High-performance PBO paper-based material and preparation method thereof

By using PBO and PBO derivatives as resin systems, combined with wet papermaking and hot pressing technology, the problem of poor compatibility between fiber and resin is solved, and the tensile strength and mechanical properties of PBO paper-based materials are significantly improved, which meets the high Performance materials demand in aerospace and other fields.

CN114790663BActive Publication Date: 2024-11-26INST OF CHEM CHINESE ACAD OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202110104336.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-26
Publication Date
2024-11-26
Estimated Expiration
2041-01-26

AI Technical Summary

Technical Problem

Due to the chemical structure differences between fibers and polymer resins, existing PBO paper-based materials lead to poor interfacial stress transmission, which cannot maximize the mechanical properties. The addition of polymers will reduce dielectric properties, heat resistance and ablation resistance. .

Method used

Using PBO and PBO derivatives as resin systems, high-performance PBO paper-based materials are prepared by wet papermaking and paper sheet molding technology, and aromatic monomers containing diamino and dihydroxyl groups and aromatics containing dicarboxyl or diacyl chloride are used. The group monomers are condensated in solution, formed polyhydroxyamide and cyclized. Combined with hot pressing and heat treatment technology, the compatibility and interface interaction between fibers and resins are improved.

Benefits of technology

It significantly improves the tensile strength and mechanical properties of PBO paper-based materials, meets the application needs in the fields of aerospace, national defense and military, and transportation, while maintaining dielectric, heat and ablation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
Patent Text Reader

Abstract

The present invention discloses a high-performance PBO paper-based material and a preparation method thereof. The method comprises: impregnating PBO base paper in a PBO precursor solution, drying, hot pressing and heat treating to obtain the high-performance PBO paper-based material. The present invention uses PBO and PBO derivatives to enhance PBO paper for the first time. The similarity of chemical structure improves the problem of poor compatibility between traditional resins and PBO fibers, and improves the interface interaction; the similar modulus also improves the stress transfer between interfaces, so that a PBO paper-based material with excellent performance can be prepared, which can meet the application requirements in the fields of aerospace, national defense and military, electrical and transportation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of special paper, and in particular relates to a high-performance PBO paper-based material and a preparation method thereof. Background Art

[0002] At present, with the progress of science and technology, the demand for high-strength, high-modulus, high-temperature resistant and lightweight materials in cutting-edge fields such as defense industry, aerospace, and transportation is increasing. Aramid fiber and PBO fiber are representatives of this type of high-performance materials. Due to the early development of aramid paper, aramid paper-based materials have been widely used in defense, aerospace, transportation, electricity and other fields, with mature production processes. Compared with the rigid straight chain conformation of the molecular chain of para-aramid fiber, the molecular chain of PBO fiber exhibits a rigid straight chain conformation, which gives it more superior mechanical properties. The tensile strength and tensile modulus of PBO fiber reach 5.8GPa and 270GPa respectively, which are about twice that of para-aramid fiber. The thermal decomposition temperature reaches 650℃ and the limiting oxygen index is as high as 68. Therefore, PBO paper may be far superior to the currently widely used aramid paper in terms of mechanical properties, and can also give paper more characteristics, such as: wave transmission performance, heat resistance, ablation resistance, etc. PBO paper, which combines many advantages, will be able to meet the growing performance requirements of paper-based materials in the aerospace, defense, military, and electronics industries.

[0003] Since the surface of PBO fiber is smooth and chemically inert, there is only a weak van der Waals force between the fibers, which makes the mechanical properties of PBO base paper very poor. The high performance of PBO paper can only be achieved by compounding with polymer resin. Patent CN1683712A proposes several ways of enhancement, such as adding polymer resin, mixing hot-melt synthetic fiber, etc. The polymers involved are: polyaramid, polyimide, polyphenylene sulfide, polyether sulfone, polyether ether ketone, polyester, polyacrylonitrile, polybenzimidazole, etc. These polymers are filled into the interior of PBO paper in the form of resin or fiber mixing, which enhances the interaction between the internal interfaces of the paper to a certain extent. However, the difference in the chemical structure of the resin and the PBO fiber will produce a difference in modulus, so that the stress transfer between the interfaces cannot be carried out well, and the mutual infiltration at the interface will also be adversely affected, which ultimately leads to the failure to maximize the mechanical properties of the PBO paper-based material. In addition, the addition of these polymers will also reduce the dielectric properties, heat resistance and ablation resistance of PBO, which will have an adverse effect on the application of PBO paper.

