 12 h. The obtained material was then placed in a tube furnace and incubated at 5°C min-1 in an argon atmosphere. -1 The carbon aerogel material, i.e., the carbon carrier material, can be obtained by increasing the heating rate to 750°C and carbonizing for 5 hours.
[0063] The carbon support material prepared in this comparative example and sublimated S were mixed in a mass ratio of 4:6, placed in a mortar and fully ground, then placed in a 50 ml closed reactor, and kept warm in a forced air drying oven at a temperature of 155° C. for 16 hours. Then, the upper cover of the reactor was opened, heated to 180° C. and kept warm for 3 hours, and naturally cooled to obtain a carbon / sulfur composite positive electrode material.
[0064] The carbon / sulfur composite positive electrode material prepared in this comparative example was used to prepare a positive electrode sheet in the same manner as in Example 1, and the positive electrode sheet was assembled into a lithium-sulfur battery.
[0065] The battery was tested for electrochemical properties such as charge and discharge using an electrochemical workstation. At a current density of 0.2C, the initial discharge capacity of the lithium-sulfur battery was only 839.5mAh / g. At a rate of 0.2C, its capacity retention rate was only 72.3% after 100 cycles.
[0066] The detailed description of the preparation method of a nitrogen / graphene / carbon carrier composite material and the positive electrode material, positive electrode and lithium-ion battery prepared therefrom by the above reference embodiments is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A method for preparing a nitrogen / graphene / carbon carrier composite material, characterized in that: The preparation method comprises the following steps: (1) Dissolve resorcinol in a mixed solution of anhydrous ethanol and ultrapure water, add concentrated hydrochloric acid and urea, stir and react for 1 to 1.5 hours, then add formaldehyde solution dropwise, and continue stirring and reacting for 1 to 1.5 hours; (2) adding the graphene suspension to step (1), stirring and reacting for 10 to 12 hours, transferring the resulting mixed solution into a closed reactor, and reacting at 65 to 75° C. for 10 to 12 hours to obtain an organic wet gel; (3) drying, washing, and drying again the organic wet gel obtained in step (2), and then carbonizing it in an inert atmosphere to obtain a nitrogen / graphene / carbon carrier composite material; The molar ratio of urea to resorcinol is 1:5-20; the mass ratio of graphene to resorcinol is 1:30-150; The volume ratio of the anhydrous ethanol to ultrapure water is 1:1; The volume ratio of the mixed solution formed by the concentrated hydrochloric acid, anhydrous ethanol and ultrapure water is 1:15-30.
2. The preparation method according to claim 1, characterized in that: The molar ratio of resorcinol to formaldehyde is 1:2-3; the concentration of the formaldehyde solution is 0.3-0.5 g / mL.
3. The preparation method according to claim 1, characterized in that: The concentration of resorcinol in the mixed solution is 0.05-0.5 g / mL.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The volume fraction of the concentrated hydrochloric acid is 37%.
5. The preparation method according to claim 1, characterized in that: In step (3), the carbonization reaction conditions are: in an argon atmosphere, at 3-8°C min -1 The heating rate is increased to 650~850℃ and kept at this temperature for 3~5 h.
6. A method for preparing a nitrogen / graphene / carbon / sulfur composite positive electrode material, characterized in that: The preparation method comprises the following steps: mixing and grinding the nitrogen / graphene / carbon carrier composite material prepared by the preparation method according to any one of claims 1 to 5 with sulfur, placing the mixture in a closed reactor, keeping the mixture at 140-160° C. for 8-24 h, then opening the upper cover of the reactor, keeping the mixture at 170-185° C. for 2-5 h, and naturally cooling the mixture to obtain a nitrogen / graphene / carbon / sulfur composite positive electrode material.
7. The nitrogen / graphene / carbon / sulfur composite positive electrode material prepared by the preparation method according to claim 6.
8. A positive electrode for a lithium ion battery, characterized in that: The lithium-ion battery positive electrode is prepared using the nitrogen / graphene / carbon / sulfur composite positive electrode material described in claim 7 as an active material.
9. A lithium ion battery, characterized in that: The lithium-ion battery is assembled using the lithium-ion battery positive electrode according to claim 8 as the positive electrode.