A flotation method for low-grade refractory ilmenite by dissolution pretreatment

Through dissolution pretreatment with acidic chemicals, the problem of complex and difficult separation of fine-grained ilmenite is solved, the sorting efficiency of ilmenite and concentrate grade are improved, and the selective flotation of ilmenite and gangue minerals is realized. Efficient separation reduces collector dosage.

CN114789086BActive Publication Date: 2024-10-29CHANGSHA RES INST OF MINING & METALLURGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210455269.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-27
Publication Date
2024-10-29
Estimated Expiration
2042-04-27

AI Technical Summary

Technical Problem

The existing technology has low efficiency in ilmenite with complex and difficult particle size. The mudification and metal ion adsorption of gangue minerals reduce the flotation effect of ilmenite, and the dissociation of ilmenite monomer is difficult, resulting in the separation effect. Not good.

Method used

The dissolution pretreatment method is used to dissolve metal ions on the surface of gangue minerals and attached ions on the surface of ilmenite through acidic chemicals, reduce the adsorption sites of the collector, clean the surface of ilmenite, enhance its flotation properties, and improve sorting. efficiency.

Benefits of technology

It significantly improves the sorting efficiency of ilmenite and concentrate grade, reduces the amount of collector, and achieves selective flotation and efficient separation of ilmenite and gangue minerals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114789086B_ABST
    Figure CN114789086B_ABST
Patent Text Reader

Abstract

The invention provides a flotation method for low-grade refractory ilmenite dissolution pretreatment, comprising the following steps: (1) adding water to ilmenite weak magnetic separation iron tailings for grinding to obtain grinding products; subjecting the grinding products to weak magnetic separation, and subjecting the obtained weak magnetic separation tailings to strong magnetic separation to obtain strong magnetic coarse concentrate; adding water to the strong magnetic coarse concentrate for grinding to obtain reground strong magnetic coarse concentrate; adding water to the reground strong magnetic coarse concentrate for slurrying, stirring, and obtaining slurry I; (2) sedimentation of slurry I, removal of upper slurry water, further addition of water for slurrying, addition of acid, stirring, and obtaining slurry II; (3) sedimentation of slurry II, removal of upper slurry water, further addition of water for slurrying, addition of acid, stirring, and obtaining slurry III; (4) sedimentation of slurry III, removal of upper slurry water, further addition of water for slurrying, and subjecting the obtained slurry to ilmenite flotation to obtain ilmenite concentrate. The present invention significantly improves the ilmenite separation efficiency, significantly improves the ilmenite concentrate grade and recovery rate, and can significantly reduce the amount of collector used.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ore dressing, and in particular relates to a flotation method for dissolution pretreatment of low-grade refractory ilmenite. Background Art

[0002] Titanium is a typical strategic key metal, an indispensable raw material in modern industry and cutting-edge technology, and is widely used in steel, aerospace, ocean, ultrasound, vehicle engineering, biomedical engineering and other fields, among which new titanium materials in military industry and aerospace are particularly eye-catching. As the main mineral phase of titanium metal, ilmenite is increasingly characterized by "poor, fine and impure". The efficiency of magnetic, gravity and electric beneficiation processes is limited by the particle size, and the effect of separation on fine-grained complex and difficult-to-separate ilmenite is extremely limited. Flotation is an important method to solve the problem of efficient separation of fine-grained complex and difficult-to-separate ilmenite.

[0003] Ilmenite is often associated with a large number of various silicate and carbonate gangues that are easy to muddy, such as pyroxene, amphibole, serpentine, chlorite, dolomite, etc. The muddy gangue covers each other and has a covering effect on ilmenite, reducing the flotation difference between ilmenite and gangue minerals. At the same time, the broken surfaces of gangue minerals such as pyroxene, amphibole, serpentine, chlorite, dolomite, etc. contain certain metal ions. These metal ions will become active sites for ilmenite flotation collectors to adsorb on the surface of gangue minerals in the acidic flotation system. The more active sites, the greater the amount of adsorbed collectors, which not only consumes a large amount of collectors, but also greatly reduces the selectivity of collectors, and the sorting effect becomes worse. On the other hand, it is difficult to dissociate ilmenite monomers. Gangue is embedded in the surface of ilmenite with a wide and thin surface layer to form a rich intergrowth. When a large number of ilmenite monomers are dissociated in the actual grinding process, the over-grinding phenomenon is serious. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the shortcomings and defects mentioned in the above background technology and provide a flotation method for low-grade and difficult-to-select ilmenite by dissolution pretreatment. The dissolution pretreatment can be used to perform surface pretreatment on the rich intergrowth ilmenite, thereby reducing the influence of the rich intergrowth embedded gangue on the flotation properties of the ilmenite. The method of the present invention can dissolve the metal ions on the surface of the gangue minerals, reduce the adsorption sites of the collector, and clean the ions and gangue minerals attached to the surface of the ilmenite, thereby improving the sorting effect of the ilmenite, significantly improving the sorting efficiency of the ilmenite, significantly improving the grade and recovery rate of the ilmenite concentrate, and significantly reducing the amount of collector used.