[0004] Based on the above problems, the present invention proposes for the first time to use PBO and PBO derivatives as resin systems for the preparation of high-strength PBO paper-based materials. Summary of the invention

[0005] The purpose of the present invention is to provide a high-performance PBO paper-based material and a preparation method thereof. The present invention utilizes wet papermaking and paper sheet forming technology to prepare a high-performance PBO paper-based material through a two-step process, namely: in the first step, aromatic monomers containing diamino and dihydroxyl groups and aromatic monomers containing dicarboxyl or diacyl chlorides are polycondensed in a solution to prepare polyhydroxyamide (PBO precursor); in the second step, polyhydroxyamide is cyclized at high temperature to prepare PBO and PBO derivatives.

[0006] The method for preparing a high-performance PBO paper-based material provided by the present invention comprises:

[0007] The PBO base paper is immersed in a PBO precursor solution, dried, hot pressed and heat treated to obtain the high-performance PBO paper-based material.

[0008] In the hot pressing step of the above method, the temperature is 100-400°C, specifically 300°C; the pressure is 2-30MPa, specifically 10MPa; the hot pressing step can adopt different hot pressing methods, such as using a hot press or a flat hot press, the hot pressing time is 2-30min, specifically 5min or 15min; if a roller press is used, the number of roller pressing times is 1-6 times, specifically 3 or 4 times;

[0009] In the heat treatment step, the temperature is 200-400° C., specifically 375° C., and the time is 5 min-2 h, specifically 15 min.

[0010] In the PBO precursor solution, the solvent is N,N-dimethylacetamide, N-methylpyrrolidone or N,N-dimethylformamide;

[0011] The concentration is 2 to 20 wt %, specifically 6 wt %;

[0012] In the dipping step, the time is 1 to 60 seconds, specifically 30 seconds;

[0013] In the drying step, the temperature is 40-100°C, specifically 80°C.

[0014] The PBO base paper is prepared according to a method comprising the following steps:

[0015] a. Pulping the PBO chopped fibers in water to obtain PBO pulp;

[0016] b. Dispersing the PBO chopped fibers and the PBO pulp in water in the presence of a dispersant to obtain a suspension, and then forming the suspension on a screen and drying the suspension.

[0017] In the step a, the length of the PBO chopped fibers is 1 to 10 mm, specifically 6 mm; the fineness is 1 to 3 detex, specifically 2.48 detex; the beating concentration is 0.01 to 2 wt%, specifically 1 wt%; the beating time is 20 to 300 min, specifically 90 min;

[0018] In the step b, in the system consisting of the PBO chopped fibers and the PBO pulp, the PBO chopped fibers account for 10 to 60 wt %, specifically 40 wt %;

[0019] The dispersant is a water-soluble polymer, specifically at least one selected from polyethylene glycol and hydroxyethyl cellulose; the concentration of the dispersant in the system is 0.01-0.5wt%, specifically 0.3wt%.

[0020] The PBO precursor is prepared according to a method comprising the following steps:

[0021] The product is prepared by polycondensing an aromatic monomer containing diamino and dihydroxyl groups with an aromatic monomer containing dicarboxylic acid or diacyl chloride in a low temperature solution in the presence of an activating agent.

[0022] The aromatic monomer containing diamino and dihydroxyl groups is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 4,6-diaminoresorcinol hydrochloride, 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone, 4,4'-diamino-3,3'-dihydroxy-biphenyl or 3,3'-diamino-4,4'-dihydroxybiphenyl;

[0023] The aromatic monomer containing dicarboxyl or diacyl chloride is 2,2'-bis(4-chlorophenyl formyl)hexafluoropropane, isophthaloyl chloride, terephthaloyl chloride, 4,4'-biphenyl dicarboxylic acid chloride, 4,4'-oxybisphthaloyl chloride, 4,4'-benzophenone dicarboxylic acid chloride or 4,4'-(4,4'-isopropyldiphenyl diphenyloxy)bis(phthaloyl chloride);

[0024] The solvent used is N,N-dimethylacetamide, N-methylpyrrolidone or N,N-dimethylformamide;

[0025] The concentration of the solution is 5 to 30 wt %, specifically 20 wt %;

[0026] The activation reagents are trimethylchlorosilane and pyridine;

[0027] The amount of the activation reagent used is 4 to 4.8 times the molar amount of the diaminodihydroxy monomer; specifically 4.4 times;

[0028] In the polycondensation reaction step, the temperature is -20 to 30°C; specifically 0°C; the time is 3 to 24 hours; specifically 12 hours.

