Preparation and application of natural polymer nanocomposite sponge for radionuclide enrichment and separation

By using the directional network channels and Janus layer structure of konjac glucomannan and Ti3C2Tx MXene composite sponge in a solar-driven interface evaporator, the problem of reduced purification effect caused by salt accumulation is solved, and efficient and stable water evaporation and radioactive elements are achieved The purification improves the purification effect and the self-floating ability of the equipment.

CN114842999BActive Publication Date: 2024-10-15SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210208951.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-03
Publication Date
2024-10-15
Estimated Expiration
2042-03-03

AI Technical Summary

Technical Problem

In the existing technology, the purification effect of solar-driven interface evaporators is reduced due to salt accumulation during long-term operation, and there is a lack of efficient and low-energy consumption radioactive wastewater purification methods.

Method used

An efficient solar-driven interface evaporator based on konjac glucomannan (KGM) and Ti3C2Tx MXene composite sponge is used to achieve efficient and stable water evaporation and salt ion absorption and diffusion balance through directional network channels and Janus layer structure to avoid salt blockage and Improve the self-floating ability of the evaporator.

Benefits of technology

It achieves high conversion efficiency and stable water evaporation rate, reduces radioactive element concentration by 6 orders of magnitude, reduces blocking of sunlight absorption, reduces heat dissipation, avoids additional equipment investment, and improves purification effect and operability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114842999B_ABST
    Figure CN114842999B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation and application of a natural polymer nano composite sponge for radionuclide enrichment and separation, comprising: preparing Ti3C2T by using Ti3AlC2 x MXene powder; by Ti3C2T x MXene powder to obtain Ti3C2T x Suspension; KGM is added to Ti3C2T x The suspension was stirred to obtain KGM‑Ti3C2T x Hydrogel; KGM‑Ti3C2T x The hydrogel was poured into a mold and placed in liquid nitrogen for directional freezing. The vacuum-dried sample was immersed in a NaOH ethanol solution and heated. The sample was washed and freeze-dried again to obtain KGM‑Ti3C2T x The sponge is coated with a PDMS solution on the top layer, and then vacuum dried to obtain a natural polymer nanocomposite sponge for radionuclide enrichment and separation. The composite sponge prepared by the present invention is a high-efficiency solar-driven interface evaporator for radioactive wastewater purification; the composite sponge has high conversion efficiency and stable water evaporation rate under simulated sunlight irradiation; the concentration of radioactive elements in the simulated radioactive wastewater is reduced by 6 orders of magnitude after J-KTS purification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of radioactive wastewater treatment, and in particular to a preparation method and application of a natural polymer nano composite sponge for radionuclide enrichment and separation. Background Art

[0002] With the widespread application of nuclear science and technology, a large amount of radioactive wastewater will inevitably be generated. In order to protect the ecological environment and human health, the purification of radioactive wastewater is extremely urgent. At present, a variety of technologies have been developed for the purification of radioactive wastewater, such as biological methods, chemical precipitation methods, photocatalytic methods and adsorption methods. However, due to the diversity of radioactive wastewater, there is currently no feasible method with low energy consumption and high efficiency. As an effective method to obtain solar energy and effectively separate soluble pollutants in water, solar-driven interfacial evaporation is a promising method for purifying radioactive wastewater. Therefore, there is an urgent need to develop an efficient solar-driven interfacial evaporator for purifying radioactive wastewater.

[0003] In the solar-driven interfacial evaporation process, the evaporator collects solar radiation energy, converts it into heat energy, and evaporates radioactive wastewater for purification. At the same time, the radioactive elements are adsorbed on the solar absorber to achieve the enrichment and deposition of radioactive elements. However, the salt accumulated on the surface of the evaporator will block the steam escape channel, reduce the absorption of sunlight in long-term operation, and lead to reduced purification effect. One way to solve the desalination problem is to construct a hydrophobic Janus layer on the top of the hydrophilic evaporator. As a result, the salt ions are retained in the bottom hydrophilic layer to prevent the salt from blocking the water transfer channel and reducing the absorption of sunlight. In addition, the hydrophobic upper layer gives the evaporator the ability to self-float on the water surface, avoiding the investment of additional equipment and improving operability.