[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0006] A flotation method for low-grade refractory ilmenite by dissolution pretreatment, comprising the following steps:

[0007] (1) adding water to the weak magnetic separation iron tailings of ilmenite to grind the ore to obtain a grinding product; subjecting the grinding product to weak magnetic separation, and then subjecting the obtained weak magnetic separation tailings to strong magnetic separation to obtain a strong magnetic coarse concentrate; then adding water to the strong magnetic coarse concentrate to grind the ore to obtain a re-ground strong magnetic coarse concentrate; adding water to the re-ground strong magnetic coarse concentrate to prepare a slurry, stirring, and obtaining slurry I;

[0008] (2) sedimenting the slurry I, removing the upper slurry water, adding water to adjust the slurry, and then adding acid and stirring to obtain slurry II;

[0009] (3) sedimenting the slurry II, removing the upper slurry water, adding water to adjust the slurry, and then adding acid and stirring to obtain slurry III;

[0010] (4) The slurry III is sedimented, the upper slurry water is removed, water is added to adjust the slurry, and then the obtained slurry is subjected to ilmenite flotation to obtain ilmenite concentrate.

[0011] The present invention processes the weak magnetic separation iron tailings of ilmenite through a specific process, and then adds certain acidic chemicals to dissolve a large amount of carbonate and silicate gangue minerals, especially the surface structural calcium and magnesium atoms of gangue minerals in ilmenite intergrowths, which can reduce the action sites of anionic collectors on the surface of gangue minerals and inhibit the adsorption of anionic collectors on the surface of gangue minerals; at the same time, the acidic chemicals dissolve and clean the surface of ilmenite minerals, so that the calcium and magnesium atoms or muddy gangue minerals attached to the ilmenite are dissolved and cleaned and released, exposing more structural titanium and iron atoms of the ilmenite, and the collector can selectively and stably adsorb on the surface of the ilmenite, thereby enhancing the selective hydrophobic flotation of ilmenite. The technical principle theoretical model diagram of the present invention is as follows Figure 1 shown.

[0012] The present invention performs a second dissolution on the basis of the first dissolution to ensure that the dissolution is completed, so that the pH of the ore pulp solution is between 6 and 8, which is basically within the neutral pH range, and at the same time has a dispersing effect on the dissolves, which is beneficial to the removal of the dissolves.

[0013] Preferably, in step (1), the grinding product has a grinding fineness of -75 μm and a particle size content of 65 to 100% of the total grinding amount; and the ilmenite monomer content (dissociation degree) of the reground strong magnetic coarse concentrate is above 55%, and the total content of monomers and rich intergrowth bodies is greater than 90%.

[0014] In the reground strong magnetic coarse concentrate, some ilmenite exists in the form of monomers, and some exist in the form of intergrowths. Intergrowths are divided into rich intergrowths and poor intergrowths. Rich intergrowths refer to ilmenite accounting for more than 3 / 4 of the whole mineral particles. The effect of subsequent dissolution and cleaning on monomers is to clean the surface, and the effect on rich intergrowths is to selectively dissolve the gangue components in the rich intergrowths of ilmenite, making it closer to the properties of ilmenite.

[0015] Preferably, in step (1), during the stirring, the stirring speed is 1.0 to 3.5 m / s and the stirring time is 5 to 30 min, so that the strong magnetic rough concentrate reaches a dissolution equilibrium in a solution with a natural pH of 6 to 8 to obtain slurry I.

[0016] The above stirring can accelerate the cleaning of the ilmenite surface and speed up the mineral dissolution equilibrium. At this time, the ions dissolved in the slurry solution are mainly calcium and magnesium ions, and other ions such as iron, aluminum, and titanium are relatively less dissolved.