[0029] In addition, the high-performance PBO paper-based material prepared according to the above method also belongs to the protection scope of the present invention. Specifically, the performance is strength; specifically, tensile strength.

[0030] Compared with the prior art, the present invention has the following advantages:

[0031] The present invention uses PBO and PBO derivatives to enhance PBO paper for the first time. The similarity of chemical structure improves the poor compatibility between traditional resins and PBO fibers and improves the interface interaction; the similar modulus also improves the stress transfer between interfaces, so that PBO paper-based materials with excellent performance can be prepared, which can meet the application needs in the fields of aerospace, national defense, military, electrical and transportation. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram for the preparation of PBO and PBO derivatives. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with specific examples, but the present invention is not limited to the following examples. The methods described are conventional methods unless otherwise specified. The raw materials described can be obtained from public commercial channels unless otherwise specified. The tensile strength of the paper obtained in the following examples is measured according to the test standard of GB / T453-89.

[0034] Example 1

[0035] Preparation of PBO pulp: PBO short-cut fibers with a length of 6 mm and a fineness of 2.48 detex were beaten by a Valley beater for 90 minutes to obtain PBO pulp, and the short-cut fiber concentration was 1 wt%;

[0036] Wet papermaking and paper sheet forming: the prepared PBO pulp and short-cut fibers are dispersed in a hydroxyethyl cellulose solution, the short-cut fiber content is 40%, and the hydroxyethyl cellulose concentration is 0.3wt%. After stirring and mixing, the mixture is placed on a cylinder former for forming, and then dried at 110°C after dehydration;

[0037] Preparation of PBO precursor: Dissolve a certain amount of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane in N,N-dimethylacetamide, cool to 0°C, add 4.4 times the molar amount of trimethylsilyl chloride and pyridine, heat to room temperature and react for 30 minutes, then cool to 0°C, add an equal molar amount of 2,2'-bis(4-formylchlorophenyl)hexafluoropropane, the final solution is 20wt%, and react at room temperature for 12 hours. After washing and drying, the PBO precursor is obtained;

[0038] Impregnation and drying of PBO base paper: The precursor was dissolved in N-methylpyrrolidone to prepare a solution with a concentration of 6wt%, and the PBO base paper was placed in it for 30s, and dried at 80°C after impregnation;

[0039] Hot pressing and heat treatment of PBO paper: PBO paper was placed in a hot press at 300℃, 10MPa, and 5min. After hot pressing, it was placed in a muffle furnace for heat treatment at 375℃ for 15min to obtain PBO paper with a thickness of 0.1mm.

[0040] The prepared PBO paper was subjected to a tensile test, and its tensile strength was 10 kN / m.

[0041] Example 2

[0042] Preparation of PBO pulp: PBO short-cut fibers with a length of 1 mm and a fineness of 1 detex were beaten by a Valley beater for 20 minutes to obtain PBO pulp, and the short-cut fiber concentration was 2 wt%;

[0043] Wet papermaking and paper sheet forming: the prepared PBO pulp and short-cut fibers are dispersed in a hydroxyethyl cellulose solution, the short-cut fiber content is 10%, and the hydroxyethyl cellulose concentration is 0.5wt%, and the mixture is stirred and evenly mixed, and then placed on a cylinder former for forming, and dried at 110°C after dehydration;

[0044] Preparation of PBO precursor: Dissolve a certain amount of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane in N,N-dimethylacetamide, cool to 0°C, add 4 times the molar amount of trimethylsilyl chloride and pyridine, heat to room temperature and react for 30 minutes, then cool to 0°C, add an equal molar amount of 2,2'-bis(4-formylchlorophenyl)hexafluoropropane, the final solution is 5wt%, react at -20°C for 24 hours. After washing and drying, the PBO precursor is obtained;

[0045] Impregnation and drying of PBO base paper: The precursor was dissolved in N-methylpyrrolidone to prepare a solution with a concentration of 20wt%, and the PBO base paper was placed in it for 1s, and dried at 100°C after impregnation;

[0046] Hot pressing and heat treatment of PBO paper: PBO paper was placed in a hot press at 400℃, 30MPa, and 2min. After hot pressing, it was placed in a muffle furnace for heat treatment at 375℃ for 15min to obtain PBO paper with a thickness of 0.1mm.