[0004] Herein, we successfully designed a highly efficient solar-driven interfacial evaporator for radioactive wastewater purification based on konjac glucomannan (KGM) and Ti3C2T3 with oriented network channels and Janus layers. x MXene composite sponge (J-KTS). J-KTS has some functions to ensure efficient and stable solar water evaporation. First, as a component of J-KTS, Ti3C2T x MXene has strong light absorption and excellent photothermal conversion performance, which ensures continuous heat energy for evaporation. Secondly, as another component of J-KTS, KGM provides J-KTS with skeleton, hydrophilicity and thermal insulation. Thirdly, the directional network channels inside J-KTS are able to quickly transport water from bulk water to the evaporation interface through capillary effect, ensuring sufficient water supply for evaporation. Last but not least, the unique salt resistance of J-KTS is due to the Janus layer, which establishes a balance between salt ion absorption and diffusion. Summary of the invention

[0005] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0006] In order to achieve these purposes and other advantages according to the present invention, a method for preparing a natural polymer nanocomposite sponge for radionuclide enrichment and separation is provided, comprising the following steps:

[0007] Step 1: Add Ti3AlC2 powder into hydrofluoric acid solution, heat to react, centrifuge, wash, and then vacuum dry to obtain Ti3C2T x MXene powder;

[0008] Step 2: Ultrasonication of Ti3C2T x MXene powder was evenly dispersed in water to obtain Ti3C2T x Then, KGM was added to Ti3C2T x The suspension was stirred to obtain KGM-Ti3C2T x Hydrogel;

[0009] Step 3: KGM-Ti3C2T x The hydrogel was poured into a mold, the bottom of which was fixed on a steel plate, which was placed in liquid nitrogen for directional freezing and then vacuum dried; the vacuum dried sample was immersed in a NaOH ethanol solution, heated, and kept warm; then, the sample was washed and freeze-dried again to obtain KGM-Ti3C2T x sponge;

[0010] Step 4: On KGM-Ti3C2T x The top layer of the sponge was coated with PDMS solution and then vacuum dried to obtain KGM-Ti3C2T3 with oriented network channels and Janus layer for radioactive wastewater treatment. x Composite sponge.

[0011] Preferably, in the step 1, the concentration of the hydrofluoric acid solution is 5-15wt%; and the mass volume ratio of the Ti3AlC2 powder to the hydrofluoric acid solution is 1g:10mL.

[0012] Preferably, in step 1, the heating reaction temperature is 85-95° C. and the time is 0.5-1.5 h; deionized water is used for washing until the pH value is 6, and the vacuum drying time is 24 h.

[0013] Preferably, in step 2, Ti3C2T x The mass volume ratio of MXene powder to water is 0.5 g:100 mL; the Ti3C2T xThe mass ratio of MXene powder to KGM is 1:2-5; the stirring time is 10-15h.

[0014] Preferably, in the step 2, dual-frequency ultrasound is applied alternately during the stirring process; the frequencies of the dual-frequency ultrasound are 35-55kHz and 100-135kHz, the time for the dual-frequency ultrasound alternating treatment is 25-30s, and the power of the dual-frequency ultrasound is 400-500W.

[0015] Preferably, in step 3, the concentration of the NaOH ethanol solution is 2-5 wt %; the heating temperature is 40-50° C., and the insulation time is 4-8 h.

[0016] Preferably, in the step 3, the vacuum dried sample is immersed in a NaOH ethanol solution, and then added to a microwave-ultrasonic integrated reactor, and microwave and ultrasonic waves are turned on at the same time, and the synergistic treatment is carried out at a treatment temperature of 40 to 50 ° C for 2 to 3 hours; then, the sample is washed and freeze-dried again to obtain KGM-Ti3C2T x Sponge; the microwave power of the coordinated treatment is 300-500W, the ultrasonic power is 300-500W, and the ultrasonic frequency is 40-55KHz.

[0017] Preferably, in step 4, the concentration of the PDMS solution is 0.5-1.5 wt %.

[0018] The present invention provides an application of a natural polymer nanocomposite sponge prepared by the preparation method described above in treating radioactive wastewater. The natural polymer nanocomposite sponge is added into the radioactive wastewater and irradiated with light to achieve evaporation and purification of the radioactive wastewater.