[0017] In the preferred step (2), the stirring is firstly carried out for 1 to 3 minutes to uniformly stir the acid and the slurry, at which time the pH value of the obtained slurry solution is 3 to 5, and the stirring is continued for 5 to 10 minutes to obtain slurry II;

[0018] In step (3), the stirring is first performed for 1 to 3 minutes to uniformly mix the acid and the slurry. At this time, the pH value of the obtained slurry solution is 6 to 8. Stirring is continued for 5 to 10 minutes to obtain slurry III.

[0019] After the ilmenite and the added acidic compound fully react, the surface of the ilmenite is cleaned, and calcium and magnesium ions are dissolved in large quantities and quickly. The dissolved calcium and magnesium ions exist in the slurry solution in the form of ions or soluble complexes. At the same time, the iron, aluminum and titanium ions of the mineral are dissolved less. Through the above stirring, the ilmenite and the added acid fully react, which promotes the cleaning of the ilmenite surface and dissolves the active ions on the surface of the gangue mineral with relatively good dissolution.

[0020] In step (2) and step (3) of the present invention, when the upper layer of clarified ore pulp water is removed after dissolution equilibrium, calcium and magnesium ions are reduced. Removing the upper layer of clarified aqueous solution containing dissolved ions can effectively reduce the non-selective adsorption of dissolved ions on the mineral surface and reduce the difference in mineral sortability.

[0021] Preferably, in step (2), the amount of the acid added is 1000 to 3000 g / t; in step (3), the amount of the acid added is 500 to 1500 g / t;

[0022] In step (2) and step (3), the acid is one or more of sulfuric acid, hydrochloric acid, oxalic acid, citric acid, tartaric acid, malic acid, maleic acid, and lactic acid.

[0023] Preferably, in step (1), water is added to the ilmenite weak magnetic iron tailings to make the ore mass concentration of 50-80%; when regrinding, water is added to the strong magnetic coarse concentrate to make the ore mass concentration of 50%-80%; after the water is added for slurrying, the ore mass concentration is 30-40%.

[0024] Preferably, in step (2), the sedimentation time of slurry I is 3 to 10 minutes; after the water is added to adjust the slurry, the mass concentration of the ore is 30 to 40%; in step (3), the sedimentation time of slurry II is 3 to 10 minutes; after the water is added to adjust the slurry, the mass concentration of the ore is 30 to 40%; in step (4), the sedimentation time of slurry III is 3 to 10 minutes; after the water is added to adjust the slurry, the mass concentration of the ore is 30 to 40%.

[0025] Preferably, in step (4), the slurry is introduced into a flotation machine for ilmenite flotation, and the flotation includes one roughing selection, one scavenging selection, and two cleaning selections.

[0026] Preferably, sulfuric acid is added as a pH adjuster during the flotation, the pH of the flotation solution is controlled to be 3-4, and inhibitors are added during the first roughing and second cleaning, and the inhibitors are one or more of carboxymethyl cellulose, acidified water glass, and sodium fluorosilicate.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) The present invention adds acidic chemicals under certain conditions to dissolve calcium, magnesium and other ions on the surface of gangue minerals, reduce the active sites of anion collectors adsorbed on the surface of gangue minerals, and dissolve ions or silicate and carbonate gangue minerals attached to the surface of ilmenite, clean the surface of ilmenite, increase the selective adsorption difference of collectors on the surfaces of ilmenite and gangue minerals, thereby improving the separation effect of ilmenite.

[0029] (2) The dissolution pretreatment flotation method of the present invention can expand the difference in properties between the surface of useful minerals and the surface of gangue minerals, and can achieve selective flotation and efficient separation of ilmenite and gangue minerals, thereby fundamentally solving the technical problem of difficulty in flotation separation of ilmenite and gangue minerals.

