A method for preparing high coercivity cerium-rich rare earth permanent magnetic material
Through innovative composition design and preparation process, continuous REFe2 and RE6Fe13Ga phases were formed, weakening the intergranular coupling effect and solving the problem of low coercivity in high-abundance rare-earth permanent magnet materials. This enabled the preparation of high-coercivity cerium-rich rare-earth permanent magnet materials.
Patent Information
- Application Number
- CN202210392116.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-04-14
AI Technical Summary
The existing high-abundance rare earth element cerium has low coercivity in rare earth permanent magnet materials, which cannot meet the requirements of commercial applications. This is mainly because the short-range exchange coupling between adjacent main phase grains has not been effectively weakened.
By increasing the proportion of rare earth elements and alloying elements through composition design, and optimizing the powder preparation, sintering and heat treatment processes, continuous REFe2 phase and RE6Fe13Ga phase are formed, which weakens the short-range exchange coupling between main phase grains. Combined with slow cooling, the distribution of grain boundary phases is optimized.
It significantly improves the coercivity of rare earth permanent magnet materials, meeting the needs of commercial applications.
Smart Images

Figure CN114823113B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of rare earth permanent magnets, and in particular to a method for preparing a high-coercivity cerium-rich rare earth permanent magnet material. Background Art
[0002] NdFeB is currently the rare earth permanent magnet material with the strongest magnetism, the widest application, and the highest rare earth consumption. It is widely used in defense and civilian fields. Under the globalization of low-carbon economy, emerging industries such as wind power generation and new energy vehicles are booming. As a key material, the demand for NdFeB is growing rapidly, and the consumption and price of strategic rare earth elements Nd / Pr have increased significantly. Therefore, in recent years, the application technology of high-abundance rare earth elements in NdFeB has received widespread attention and has become a key development direction in the field of rare earth permanent magnets.
[0003] Among the three rare earth elements with high abundance, lanthanum (La), cerium (Ce), and yttrium (Y), Ce has the highest abundance in the earth's crust, and Ce2Fe 14 Theoretical magnetocrystalline anisotropy field H of tetragonal phase A Also higher than La2Fe 14 B and Y2Fe 14 B, and thus became the focus of research. However, Ce2Fe 14 The intrinsic magnetic properties of the B tetragonal phase are still much lower than those of Nd2Fe 14 B. At present, the magnetic properties of cerium-rich magnets with high Ce substitution are generally low, especially the coercivity, which is far lower than the theoretical H A , which cannot meet the requirements of commercial applications. If we can invent high coercivity Ce-rich rare earth permanent magnet materials through innovations in component design and preparation technology, it will be possible to achieve large-scale application of high-abundance rare earth Ce in rare earth permanent magnets and promote the efficient and balanced utilization of rare earth elements.
[0004] Based on the existing research results of NdFeB, the coercive force of NdFeB magnets is much lower than the theoretical value, which is largely attributed to the ferromagnetic grain boundary phase of the magnet. The iron content in the grain boundary phase is too high, even reaching more than 60%, and there is still a short-range exchange coupling between adjacent ferromagnetic main phase grains. In traditional NdFeB magnets, the main phase is Nd-rich grain boundary phase; while in Ce-rich magnets, in addition to some rare earth-rich grain boundary phases, there are also a large number of REFe2 grain boundary phases, and they mainly exist in the form of triple grain boundaries, and the magnetic isolation effect on the main phase grains is still relatively small. How to effectively play the role of grain boundary phases such as REFe2 is a key issue in the preparation of high coercive force Ce-rich rare earth permanent magnet materials. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for preparing a high coercive force cerium-rich rare earth permanent magnet material.
[0006] A method for preparing a high coercivity cerium-rich rare earth permanent magnetic material comprises the following steps:
[0007] (1) The preparation composition is (A 1-a Ce a ) b Fe bal M c B d Ga e Magnetic powder, wherein A is one or more of the rare earth elements Nd, Pr, Dy, Tb, La, Y, and Gd, Ce is the rare earth element cerium, Fe is the iron element, M is one or more of the alloy elements Co, Ni, Al, Cu, Mn, Nb, Zr, Ti, V, and Ta, B is the boron element, and Ga is the gallium element, and in terms of mass percentage, 0.3≤a≤0.7, 30≤b≤35, 0≤c≤2, 0.75≤d≤0.95, and 0.2≤e≤3;
[0008] (2) preparing the obtained magnetic powder into a magnet by sintering or hot pressing and hot deformation process;
[0009] (3) The prepared magnet is subjected to heat treatment to obtain a high coercive force cerium-rich rare earth permanent magnet material.