[0019] The present invention includes at least the following beneficial effects: the J-KTS prepared by the present invention is a high-efficiency solar-driven interfacial evaporator for radioactive wastewater purification; the J-KTS has high conversion efficiency and a stable water evaporation rate under simulated sunlight. In addition, the concentrations of radioactive elements (Sr, Cs and U) in the simulated radioactive wastewater were reduced by 6 orders of magnitude after purification by J-KTS. Due to the Janus layer of J-KTS, salt ions are retained in the bottom hydrophilic layer, preventing salt from blocking the water transport channel and reducing the absorption of sunlight. The hydrophobic upper layer gives J-KTS the ability to float on the water surface, reducing heat dissipation and avoiding investment in additional equipment.

[0020] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 ac show scanning electron microscopy (SEM) images of J-KTS at different magnifications;

[0022] Figure 2 X-ray (EDX) elemental mapping of J-KTS is shown;

[0023] Figure 3 X-ray diffraction (XRD) of different materials is shown;

[0024] Figure 4 Fourier transform infrared (FTIR) spectra of different materials are shown;

[0025] Figure 5 The ultraviolet and visible (UV-vis) spectra of different materials are shown;

[0026] Figure 6 J-KTS and Ti3C2T are shown x Ultraviolet and visible (UV-vis) spectra;

[0027] Figure 7 The water contact angle image of J-KTS is shown;

[0028] Figure 8 The surface temperature variation diagram of J-KTS is shown;

[0029] Fig. 9 The heating curves of different samples are shown;

[0030] Fig.10 The water evaporation rate curves of different samples are shown;

[0031] Fig.11 The water evaporation rate curves of different samples (J-KTS, J-KTS-1, and J-KTS-3) are shown;

[0032] Fig.12 The water evaporation rate curves of different samples (J-KTS, J-KTS-2, and J-KTS-3) are shown;

[0033] Fig.13 A graph showing the light-to-heat conversion efficiency of different samples is shown;

[0034] Fig.14 The changes in Na, K, Ca, and Mg concentrations in seawater before and after J-KTS purification are shown;

[0035] Fig.15 The image of J-KTS evaporation anti-salt scaling in 100 minutes is shown;

[0036] Fig.16The changes of Sr, Cs and U concentrations in radioactive wastewater before and after J-KTS purification are shown;

[0037] Fig.17 The changes of Sr, Cs and U concentrations in radioactive wastewater after purification of different samples (J-KTS, J-KTS-1, J-KTS-3) are shown (the concentrations before purification are as follows Fig.16 shown);

[0038] Fig.18 The changes of Sr, Cs and U concentrations in radioactive wastewater after purification of different samples (J-KTS, J-KTS-2, J-KTS-3) are shown (the concentrations before purification are as follows Fig.16 shown);

[0039] Fig.19 The SEM image and corresponding EDX elemental mapping of J-KTS after solar-driven radioactive wastewater decontamination are shown;

[0040] Fig. 20 The concentration changes of Sr, Cs and U in radioactive wastewater with different pH values ​​before and after J-KTS purification are shown;

[0041] Fig.21 The evaporation efficiency of J-KTS at different pH is shown;

[0042] Fig. 22 The concentrations and changes of Na, K, Mg, Ca, Sr, Cs, and U after J-KTS purification are shown.

[0043] Fig.23 The evaporation rate of J-KTS during 10 cycles is shown. DETAILED DESCRIPTION

[0044] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0045] It should be understood that terms such as “having”, “including” and “comprising” used herein do not specify the existence or addition of one or more other elements or combinations thereof.

[0046] Embodiment 1:

[0047] A method for preparing a natural polymer nanocomposite sponge for radionuclide enrichment and separation comprises the following steps:

[0048] Step 1: Add 1 g of Ti3AlC2 powder to 10 mL of hydrofluoric acid solution (10 wt%), heat to 90 °C for reaction, centrifuge, wash with deionized water until pH = 6, and then vacuum dry for 24 h to obtain Ti3C2T xMXene powder (Ti3C2T x );

[0049] Step 2: 0.5 g Ti3C2T x MXene powder was evenly dispersed in 100 mL of deionized water to obtain Ti3C2T x Then, 1.5 g KGM was added to Ti3C2T x The suspension was stirred for 12 h to obtain KGM-Ti3C2T x Hydrogel;

[0050] Step 3: KGM-Ti3C2T x The hydrogel was poured into a mold, the bottom of which was fixed on a steel plate, which was placed in liquid nitrogen for directional freezing and then vacuum dried. The vacuum dried sample was immersed in 100 mL of NaOH ethanol solution (3 wt%), heated to 45 ° C, and kept warm for 6 h. Subsequently, the sample was washed and freeze-dried again to obtain KGM-Ti3C2T x Sponge (KTS);

[0051] Step 4: On KGM-Ti3C2T x The top layer of the sponge was coated with PDMS solution (1 wt%) and then vacuum dried to obtain KGM-Ti3C2T3 with oriented network channels and Janus layer for radioactive wastewater treatment. x Composite sponge (J-KTS).