[0030] (3) The present invention significantly improves the ilmenite sorting efficiency, significantly improves the grade and recovery rate of ilmenite concentrate, and can significantly reduce the amount of collector used. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 It is a theoretical model diagram of the technical principle of the present invention;

[0033] Figure 2 1 is a flotation flow chart of the slurry in the embodiment. DETAILED DESCRIPTION

[0034] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0035] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0036] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0037] Embodiment 1:

[0038] A flotation method for low-grade refractory ilmenite by dissolution pretreatment, comprising the following steps:

[0039] (1) adding water to the ilmenite weak magnetic separation iron tailings to make the ore mass concentration of 50%, grinding until the grinding fineness is -75μm and the particle size content accounts for 85% of the grinding amount, thereby obtaining a grinding product; subjecting the grinding product to weak magnetic separation, and then subjecting the obtained weak magnetic separation tailings to strong magnetic separation to obtain a strong magnetic coarse concentrate; then adding water to the strong magnetic coarse concentrate to make the ore mass concentration of 50%, and then re-grinding to obtain a re-ground strong magnetic coarse concentrate; transferring the re-ground strong magnetic coarse concentrate to a stirring tank, adding water to slurry to make the ore mass concentration of 35%, and then stirring at a stirring speed of 2.5m / s for 10min to achieve dissolution equilibrium of the ilmenite strong magnetic coarse concentrate in a solution with a natural pH of 6 to 8, and the pH of the slurry solution after dissolution equilibrium is 7.8, thereby obtaining slurry I.

[0040] The TiO2 grade of the above-mentioned reground strong magnetic rough concentrate sample is 17.58%, and the main gangue minerals are pyroxene, serpentine, chlorite and titanite. The results of mineral composition analysis are shown in Table 1. The dissociation degree of ilmenite in the strong magnetic rough concentrate is shown in Table 2, among which the monomer dissociation degree is 59.10%, and the total content of monomer and rich intergrowth is 90.67%.

[0041] Table 1 Content of main minerals in reground strong magnetic rough concentrate / %

[0042]

[0043]

[0044] Table 2 Dissociation degree of ilmenite in regrinding strong magnetic coarse concentrate / %

[0045]

[0046] (2) After the slurry I obtained in step (1) is settled for 5 minutes, the upper layer of clarified slurry water is removed, and new water is added to adjust the slurry so that the mass concentration of the ore is 35%; then 1000 g / t of citric acid is added, and the slurry is stirred at a speed of 1.0 m / s for 2 minutes to make the acid and the slurry evenly mixed. At this time, the pH value of the obtained slurry solution is 3-5, and then stirred at a speed of 2.5 m / s for 10 minutes. After the dissolution is completed, the pH value of the slurry solution is 7.14, and slurry II is obtained.

[0047] (3) After the slurry II obtained in step (2) is settled for 5 minutes, the upper layer of clarified slurry water is removed, and new water is added to adjust the slurry so that the mass concentration of the ore is 35%; then 500 g / t of citric acid is added, and the slurry is stirred at a speed of 1.0 m / s for 2 minutes to make the acid and the slurry uniformly mixed. At this time, the pH value of the obtained slurry solution is 7.00, and then stirred at a speed of 2.5 m / s for 10 minutes. After the dissolution is completed, the pH value of the slurry solution is 7.50, and slurry III is obtained.

[0048] (4) After the slurry III obtained in step (3) is settled for 5 minutes, the upper layer of clarified slurry water is removed, and new water is added to adjust the slurry so that the mass concentration of the ore is 35%. The obtained slurry is introduced into a flotation machine for conventional flotation of ilmenite to obtain ilmenite concentrate.

[0049] The specific flotation process is one roughing, one sweeping and two fine separations. Figure 2 As shown, sulfuric acid is added as a pH adjuster in flotation, the pH of the flotation solution is controlled at 3-4, and an inhibitor is added in the first roughing and second concentrating. The inhibitor is a combination of carboxymethyl cellulose, sodium fluorosilicate, and acidified water glass in a mass ratio of 2.5:5:10. The amount in the roughing is 1500 g / t, and the amount in the concentrating is 500 g / t.

[0050] The TiO2 content of the ilmenite concentrate obtained in this embodiment is 47.26%, and the recovery rate is 75.21%, which is a beneficiation index. Compared with the beneficiation index of the non-dissolution pretreatment process, the TiO2 content of the ilmenite concentrate is 46.37%, and the recovery rate is 60.20%. The recovery rate of this embodiment is increased by 15.01 percentage points, and the TiO2 grade of the concentrate is increased by 0.89 percentage points, as shown in Table 3.