[0010] The preparation process of magnetic powder in step (1) includes:
[0011] (1) Belt spinning, hydrogen crushing and air flow grinding;
[0012] (2) Rapid quenching zone and hydrogen fracture;
[0013] (3) The sequence is hydrogen absorption, disproportionation, dehydrogenation and recombination.
[0014] The magnetic powder in step (1) is obtained directly through a single-main-phase method or through a multi-main-phase method to obtain a final defined composition.
[0015] The sintering process in step (2) includes: a conventional sintering process, a spark plasma sintering process or a microwave sintering process.
[0016] The heat treatment process in step (3) includes: one-step heat treatment or two-step heat treatment or slow cooling after sintering or hot pressing and hot deformation in step (2).
[0017] Specifically, the heat treatment temperature of the one-step heat treatment is 400-800° C., and the heat treatment time is 0.5 h-5 h.
[0018] Specifically, the first step of the two-step heat treatment has a heat treatment temperature of 850-950° C. and a heat treatment time of 0.5 h to 4 h; the second step of the heat treatment has a heat treatment temperature of 400-600° C. and a heat treatment time of 0.5 h to 5 h.
[0019] Specifically, the cooling rate after sintering or hot pressing and thermal deformation is less than or equal to the furnace cooling rate at room temperature.
[0020] The beneficial effects of the present invention compared with the prior art are as follows:
[0021] 1) Based on a large number of experimental studies, the present invention has mastered the organizational structure characteristics of cerium-rich rare earth permanent magnet materials. For magnets with different Ce contents, the content of alloying element Ga in the magnets is increased to varying degrees through targeted component design, supplemented by optimizing the ratio of alloying elements such as Cu and Al, while reducing the content of element B, promoting the formation of a large number of REFe2 phases. More importantly, the REFe2 phase is promoted to extend into the interface region of the adjacent main phase grains to form a continuous REFe2 grain boundary phase, and at the same time forming part of the RE6Fe 13 Ga phase, these Fe-rich non-ferromagnetic grain boundary phases will consume a large amount of iron in the rare earth-rich grain boundary phase, reduce the magnetism of the rare earth-rich grain boundary phase, thereby weakening or even eliminating the short-range exchange coupling between the main phase grains, and greatly improving the coercive force of the magnet.
[0022] 2) The composition design of the present invention increases the content of rare earth elements at the same time, and matches the ratio of different rare earth elements and alloy elements. On the one hand, it is more conducive to forming a good organizational structure during the preparation of magnetic powder, and promotes the formation of a large number of continuous REFe2 phases and part of RE6Fe during sintering and heat treatment. 13 Ga grain boundary phase, on the other hand, increases the rare earth element content in the rare earth-rich grain boundary phase, relatively reduces the Fe element content therein, and further improves the coercivity.
[0023] 3) While designing targeted ingredients, the present invention cooperates with preparation technology innovation and innovatively combines different powder making, sintering and heat treatment technologies, including the innovatively proposed cooling at a slower speed after sintering or hot pressing and hot deformation, where the cooling speed is less than or equal to the furnace cooling speed at room temperature, etc., which can further optimize the formation and distribution of grain boundary phases, thereby improving the coercive force, and ultimately obtaining a high coercive force cerium-rich rare earth permanent magnet material. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 1 is a comparison of backscattering images, wherein (a) the Ce-rich magnet of Comparative Example 1; (b) the Ce-rich magnet of Example 1; DETAILED DESCRIPTION
[0025] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments:
[0026] Embodiment 1:
[0027] (1) Two magnetic powders with different compositions were prepared. In terms of mass percentage, the composition of magnetic powder 1 was [(Pr 0.2 Nd0.8 ) 0.5 Ce 0.5 ] 32 Fe bal Zr 0.15 Cu 0.12 Al 0.2 Co 0.6 B 0.9 Ga 0.5 , the composition of magnetic powder 2 is (Pr 0.2 Nd 0.8 ) 32 Fe bal Zr 0.15 Cu 0.12 Al 0. 2Co 0.6 B 0.9 Ga 0.5 , and the preparation processes are belt spinning, hydrogen breaking and air flow milling in sequence;
[0028] (2) the obtained magnetic powder 1 and magnetic powder 2 were uniformly mixed in a mass ratio of 4:1, and a magnet was prepared by a common sintering process at a sintering temperature of 1040°C and a sintering time of 4 hours;
[0029] (3) The prepared magnet is subjected to a one-step heat treatment to obtain a high coercive force cerium-rich rare earth permanent magnet material, the one-step heat treatment temperature is 650°C, and the one-step heat treatment time is 2 hours.