[0052] Embodiment 2:

[0053] A method for preparing a natural polymer nanocomposite sponge for radionuclide enrichment and separation comprises the following steps:

[0054] Step 1: Add 1 g of Ti3AlC2 powder to 10 mL of hydrofluoric acid solution (10 wt%), heat to 90 °C for reaction, centrifuge, wash with deionized water until pH = 6, and then vacuum dry for 24 h to obtain Ti3C2T x MXene powder;

[0055] Step 2: 0.5 g Ti3C2T x MXene powder was evenly dispersed in 100 mL of deionized water to obtain Ti3C2T x Then, 1.5 g KGM was added to Ti3C2T x The suspension was stirred for 12 h to obtain KGM-Ti3C2T xhydrogel; applying alternating dual-frequency ultrasound during stirring; the frequencies of the dual-frequency ultrasound are 35kHz and 135kHz, the dual-frequency ultrasound alternating treatment time is 30s, and the power of the dual-frequency ultrasound is 500W;

[0056] Step 3: KGM-Ti3C2T x The hydrogel was poured into a mold, the bottom of which was fixed on a steel plate, which was placed in liquid nitrogen for directional freezing and then vacuum dried. The vacuum dried sample was immersed in 100 mL of NaOH ethanol solution (3 wt%), heated to 45 ° C, and kept warm for 6 h. Subsequently, the sample was washed and freeze-dried again to obtain KGM-Ti3C2T x sponge;

[0057] Step 4: On KGM-Ti3C2T x The top layer of the sponge was coated with PDMS solution (1 wt%) and then vacuum dried to obtain KGM-Ti3C2T3 with oriented network channels and Janus layer for radioactive wastewater treatment. x Composite sponge (J-KTS-1).

[0058] Embodiment 3:

[0059] A method for preparing a natural polymer nanocomposite sponge for radionuclide enrichment and separation comprises the following steps:

[0060] Step 1: Add 1 g of Ti3AlC2 powder to 10 mL of hydrofluoric acid solution (10 wt%), heat to 90 °C for reaction, centrifuge, wash with deionized water until pH = 6, and then vacuum dry for 24 h to obtain Ti3C2T x MXene powder;

[0061] Step 2: 0.5 g Ti3C2T x MXene powder was evenly dispersed in 100 mL of deionized water to obtain Ti3C2T x Then, 1.5 g KGM was added to Ti3C2T x The suspension was stirred for 12 h to obtain KGM-Ti3C2T x Hydrogel;

[0062] Step 3: KGM-Ti3C2T xThe hydrogel was poured into a mold, the bottom of which was fixed on a steel plate, which was placed in liquid nitrogen for directional freezing and then vacuum dried. The vacuum dried sample was immersed in 100 mL of NaOH ethanol solution (3 wt%) and then added to a microwave-ultrasonic integrated reactor. The microwave and ultrasound were turned on at the same time and the synergistic treatment was performed at a treatment temperature of 45 ° C for 2 h. Subsequently, the sample was washed and freeze-dried again to obtain KGM-Ti3C2T x sponge; the microwave power of the coordinated treatment is 500W, the ultrasonic power is 500W, and the ultrasonic frequency is 45KHz;

[0063] Step 4: On KGM-Ti3C2T x The top layer of the sponge was coated with PDMS solution (1 wt%) and then vacuum dried to obtain KGM-Ti3C2T3 with oriented network channels and Janus layer for radioactive wastewater treatment. x Composite sponge (J-KTS-2).