[0051] Table 3 Dissolution pretreatment flotation beneficiation process comparison table

[0052]

[0053]

[0054] Embodiment 2:

[0055] A flotation method for low-grade refractory ilmenite by dissolution pretreatment, comprising the following steps:

[0056] (1) adding water to the ilmenite weak magnetic separation iron tailings to make the ore mass concentration of 50%, grinding until the grinding fineness is -30μm and the content of the particle size accounts for 90% of the grinding amount, thereby obtaining a grinding product; subjecting the grinding product to weak magnetic separation, and then subjecting the obtained weak magnetic separation tailings to strong magnetic separation to obtain a strong magnetic coarse concentrate; then adding water to the strong magnetic coarse concentrate to make the ore mass concentration of 50%, and then re-grinding to obtain a re-ground strong magnetic coarse concentrate; transferring the re-ground strong magnetic coarse concentrate to a stirring tank, adding water to slurry to make the ore mass concentration of 35%, and then stirring at a stirring speed of 2.5m / s for 10min to achieve dissolution equilibrium of the ilmenite re-ground strong magnetic coarse concentrate in a solution with a natural pH of 6 to 8, and the pH of the slurry solution after dissolution equilibrium is 7.5, thereby obtaining slurry I.

[0057] The TiO2 grade of the above-mentioned reground strong magnetic rough concentrate sample is 18.13%, and the main gangue minerals are pyroxene, serpentine, chlorite and titanite. The results of mineral composition analysis are shown in Table 4. The dissociation degree of ilmenite in the reground strong magnetic rough concentrate is shown in Table 5, among which the monomer dissociation degree is 66.73%, and the total content of monomer and rich intergrowth is 91.18%.

[0058] Table 4 Content of main minerals in reground strong magnetic rough concentrate / %

[0059] mineral Ilmenite Titanomagnetite Sphene Titanium pyroxene Titanium amphibole Perovskite Serpentine Chlorite Feldspar content 32.85 9.07 4.30 17.86 6.43 0.35 15.86 10.72 0.06 mineral Zoisite quartz Calcite Garnet Mica apatite Pyrite other Burning content 0.21 0.03 0.19 0.59 0.39 0.07 0.55 0.47 2.50

[0060] Table 5 Dissociation degree of ilmenite in regrinding strong magnetic coarse concentrate / %

[0061]

[0062] (2) After the slurry I obtained in step (1) is settled for 5 minutes, the upper layer of clarified slurry water is removed, and new water is added to adjust the slurry so that the mass concentration of the ore is 35%; then 1000 g / t of citric acid is added, and the slurry is stirred at a speed of 1.0 m / s for 2 minutes to make the acid and the slurry evenly stirred. At this time, the pH value of the obtained slurry solution is 3-5, and then stirred at a speed of 2.5 m / s for 10 minutes. After the dissolution is completed, the pH value of the slurry solution is 7.10, and slurry II is obtained.

[0063] (3) After the slurry II obtained in step (2) is settled for 5 minutes, the upper layer of clarified slurry water is removed, and new water is added to adjust the slurry so that the mass concentration of the ore is 35%; then 500 g / t of citric acid is added, and the slurry is stirred at a speed of 1.0 m / s for 2 minutes to make the acid and the slurry evenly mixed. At this time, the pH value of the obtained slurry solution is 6.90, and then stirred at a speed of 2.5 m / s for 10 minutes. After the dissolution is completed, the pH value of the slurry solution is 7.60, and slurry III is obtained.

[0064] (4) After the slurry III obtained in step (3) is settled for 5 minutes, the upper layer of clarified slurry water is removed, and new water is added to adjust the slurry so that the mass concentration of the ore is 35%. The obtained slurry is introduced into a flotation machine for conventional flotation of ilmenite to obtain ilmenite concentrate.

[0065] The specific flotation process is one roughing, one sweeping and two fine separations. Figure 2 As shown, sulfuric acid is added as a pH adjuster in flotation, the pH of the flotation solution is controlled at 3-4, and an inhibitor is added in the first roughing and second concentrating, the inhibitor is a combination of carboxymethyl cellulose, sodium fluorosilicate, and acidified water glass, the mass ratio is 2.5:5:10, the roughing amount is 1500g / t, and the concentrating amount is 500g / t.

[0066] The present embodiment can obtain the mineral processing index of ilmenite concentrate TiO2 content of 47.57% and recovery rate of 73.32%. Compared with the mineral processing index of the non-dissolution pretreatment process, the ilmenite concentrate TiO2 content is 46.89% and the recovery rate is 61.22%. The recovery rate of the present embodiment is increased by 12.10 percentage points, and the TiO2 grade of the concentrate is increased by 0.68 percentage points, as shown in Table 6.

