Positive electrode, lithium battery including the positive electrode, and method for manufacturing the positive electrode

By using the structure of a composite positive electrode active material, including a lithium transition metal oxide core and a carbonaceous material shell, the problem of deterioration of the positive electrode density in the prior art is solved, and the circulation characteristics and energy density of the lithium battery are improved.

CN114843457BActive Publication Date: 2024-12-06SAMSUNG SDI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202210105474.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-02-01
Filing Date
2022-01-28
Publication Date
2024-12-06
Estimated Expiration
2042-01-28

AI Technical Summary

Technical Problem

The density deterioration of the existing lithium battery positive electrode during the cycle process leads to a decrease in energy density, and it is difficult to simultaneously improve the circulation characteristics and mixing density.

Method used

A new positive electrode including a composite positive electrode active material is adopted. The composite positive electrode active material consists of a lithium transition metal oxide core and a carbonaceous material shell. The carbonaceous conductive agent is only present in the shell, and the first metal oxide content is 0.3 wt% or more. High, uniform shell is formed by mechanical grinding to prevent contact between the core and the electrolyte.

Benefits of technology

The cycle characteristics and energy density of lithium batteries are improved, side reactions and resistance layers are generated, elution of transition metal ions is suppressed, and internal resistance is maintained or reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114843457B_ABST
    Figure CN114843457B_ABST
Patent Text Reader

Abstract

A positive electrode, a lithium battery including the positive electrode, and a method for manufacturing the positive electrode are provided. The positive electrode may include a positive electrode current collector and a positive active material layer on the positive electrode current collector. The positive active material layer may include a composite positive electrode active material and a binder. The composite positive electrode active material may include a core including a lithium transition metal oxide and a shell disposed on the surface of the core and conforming to the surface of the core. The shell may include a a O b (0
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is based on and claims the benefit of priority from Korean Patent Application No. 10-2021-0014324 filed on February 1, 2021, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field

[0002] One or more embodiments relate to a positive electrode, a lithium battery including the positive electrode, and a method of manufacturing the positive electrode. Background Art

[0003] In order to meet the miniaturization and high performance of various devices, high energy density is becoming more and more important in addition to the miniaturization and lightness of lithium batteries. In other words, high-capacity lithium batteries are becoming more and more important.

[0004] In order to realize a lithium battery suitable for such use, a positive electrode having a high mixing density is being considered.

[0005] The existing positive electrode is prepared by mixing a positive electrode active material and a binder with a carbonaceous conductive agent.

[0006] Since the positive electrode contains a carbonaceous conductive agent, the cycle characteristics of the lithium battery are improved, but the mixture density of the positive electrode is deteriorated. As a result, the energy density of the lithium battery is deteriorated.

[0007] Therefore, a method of preventing the degradation of the cycle characteristics of a lithium battery and simultaneously increasing the mixing density of a positive electrode is needed. Summary of the invention

[0008] One or more embodiments include a novel positive electrode having excellent room temperature and high temperature life characteristics.

[0009] One or more embodiments include a lithium battery having improved energy density by including the positive electrode.

[0010] One or more embodiments include a method of manufacturing the positive electrode.

[0011] Additional aspects will be set forth in part in the description which follows and, in part, will be apparent from the description, or may be learned by practice of the presented disclosed embodiments.

[0012] According to an embodiment, the positive electrode may include:

[0013] a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector,

[0014] The positive electrode active material layer may include a composite positive electrode active material and a binder.

[0015] The composite positive electrode active material may include: a core including a lithium transition metal oxide; and a shell disposed on the surface of the core and conformal with the surface of the core.

[0016] The shell may include: at least one first metal oxide represented by the formula M a O b (where 0 < a ≤ 3 and 0 < b < 4, provided that a is 1, 2, or 3 and b may not be an integer); and a carbonaceous material.

[0017] The at least one first metal oxide may be disposed in a carbonaceous material matrix, and M may be at least a metal selected from Group 2 to Group 13, Group 15, and Group 16 of the periodic table.

[0018] The positive electrode active material layer may include a carbonaceous conductive agent, and the carbonaceous conductive agent may be present only in the shell, and

[0019] In the total content of the composite positive electrode active material, the content of the first metal oxide may be 0.3 wt% or higher.