[0064] Embodiment 4:

[0065] A method for preparing a natural polymer nanocomposite sponge for radionuclide enrichment and separation comprises the following steps:

[0066] Step 1: Add 1 g of Ti3AlC2 powder to 10 mL of hydrofluoric acid solution (10 wt%), heat to 90 °C for reaction, centrifuge, wash with deionized water until pH = 6, and then vacuum dry for 24 h to obtain Ti3C2T x MXene powder;

[0067] Step 2: 0.5 g Ti3C2T x MXene powder was evenly dispersed in 100 mL of deionized water to obtain Ti3C2T x Then, 1.5 g KGM was added to Ti3C2T x The suspension was stirred for 12 h to obtain KGM-Ti3C2T x hydrogel; applying alternating dual-frequency ultrasound during stirring; the frequencies of the dual-frequency ultrasound are 35kHz and 135kHz, the dual-frequency ultrasound alternating treatment time is 30s, and the power of the dual-frequency ultrasound is 500W;

[0068] Step 3: KGM-Ti3C2T xThe hydrogel was poured into a mold, the bottom of which was fixed on a steel plate, which was placed in liquid nitrogen for directional freezing and then vacuum dried. The vacuum dried sample was immersed in 100 mL of NaOH ethanol solution (3 wt%) and then added to a microwave-ultrasonic integrated reactor. The microwave and ultrasound were turned on at the same time and the synergistic treatment was performed at a treatment temperature of 45 ° C for 2 h. Subsequently, the sample was washed and freeze-dried again to obtain KGM-Ti3C2T x sponge; the microwave power of the coordinated treatment is 500W, the ultrasonic power is 500W, and the ultrasonic frequency is 45KHz;

[0069] Step 4: On KGM-Ti3C2T x The top layer of the sponge was coated with PDMS solution (1 wt%) and then vacuum dried to obtain KGM-Ti3C2T3 with oriented network channels and Janus layer for radioactive wastewater treatment. x Composite sponge (J-KTS-3).

[0070] Figure 1 ac show scanning electron microscopy (SEM) images of J-KTS at different magnifications. Due to the sublimation of internal ice crystals during freeze-drying, J-KTS shows many vertically aligned channels with a diameter of 10-20 μm. Figure 1 c shows a typical accordion structure of Ti3C2T x Embedded in the micron channels of J-KTS. The chemical composition of the top hydrophobic layer was characterized by SEM images and corresponding energy dispersive X-ray (EDX) elemental mapping ( Figure 2 ). Ti element comes from Ti3C2T x and evenly distributed throughout the J-KTS, indicating that Ti3C2T x The distribution of Si element indicates the successful construction of hydrophobic PDMS coating. In order to analyze the chemical composition of J-KTS, X-ray diffraction (XRD) patterns and Fourier transform infrared (FTIR) spectra are provided. Figure 3 ) as shown, KGM and Ti3C2T x All the diffraction peaks of were shown in J-KTS, indicating that the synthesis of J-KTS was successful. Figure 4 The FTIR spectra of the samples are shown, where KGM and Ti3C2T x All characteristic peaks of J-KTS are not shifted in the FTIR spectrum, which confirms the existence of Ti3C2T in the KGM network. x .

[0071] The optical properties of the samples were further evaluated by ultraviolet and visible (UV-vis) spectroscopy. Figure 5As shown, pure KGM exhibits relatively low light absorption. In contrast, Ti3C2T x and J-KTS exhibit strong light absorption in the range of 200 to 1000 nm. In addition, J-KTS and Ti3C2T x It also exhibits low light transmittance and reflectivity, and excellent near-infrared light absorption capability ( Figure 6 The excellent solar absorption capacity of J-KTS is due to the Ti3C2T x The surface of J-KTS was further verified to verify the Janus layer by water contact angle test. The contact angle of J-KTS bottom layer with water was 45.76 degrees ( Figure 7 In contrast, after hydrophobic treatment, the contact angle of the upper layer with water increased from 45.76 degrees to 126.26 degrees ( Figure 7 ). Therefore, J-KTS showed a Janus layer structure with an upper hydrophobic layer and a lower hydrophilic layer. Therefore, J-KTS has the potential to be an evaporator for efficient water evaporation.

[0072] To evaluate the effective solar-driven water evaporation of J-KTS, tests were conducted under simulated solar illumination using the following test methods:

[0073] KTS (~1 cm thick), J-KTS (~1 cm thick) or Ti3C2T x (0.1 g) was added to a 60 mL glass mold, and the light intensity of a xenon lamp with an AM 1.5 filter was adjusted to 1 kW m 2 (one sun) to simulate sunlight. In each test, a glass mold filled with 50mL of pure water or artificial radioactive wastewater was exposed to simulated sunlight. Changes in water quality were monitored by an electronic balance. In addition, infrared temperature images were taken by an infrared thermal imager.