[0047] The prepared PBO paper was subjected to a tensile test, and its tensile strength was 5 kN / m.

[0048] Example 3

[0049] Preparation of PBO pulp: PBO short-cut fibers with a length of 10 mm and a fineness of 3 detex were beaten by a Valley beater for 300 min to obtain PBO pulp, and the concentration of the short-cut fibers was 0.01 wt%;

[0050] Wet papermaking and paper sheet forming: the prepared PBO pulp and short-cut fibers are dispersed in a hydroxyethyl cellulose solution, the short-cut fiber content is 60%, the hydroxyethyl cellulose concentration is 0.01wt%, and the mixture is stirred and evenly mixed, and then placed on a cylinder former for forming, and dried at 110°C after dehydration;

[0051] Preparation of PBO precursor: Dissolve a certain amount of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane in N,N-dimethylacetamide, cool to 0°C, add 4.8 times the molar amount of trimethylsilyl chloride and pyridine, heat to room temperature and react for 30 minutes, then cool to 0°C, add an equal molar amount of terephthaloyl chloride, the final solution is 30wt%, and react at 0°C for 3 hours. After washing and drying, the PBO precursor is obtained;

[0052] Impregnation and drying of PBO base paper: The precursor was dissolved in N-methylpyrrolidone to prepare a solution with a concentration of 2wt%, and the PBO base paper was placed in it for 60s, and dried at 40°C after impregnation;

[0053] Hot pressing and heat treatment of PBO paper: PBO paper was placed in a hot press at 100°C, 2MPa, and 30 minutes. After hot pressing, it was placed in a muffle furnace for heat treatment at 400°C for 5 minutes to obtain PBO paper with a thickness of 0.1mm.

[0054] The prepared PBO paper was subjected to a tensile test, and its tensile strength was 6 kN / m.

[0055] Example 4

[0056] Preparation of PBO pulp: PBO short-cut fibers with a length of 6 mm and a fineness of 2.48 detex were beaten by a Valley beater for 90 min to obtain PBO pulp, and the short-cut fiber concentration was 1 wt%;

[0057] Wet papermaking and paper sheet forming: the prepared PBO pulp and short-cut fibers are dispersed in a hydroxyethyl cellulose solution, the short-cut fiber content is 40%, and the hydroxyethyl cellulose concentration is 0.3wt%. After stirring and mixing, the mixture is placed on a cylinder former for forming, and then dried at 110°C after dehydration;

[0058] Preparation of PBO precursor: Dissolve a certain amount of 4,6-diaminobenzene hydrochloride in N-methylpyrrolidone, cool to 0°C, add 4.4 times the molar amount of trimethylsilyl chloride and 6.4 times the molar amount of pyridine, heat to room temperature and react for 30 minutes, then cool to 0°C, add an equal molar amount of terephthaloyl chloride, the final solution is 20wt%, and react at 0°C for 12 hours. After washing and drying, the PBO precursor is obtained;

[0059] Impregnation and drying of PBO base paper: The precursor was dissolved in N-methylpyrrolidone to prepare a solution with a concentration of 6wt%, and the PBO base paper was placed in it for 30s, and dried at 80°C after impregnation;

[0060] Hot pressing and heat treatment of PBO paper: PBO paper was placed in a hot press at 100°C, 10 MPa, and 5 min. After hot pressing, it was placed in a muffle furnace for heat treatment at 200°C for 2 h to obtain PBO paper with a thickness of 0.1 mm.

[0061] The prepared PBO paper was subjected to a tensile test, and its tensile strength was 8 kN / m.

[0062] Example 5

[0063] The difference from Example 1 is that a roller press is used to process the reinforced paper, and the number of roller presses is 6, to obtain a PBO paper with a thickness of 0.1 mm and a tensile strength of 9 KN / m.

[0064] Example 6

[0065] The difference from Example 2 is that a roller press is used to process the reinforced paper, and the number of roller presses is 1, to obtain a PBO paper with a thickness of 0.1 mm and a tensile strength of 3 KN / m.

[0066] Example 7

[0067] The difference from Example 3 is that a roller press is used to process the reinforced paper, and the number of roller presses is 3 times, to obtain a PBO paper with a thickness of 0.2 mm and a tensile strength of 7 KN / m.