[0020] According to another embodiment,

[0021] The lithium battery may include this positive electrode.

[0022] According to still another embodiment, a method of manufacturing a positive electrode may include:

[0023] Providing a composite positive electrode active material;

[0024] Preparing a positive electrode active material composition including the composite positive electrode active material and a binder; and preparing a positive electrode by providing the positive electrode active material composition or its dry matter on a positive electrode current collector,

[0025] wherein the positive electrode active material composition may not include a carbonaceous conductive agent. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The above and other aspects, features, and advantages of certain embodiments disclosed will become more apparent from the following description in conjunction with the drawings, in which:

[0027] Figure 1 A schematic diagram of an embodiment of a lithium battery is shown;

[0028] Figure 2 is a scanning electron microscope (SEM) image of a cross-section of the positive electrode manufactured in Example 1; and

[0029] Figure 3 is a scanning electron microscope (SEM) image of a cross-section of the positive electrode manufactured in Comparative Example 4. DETAILED DESCRIPTION

[0030] Now will refer to embodiment in detail, the example of embodiment is shown in the accompanying drawings, wherein the same reference numerals refer to the same element from time to time. In this regard, the embodiment provided can have different forms, and should not be construed as being limited to the description set forth herein. Therefore, the embodiment is described below only by reference to the drawings to explain the aspects of this description. As used herein, the term "and / or" includes any combination and all combinations of one or more of the related listed items. When a statement such as "at least one (kind / person) of ... " is after a column of elements (elements), what is modified is the entire column of elements (elements), rather than modifying the individual elements (elements) in the column.

[0031] Since the inventive concept allows various changes and many embodiments, specific embodiments will be shown in the drawings and described in detail in the specification. However, this is not intended to limit the inventive concept to a specific mode of practice, and it will be understood that all changes, equivalents and substitutes that do not depart from the spirit and technical scope of the inventive concept are included in the inventive concept.

[0032] The terms used in this specification are only used to describe specific embodiments and are not intended to limit the inventive concept. The expressions used in the singular cover the expressions of the plural number unless they have a significantly different meaning in the context. In this specification, it will be understood that the terms such as "including", "having" etc. are intended to indicate the presence of features, numbers, steps, actions, components, parts, ingredients, materials or combinations thereof disclosed in the specification, and are not intended to exclude the possibility that one or more other features, numbers, steps, actions, components, parts, ingredients, materials or combinations thereof may be present or may be added. As used herein, " / " can be interpreted as referring to "and" or "or" according to the context.

[0033] In the drawings, the thickness of layers and regions is exaggerated or reduced for clarity. The same reference numerals in the drawings and the specification represent the same elements. In this specification, it will be understood that when an element (e.g., a layer, a film, a region, or a substrate) is referred to as being "on" or "above" another element, the element may be directly on the other element, or there may be an intervening layer. Although various components may be described using terms such as "first", "second", etc., these components are not necessarily limited to the above terms. The above terms are only used to distinguish one component from another component.

[0034] Hereinafter, according to example embodiments, a positive electrode, a lithium battery including the positive electrode, and a method of manufacturing the positive electrode will be described in more detail.

[0035] The positive electrode may include a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector. Among them, the positive electrode active material layer may include a composite positive electrode active material and a binder. The composite positive electrode active material may include a core containing a lithium transition metal oxide and a shell disposed on the surface of the core and conformal with the surface of the core. The shell may include: at least one first metal oxide represented by the formula M a O b (where 0 < a ≤ 3 and 0 < b < 4, provided that a is 1, 2, or 3 and b may not be an integer); and a carbonaceous material. The at least one first metal oxide may be disposed in a carbonaceous material matrix, and M may be at least a metal selected from Group 2 to Group 13, Group 15, and Group 16 of the periodic table. The positive electrode active material layer may include a carbonaceous conductive agent, and the carbonaceous conductive agent may only be present in the shell. And the content of the first metal oxide may be 0.3 wt% or more of the total content of the composite positive electrode active material.

[0036] Hereinafter, the theoretical basis for providing the excellent effects of the positive electrode according to the embodiments will be described. However, this theoretical basis is for helping to understand the inventive concept and is not intended to limit the inventive concept in any way.