[0074] To evaluate the photothermal purification capability of J-KTS, artificial radioactive wastewater (1.0 L) was prepared by dissolving UO2(NO3)2·6H2O (1.66 g), CsCl (1.27 g), and SrCl2·6H2O (3.04 g) in deionized water. NaCl (2.54 g), KCl (1.91 g), MnCl2·4H2O (3.60 g), and MgCl2 (3.91 g) were added to the artificial radioactive wastewater (1.0 L) to test the influence of coexisting ions.

[0075] The evaporation rate can be calculated by the following formula:

[0076]

[0077] where v is the evaporation rate, m is the mass of evaporated water, S is the area of ​​the sponge exposed to the sun, and dt is the exposure time.

[0078] The photothermal conversion efficiency can be estimated by the following formula:

[0079]

[0080] Where η is the solar thermal conversion efficiency, v is the evaporation rate, He is the total enthalpy of sensible heat and liquid-vapor phase change, and Qs is the illumination density of the incident solar energy.

[0081] In each test, the glass mold and the self-floating J-KTS were placed under constant simulated sunlight. Figure 8 As shown, the surface temperature variation of J-KTS was visually recorded by using an infrared camera, indicating that J-KTS has excellent photothermal performance and thermal diffusion. Fig. 9 The heating curves of different samples are shown, where J-KTS is at 1 kW·m 2 The simulated sunlight rapidly heated the sample to 45°C and remained stable within 10 minutes. In contrast, the temperature of KTS was 40°C after 10 minutes, while that of Ti3C2T x The temperature of the suspension was 35 °C. Therefore, the results further demonstrated the excellent photothermal conversion performance of J-KTS. In order to quantitatively test the output performance of solar-driven water vapor, the change of water mass over time was recorded by an electronic balance. Fig.10 As shown, at 1kw·m 2 After calculation, KTS and Ti3C2T x The evaporation rates of the suspension were 1.36 kg·m -2 h -1 and 0.45kg·m -2 h -1 In contrast, the evaporation rate of J-KTS is higher, up to 1.61 kg·m -2 h -1 In addition, from Figures 11-12 It can be seen that the water evaporation rates of J-KTS-1, J-KTS-2 and J-KTS-3 prepared by the present invention are higher, and better effects are achieved; Fig.13 As shown, Ti3C2T x The photothermal conversion efficiency of the suspension was only 31%, while that of KTS and J-KTS reached 82.6% and 93.0%, respectively. The difference in photothermal conversion efficiency between KTS and J-KTS is attributed to the different heat dissipation caused by the Janus layer. Since the upper layer of J-KTS floats on the water surface, the heat dissipation of J-KTS is smaller, while the heat dissipation of KTS is larger because the upper layer of KTS contacts the water surface.

[0082] In order to explore the water purification ability of J-KTS, a solution with a salt ion concentration of 1 g / L was prepared to simulate seawater. After treatment with J-KTS under light, the concentrations of Na, K, Ca, and Mg were greatly reduced ( Fig.14 ). When a pile of salt (NaCl) was sprayed on the surface of J-KTS, the salt was eliminated within 100 minutes ( Fig.15 ). Therefore, J-KTS has excellent self-cleaning function. The unique salt resistance of J-KTS is due to the Janus layer, which establishes a balance between salt ion absorption and diffusion.

[0083] like Fig.16 As shown, using simulated radioactive wastewater at 1kw·m 2 The purification effect of J-KTS on radioactive elements (Sr, Cs and U) was tested under simulated sunlight. The concentrate evaporated by J-KTS was collected and the ion concentration was determined by inductively coupled plasma mass spectrometry (ICP-MS). After solar-driven purification, the concentrations of Sr, Cs and U in the simulated radioactive wastewater decreased from 1 g / L to 6.098, 12.452 and 7.361 μg / L, respectively. Fig.16 ). In addition, from Figures 17-18 It can be seen that the J-KTS-1, J-KTS-2 and J-KTS-3 prepared by the present invention have better purification effects on radioactive elements (Sr, Cs and U), and have achieved better purification effects; the SEM image and corresponding EDX element mapping of J-KTS after solar-driven radioactive wastewater purification show the distribution of Sr, Cs and U, indicating that the radioactive elements are adsorbed on J-KTS ( Fig.19 ). In addition, considering the high acidity and high salt concentration of radioactive wastewater in actual situations, the purification effect of J-KTS was further tested under different pH and coexisting salt ions. Fig. 20 It can be seen that the effect of pH on the purification of radioactive wastewater is negligible, while J-KTS still has a large water evaporation rate at different pH values ​​( Fig.21 ). To evaluate the purification effect in the presence of salt ions, 1 g / LM ions (here M = Na + , K + , Mn 2+ Mg 2+ ) simulation test. The results show that the coexisting ions have little effect on the purification of Sr, Cs and U in J-KTS ( Fig. 22 ). In addition, the structure of J-KTS remained stable without dissolving at pH = 1 and 1g / LM ions. For cost reasons, the durability and stability of the material are crucial. Therefore, a cycle test was performed to confirm the stability of J-KTS. Fig.23 As shown, J-KTS exhibited an extremely stable water evaporation rate even after 10 cycles.