[0067] Table 6 Dissolution pretreatment flotation beneficiation process comparison table

[0068]

Claims

1. A flotation method for low-grade refractory ilmenite by dissolution pretreatment. It is characterized in that The following steps are involved: (1) adding water to the ilmenite weak magnetic separation iron tailings for grinding to obtain a grinding product, wherein the grinding product has a grinding fineness of -75 μm and a particle size content of 65 to 100% of the total grinding amount; subjecting the grinding product to weak magnetic separation, and then subjecting the obtained weak magnetic separation tailings to strong magnetic separation to obtain a strong magnetic coarse concentrate; then adding water to the strong magnetic coarse concentrate for grinding to obtain a reground strong magnetic coarse concentrate, wherein the ilmenite monomer content in the reground strong magnetic coarse concentrate is above 55%, and the total content of the monomer and the rich intergrowth is greater than 90%; adding water to the reground strong magnetic coarse concentrate for slurrying, stirring, the stirring speed is 1.0 to 3.5 m / s, and the stirring time is 5 to 30 min, so that the strong magnetic coarse concentrate reaches a dissolution equilibrium in a solution with a natural pH of 6 to 8, to obtain slurry I; (2) sedimenting the slurry I, the sedimentation time of slurry I is 3 to 10 minutes; removing the upper slurry water, and then adding water to adjust the slurry so that the mass concentration of the ore is 30 to 40%; then adding acid, the amount of the acid added is 1000 to 3000 g / t, stirring for 1 to 3 minutes to make the acid and slurry evenly stirred, at this time the pH value of the obtained slurry solution is 3 to 5, and continuing to stir for 5 to 10 minutes to obtain slurry II; (3) sedimenting the slurry II, the sedimentation time of slurry II is 3 to 10 minutes; removing the upper slurry water, and then adding water to adjust the slurry so that the mass concentration of the ore is 30 to 40%; then adding acid, the amount of the acid added is 500 to 1500 g / t, stirring for 1 to 3 minutes to make the acid and slurry evenly stirred, at which time the pH value of the obtained slurry solution is 6 to 8, and continuing to stir for 5 to 10 minutes to obtain slurry III; (4) The slurry III is subjected to sedimentation, and the sedimentation time of the slurry III is 3 to 10 minutes; the upper slurry water is removed, and water is added to adjust the slurry so that the mass concentration of the ore is 30 to 40%, and then the obtained slurry is subjected to ilmenite flotation to obtain ilmenite concentrate.

2. The flotation method for low-grade refractory ilmenite by dissolution pretreatment according to claim 1, It is characterized in that In step (2) and step (3), the acid is one or more of sulfuric acid, hydrochloric acid, oxalic acid, citric acid, tartaric acid, malic acid, maleic acid, and lactic acid.

3. The flotation method for low-grade refractory ilmenite by dissolution pretreatment according to any one of claims 1 to 2, It is characterized in that In step (1), water is added to the ilmenite weak magnetic iron tailings to make the ore mass concentration of 50-80%; when regrinding, water is added to the strong magnetic coarse concentrate to make the ore mass concentration of 50%-80%; after the water is added and the slurry is adjusted, the ore mass concentration is 30-40%.

4. The flotation method for low-grade refractory ilmenite by dissolution pretreatment according to any one of claims 1 to 2, It is characterized in that In step (4), the slurry is introduced into a flotation machine for ilmenite flotation, and the flotation includes one roughing selection, one scavenging selection, and two cleaning selections.

5. The flotation method for low-grade refractory ilmenite by dissolution pretreatment according to claim 4, It is characterized in that Sulfuric acid is added as a pH adjuster in the flotation, the pH of the flotation solution is controlled to be 3-4, and inhibitors are added in the first roughing and second cleaning, and the inhibitors are one or more of carboxymethyl cellulose, acidified water glass, and sodium fluorosilicate.

Citation Information

Patent Citations

  • Titaniferous metallurgical residue treatment method

    CN104313338A

  • Weathering type ilmenite beneficiation treatment method

    CN108993766A

  • Flotation method and flotation system for micro-fine-particle ilmenite

    CN113941452A