[0030] The test results of AMT-4 permanent magnet property measuring instrument show that the coercive force of sintered magnet is 12.0kOe, and the coercive force of heat-treated magnet is 13.2kOe.
[0031] Comparative Example 1:
[0032] The difference from Example 1 is that the composition of the magnetic powder in step (1) is different, the content of rare earth elements is reduced, the content of B element is increased, and the content of Ga element is reduced. In terms of mass percentage, the composition of magnetic powder 1 is [(Pr 0.2 Nd 0.8 ) 0.5 Ce 0.5 ] 31 Fe bal Zr 0.15 Cu 0.12 Al 0.2 Co 0.6 B1 0.1 , the composition of magnetic powder 2 is (Pr 0.2 Nd 0.8 ) 31 Fe bal Zr 0.15 Cu 0.12 Al 0.2 Co0.6 B1 0.1 The test results of AMT-4 permanent magnet property measuring instrument show that the coercive force of the sintered magnet is 8.9 kOe, and the coercive force of the heat-treated magnet is 10.1 kOe, which are much smaller than those of Example 1.
[0033] Comparison of Ce-rich magnet structure morphology between Example 1 and Comparative Example 1 Figure 1 As shown, the magnet designed by the present invention forms a large amount of continuous REFe2 phase and part of RE6Fe 13 Ga phase, thereby weakening or even eliminating the short-range exchange coupling between the main phase grains and improving the coercive force of the magnet.
[0034] Embodiment 2:
[0035] (1) Prepare magnetic powder, the composition of which is [(Pr 0.3 Nd 0.7 ) 0.45 Ce 0.55 ] 32.2 Fe bal Nb 0.2 Cu 0.2 Al 0.3 Co 0.8 B 0.85 Ga1, whose preparation process is belt spinning, hydrogen breaking and jet milling;
[0036] (2) preparing the obtained magnetic powder into a magnet through a common sintering process, the sintering temperature is 1030° C., and the sintering time is 4.5 h;
[0037] (3) The prepared magnet is subjected to a one-step heat treatment to obtain a high coercive force cerium-rich rare earth permanent magnet material. The heat treatment temperature is 630°C and the heat treatment time is 2 hours.
[0038] The test results of AMT-4 permanent magnet property measuring instrument show that the coercive force of sintered magnet is 10.6kOe, and the coercive force of heat-treated magnet is 12.0kOe.
[0039] Comparative Example 2:
[0040] The difference from Example 2 is that: the composition of the magnetic powder in step (1) is different, the content of rare earth elements is reduced, the content of B element is increased, and Ga element is not included. In terms of mass percentage, the composition of the magnetic powder is [(Pr 0.3 Nd 0.7 ) 0.45 Ce 0.55 ] 31.6 Fe bal Nb 0.2 Cu 0.2 Al 0.3 Co 0.8B1. The test results of AMT-4 permanent magnet property measuring instrument show that the coercive force of the sintered magnet is 6.8 kOe, and the coercive force of the heat-treated magnet is 7.5 kOe, which are much smaller than those of Example 2.
[0041] Embodiment 3:
[0042] (1) Prepare magnetic powder. The composition of the magnetic powder is (Nd 0.4 Ce 0.6 ) 32.5 Fe bal Zr 0.25 Cu 0.25 Co 0. 9B 0.85 Ga 0.65 , and its preparation process is hydrogen absorption, disproportionation, dehydrogenation and recombination;
[0043] (2) preparing the obtained magnetic powder into a magnet by hot pressing and hot deformation process, with the hot pressing temperature being 660°C, the pressure being 380 MPa, and the heat deformation temperature being 800°C;
[0044] (3) The prepared magnet is free from heat treatment, and a high coercive force cerium-rich rare earth permanent magnet material is obtained.
[0045] The test results of AMT-4 permanent magnet property measuring instrument show that the coercive force of the magnet is 9.8kOe.
[0046] Comparative Example 3:
[0047] The difference from Example 3 is that: the composition of the magnetic powder in step (1) is different, the content of rare earth elements is reduced, the content of B element is increased, and Ga element is not included. In terms of mass percentage, the composition of the magnetic powder is (Nd 0.4 Ce 0.6 ) 31 Fe bal Zr 0.25 Cu 0.25 Co 0.9 B1. The test results of AMT-4 permanent magnet property measuring instrument show that the coercive force of the magnet is 5.8 kOe, which is much smaller than that of Example 3.