[0084] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for preparing a natural polymer nanocomposite sponge for radionuclide enrichment and separation, characterized in that: The following steps are involved: Step 1: Add Ti3AlC2 powder into hydrofluoric acid solution, heat to react, centrifuge, wash, and then vacuum dry to obtain Ti3C2T x MXene powder; Step 2: Ultrasonication of Ti3C2T x MXene powder was evenly dispersed in water to obtain Ti3C2T x Then, KGM was added to Ti3C2T x The suspension was stirred to obtain KGM-Ti3C2T x Hydrogel; Step 3: KGM-Ti3C2T x The hydrogel is poured into a mold, the bottom of the mold is fixed on a steel plate, the steel plate is placed in liquid nitrogen for directional freezing, and then vacuum dried; the vacuum dried sample is immersed in a NaOH ethanol solution, heated, and kept warm; Subsequently, the sample was washed and freeze-dried again to obtain KGM-Ti3C2T x sponge; Step 4: On KGM-Ti3C2T x The top layer of the sponge was coated with PDMS solution and then vacuum dried to obtain KGM-Ti3C2T3 with oriented network channels and Janus layer for radioactive wastewater treatment. x Composite sponge, i.e. natural polymer nanocomposite sponge; In the step 1, the concentration of the hydrofluoric acid solution is 5-15wt%; the mass volume ratio of the Ti3AlC2 powder to the hydrofluoric acid solution is 1g:10mL; In the step 1, the heating reaction temperature is 85-95°C and the time is 0.5-1.5h; the washing is carried out with deionized water until the pH value is 6, and the vacuum drying time is 24h; In the step 2, Ti3C2T x The mass volume ratio of MXene powder to water is 0.5 g:100 mL; the Ti3C2T x The mass ratio of MXene powder to KGM is 1:2~5; the stirring time is 10~15h; In the step 2, dual-frequency ultrasound is applied during stirring; the frequencies of the dual-frequency ultrasound are 35-55kHz and 100-135kHz, the time of dual-frequency ultrasound alternation is 25-30s, and the power of the dual-frequency ultrasound is 400-500W.

2. The method for preparing the natural polymer nanocomposite sponge for radionuclide enrichment and separation as claimed in claim 1, characterized in that: In the step 3, the concentration of the NaOH ethanol solution is 2-5wt%; the heating temperature is 40-50°C, and the insulation time is 4-8h.

3. The method for preparing the natural polymer nanocomposite sponge for radionuclide enrichment and separation as claimed in claim 1, characterized in that: In the step 3, the vacuum-dried sample is immersed in a NaOH ethanol solution, and then added to a microwave-ultrasonic integrated reactor, and microwave and ultrasonic waves are turned on at the same time, and the synergistic treatment is performed at a treatment temperature of 40-50°C for 2-3 hours; then, the sample is washed and freeze-dried again to obtain KGM-Ti3C2T x Sponge; the microwave power of the coordinated treatment is 300~500W, the ultrasonic power is 300~500W, and the ultrasonic frequency is 40~55KHz.

4. The method for preparing the natural polymer nanocomposite sponge for radionuclide enrichment and separation as claimed in claim 1, characterized in that: In the step 4, the concentration of the PDMS solution is 0.5-1.5wt%.

5. Use of a natural polymer nanocomposite sponge prepared by the preparation method according to any one of claims 1 to 4 in treating radioactive wastewater, characterized in that: Natural polymer nanocomposite sponge is added to radioactive wastewater and irradiated with light to achieve evaporation and purification of the radioactive wastewater.