[0068] Example 8

[0069] The difference from Example 4 is that a roller press is used to process the reinforced paper, and the number of roller presses is 4, to obtain a PBO paper with a thickness of 0.1 mm and a tensile strength of 8 KN / m.

Claims

1. A method for preparing a high-performance PBO paper-based material, comprising: The PBO base paper is immersed in a PBO precursor solution, dried, hot-pressed and heat-treated to obtain the high-performance PBO paper-based material; The PBO precursor is prepared according to a method comprising the following steps: The aromatic monomer containing diamino and dihydroxyl groups and the aromatic monomer containing dicarboxylic acid or diacyl chloride are subjected to low-temperature solution polycondensation in the presence of an activating agent; in the polycondensation step, the temperature is -20 to 30 o C; the activation reagent is trimethylchlorosilane and pyridine; The aromatic monomer containing diamino and dihydroxy groups is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 4,6-diaminoresorcinol hydrochloride, 3,3'-diamino-4,4'-dihydroxydiphenyl sulfone, 4,4'-diamino-3,3'-dihydroxy-biphenyl or 3,3'-diamino-4,4'-dihydroxybiphenyl; The aromatic monomer containing a dicarboxyl group or a diacyl chloride is 2,2'-bis(4-chlorophenyl formyl)hexafluoropropane, isophthaloyl chloride, terephthaloyl chloride, 4,4'-biphenyl dicarboxylic acid chloride, 4,4'-oxybisphthaloyl chloride, 4,4'-benzophenone dicarboxylic acid chloride or 4,4'-(4,4'-isopropyldiphenyldiphenoxy)bis(phthaloyl chloride).

2. The method according to claim 1, wherein: In the hot pressing step, the temperature is 100~400 o C, pressure is 2~30 MPa, time is 2~30 min; number of roller pressing is 1~6 times; In the heat treatment step, the temperature is 200~400 o C, time is 5 min~2 h.

3. The method according to claim 1 or 2, characterized in that: In the PBO precursor solution, the solvent is N,N-dimethylacetamide, N-methylpyrrolidone or N,N-dimethylformamide; Concentration is 2~20wt%; In the dipping step, the time is 1 to 60 seconds; In the drying step, the temperature is 40-100°C.

4. The method according to claim 1 or 2, characterized in that: The PBO base paper is prepared according to a method comprising the following steps: a. Pulping the PBO chopped fibers in water to obtain PBO pulp; b. Dispersing the PBO chopped fibers and the PBO pulp in water in the presence of a dispersant to obtain a suspension, which is then formed on a screen and dried.

5. The method according to claim 4, characterized in that: In step a, the PBO chopped fibers have a length of 1 to 10 mm and a fineness of 1 to 3 detex; the beating concentration is 0.01 to 2 wt%, and the beating time is 20 to 300 min; In the step b, in the system consisting of the PBO chopped fibers and the PBO pulp, the PBO chopped fibers account for 10 to 60 wt %; The dispersant is a water-soluble polymer; the concentration of the dispersant in the system is 0.01-0.5 wt%.

6. The method according to claim 5, characterized in that: The water-soluble polymer is selected from at least one of polyethylene glycol and hydroxyethyl cellulose.

7. The method according to claim 1, wherein: In the preparation method of the PBO precursor, the solvent used is N,N-dimethylacetamide, N-methylpyrrolidone or N,N-dimethylformamide; The concentration of the solution is 5~30 wt%; The amount of the activation reagent is 4 to 4.8 times the molar amount of the diaminodihydroxy monomer; In the polycondensation reaction step, the reaction time is 3 to 24 hours.

8. The high-performance PBO paper-based material prepared by the method according to any one of claims 1 to 7.

9. The high-performance PBO paper-based material according to claim 8, characterized in that: The property in question is tensile strength.

Citation Information

Patent Citations

  • PBO fiber paper base material and its preparing method and use

    CN1683712A

  • Fibrillation dissolving pulp, method for making same and applications

    CN101381898A

  • Polybenzoxazole copolymer with phthalazinone terphenyl structure and preparation method thereof

    CN102219903A

  • Paper material applicable to electrical insulation, and preparation method and application thereof

    CN105986506A

  • Novel process for synthesizing poly-p-phenylene benzobisthiazole

    CN109354684A