[0048] Embodiment 4:
[0049] (1) Two magnetic powders with different compositions were prepared. In terms of mass percentage, the composition of magnetic powder 1 was [(Pr 0.1 Nd 0.9 ) 0.5 La 0.2 Ce 0.3 ] 31.5 Fe bal Zr 0.15 Al 0.25 Cu 0.25Ti 0.1 B 0.9 Ga 0.8 , the composition of magnetic powder 2 is (Pr 0.1 Nd 0.9 ) 31.5 Fe bal Zr 0.15 Al 0.25 Cu 0.25 Ti 0.1 B 0.9 Ga 0.8 , and the preparation processes are belt spinning, hydrogen breaking and air flow milling in sequence;
[0050] (2) the obtained magnetic powder 1 and magnetic powder 2 were uniformly mixed in a mass ratio of 3:2, and a magnet was prepared by a common sintering process at a sintering temperature of 1040°C and a sintering time of 3 h;
[0051] (3) The prepared magnet is subjected to a one-step heat treatment to obtain a high coercive force cerium-rich rare earth permanent magnet material. The heat treatment temperature is 480°C and the heat treatment time is 4 hours.
[0052] The test results of AMT-4 permanent magnet property measuring instrument show that the coercive force of sintered magnet is 9.5kOe, and the coercive force of heat-treated magnet is 15.7kOe.
[0053] Comparative Example 4:
[0054] The difference from Example 4 is that: the composition of the magnetic powder in step (1) is different, the content of rare earth elements is reduced, the content of B element is increased, and the content of Ga element is reduced. In terms of mass percentage, the composition of magnetic powder 1 is [(Pr 0.1 Nd 0.9 ) 0.5 La 0.2 Ce 0.3 ] 30.5 Fe bal Zr 0.15 Al 0.25 Cu 0.25 Ti 0.1 B1 0.15 , the composition of magnetic powder 2 is (Pr 0.1 Nd 0.9 ) 30.5 Fe bal Zr 0.15 Al 0.25 Cu 0.25 Ti 0.1 B1 0.15 The test results of AMT-4 permanent magnet property measuring instrument show that the coercive force of the sintered magnet is 7.5 kOe, and the coercive force of the heat-treated magnet is 9.6 kOe, which are much smaller than those of Example 4.
Claims
1. A method for preparing a high coercive force cerium-rich rare earth permanent magnetic material, characterized in that: The following steps are involved: (1) The preparation composition is (A 1-a Ce a ) b Fe bal M c B d Ga e Magnetic powder, wherein A is one or more of the rare earth elements Nd, Pr, Dy, Tb, La, Y, and Gd, Ce is the rare earth element cerium, Fe is the iron element, M is one or more of the alloy elements Co, Ni, Al, Cu, Mn, Nb, Zr, Ti, V, and Ta, B is the boron element, and Ga is the gallium element, and in terms of mass percentage, 0.3≤a≤0.7, 31.5≤b≤35, 0.75≤c≤2, 0.75≤d≤0.95, and 0.2≤e≤3; (2) preparing the obtained magnetic powder into a magnet by sintering or hot pressing and hot deformation process, wherein the sintering process includes: ordinary sintering process, spark plasma sintering process or microwave sintering process; (3) subjecting the prepared magnet to heat treatment to obtain a high coercive force cerium-rich rare earth permanent magnet material, the heat treatment process comprising: 1) one-step heat treatment; or 2) two-step heat treatment; or 3) slow cooling after sintering or hot pressing and heat deformation in step (2), wherein the cooling rate after sintering or hot pressing and heat deformation is less than or equal to the furnace cooling rate at room temperature.
2. The preparation method according to claim 1, characterized in that: The preparation process of the magnetic powder in step (1) includes: 1) belt spinning, hydrogen pulverization and air flow milling in sequence; or 2) belt quenching and hydrogen pulverization in sequence; or 3) hydrogen absorption, disproportionation, dehydrogenation and recombination in sequence.
3. The preparation method according to claim 1, characterized in that: The magnetic powder in step (1) is obtained directly through a single-main-phase method or through a multi-main-phase method to obtain a final defined composition.
4. The preparation method according to claim 1, characterized in that: The heat treatment temperature of the heat treatment in step (3) is 400-800° C., and the heat treatment time is 0.5 h-5 h.
5. The preparation method according to claim 1, characterized in that: In step (3), the first step of the two-step heat treatment has a heat treatment temperature of 850-950°C and a heat treatment time of 0.5h-4h; the second step of the heat treatment has a heat treatment temperature of 400-600°C and a heat treatment time of 0.5h-5h.