[0037] In the positive electrode, the carbonaceous conductive agent may be present in the positive electrode by being included in the shell of the composite positive electrode active material, and the carbonaceous conductive agent may not be present in other regions of the positive electrode. That is, the positive electrode may include a composite positive electrode active material coated with a carbonaceous conductive agent and may not additionally include a separate carbonaceous conductive agent. Since the positive electrode may not include a separate conductive agent, the positive electrode may have a higher mixture density compared to a positive electrode that also includes a separate conductive agent. As a result, a lithium battery including this positive electrode may have an improved energy density.

[0038] In addition, the positive electrode may include a composite positive electrode active material having a new structure. A shell including a first metal oxide and a carbonaceous material may be provided on the core of the composite positive electrode active material. Due to agglomeration, it may be difficult to coat the existing carbonaceous material on the core. However, by using a first composite including a plurality of first metal oxides located in a carbonaceous material matrix in the composite positive electrode active material, agglomeration of the carbonaceous material can be prevented, and a uniform shell can be formed on the core. By effectively blocking the contact between the core and the electrolyte, side reactions caused by the contact between the core and the electrolyte can be prevented. In addition, the generation of the resistance layer can be suppressed by suppressing the cation mixing of the electrolyte solution. In addition, the elution of transition metal ions can also be suppressed. The carbonaceous material may be, for example, a crystalline carbonaceous material. The carbonaceous material may be, for example, a carbonaceous nanostructure. The carbonaceous material may be, for example, a two-dimensional carbonaceous nanostructure. The carbonaceous material may be, for example, graphene. In this case, since the shell containing graphene is flexible, the occurrence of cracks inside the composite positive electrode active material can be suppressed by easily adapting to the volume change of the composite positive electrode active material during charging and discharging. Since graphene has high electronic conductivity, the interfacial resistance between the composite positive active material and the electrolyte solution is reduced. Therefore, despite the introduction of a shell containing graphene, the internal resistance of the lithium battery can be maintained or reduced. In addition, since the first metal oxide has a high voltage resistance (i.e., high voltage resistance), it is possible to prevent the degradation of the lithium transition metal oxide included in the core during charging and discharging at high voltage. As a result, the cycle characteristics and high temperature stability of the lithium battery containing the composite positive active material can be improved. For example, the shell may contain one type of first metal oxide or two or more different types of first metal oxides. By including a carbonaceous material as described above, the shell included in the composite positive active material can be used as a carbonaceous conductive agent at the same time.

[0039] Since the carbonaceous material included in the shell of the composite positive active material is derived from a graphene matrix, the carbonaceous material may have a relatively low density and a high porosity compared to existing carbonaceous materials derived from graphite-based materials. The d002 interplanar spacing of the carbonaceous material included in the shell of the composite positive active material may be, for example, or larger, or larger, or larger, or larger, or larger, or greater or The d002 interplanar spacing of the carbonaceous material included in the shell of the composite positive active material may be, for example, about To about About To about About To about About To about or approximately To about The d002 interplanar spacing of existing carbonaceous materials derived from graphite-based materials can be, for example, or less or approximately To about

[0040] Therefore, although the positive electrode does not include a separate carbonaceous conductive agent, by including the composite positive electrode active material, the cycle characteristics and energy density of a lithium battery including the positive electrode can be improved at the same time.

[0041] Based on the total weight of the composite positive electrode active material, the content of the shell in the composite positive electrode active material can be, for example, in the range of about 0.5wt% to about 3wt%, about 0.5wt% to about 2.5wt%, about 0.5wt% to about 2wt%, or about 0.5wt% to about 1.5wt%. In addition, based on the total weight of the composite positive electrode active material, the content of the first metal oxide can be in the range of about 0.3wt% to about 1.8wt%, about 0.3wt% to about 1.5wt%, about 0.3wt% to about 1.2wt%, or about 0.3wt% to about 0.9wt%. Since the composite positive electrode active material contains the shell and the first metal oxide within these content ranges, the cycle characteristics of the lithium battery can be further improved.

[0042] like Figure 2 As shown in , in a positive electrode that does not include a separate carbonaceous conductive agent, the positive electrode active material layer may include a plurality of composite positive electrode active material particles. The plurality of composite positive electrode active material particles included in the positive electrode may be arranged adjacent to each other, and voids may be arranged between adjacent composite positive electrode active material particles. The voids may be defined by adjacent composite positive electrode active material particles. For example, the size and shape of the voids may be defined by adjacent composite positive electrode active material particles. The shape of the void may be, for example, a non-spherical shape. The shape of the void may be, for example, a polyhedral shape. The sphericity of the void may be, for example, 0.9 or less, 0.8 or less, or 0.7 or less. The sphericity of the void may be, for example, the ratio of the surface area of ​​spherical pores of equal volume to the surface area of ​​the void itself. As Figure 2 As shown in , a plurality of voids may be arranged, for example, irregularly and non-periodically in the positive electrode.

[0043] like Figure 3As shown, in the positive electrode including a separate carbonaceous conductive agent, the carbonaceous conductive agent may be filled in the space between adjacent composite positive electrode active material particles. Therefore, there are no voids defined by adjacent composite positive electrode active material particles. For example, in the positive electrode including a separate carbonaceous conductive agent, the voids may be defined by adjacent carbonaceous conductive agents, or the voids may be defined by adjacent carbonaceous conductive agents and composite positive electrode active material particles.

[0044] The metal included in the first metal oxide may be at least one metal selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide may be, for example, selected from Al2O z (where 0 < z < 3), NbO x (where 0 < x < 2.5), MgO x (where 0 < x < 1), Sc2O z (where 0 < z < 3), TiO y (where 0 < y < 2), ZrO y (where 0 < y < 2), V2O z (where 0 < z < 3), WO y (where 0 < y < 2), MnO y (where 0 < y < 2), Fe2O z (where 0 < z < 3), Co3O w (where 0 < w < 4), PdO x (where 0 < x < 1), CuO x (where 0 < x < 1), AgO x (where 0 < x < 1), ZnO x (where 0 < x < 1), Sb2O z (where 0 < z < 3) and SeO y (where 0 < y < 2). By disposing the first metal oxide in the carbonaceous material matrix, the uniformity of the shell disposed on the core can be improved, and the voltage resistance (i.e., voltage resistance) of the composite positive electrode active material can be further improved. For example, the shell may include Al2O z (where 0 < z < 3) as the first metal oxide.

[0045] The shell may further include a compound represented by the formula M a O c(where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2, or 3 and c can be an integer) represents at least one second metal oxide. M can be at least one metal selected from Groups 2 to 13, 15, and 16 of the periodic table. For example, the second metal oxide can include the same metal as the metal of the first metal oxide, and the ratio c / a of c to a in the second metal oxide can be greater than the ratio b / a of b to a in the first metal oxide. For example, c / a > b / a. The second metal oxide can be selected from Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2. The first metal oxide can be a reduction product of the second metal oxide. The first metal oxide can be obtained by reducing some or all of the second metal oxide. Accordingly, the oxygen content of the first metal oxide can be less than the oxygen content of the second metal oxide, and the first metal oxide can have a metal oxidation number less than the metal oxidation number of the second metal oxide. For example, the shell can include Al2O z (where 0 < z < 3) and Al2O3 as the second metal oxide.

[0046] In the composite cathode active material, for example, the transition metal of the carbonaceous material included in the shell and the lithium transition metal oxide included in the core can be chemically bonded to each other. The carbon atoms (C) of the carbonaceous material included in the shell and the transition metal (Me) of the lithium transition metal oxide can be chemically bonded through an oxygen atom (e.g., through a C-O-Me bond (e.g., a C-O-Co bond)). The carbonaceous material included in the shell and the lithium transition metal oxide included in the core can be chemically bonded through a chemical bond, and thus the core and the shell form a composite cathode active material. Accordingly, the composite cathode active material can be distinguished from a simple physical mixture of the carbonaceous material and the lithium transition metal oxide.

[0047] In addition, the first metal oxide and the carbonaceous material included in the shell can be chemically bonded through a chemical bond. Here, the chemical bond can be, for example, a covalent bond or an ionic bond. The covalent bond can be a bond including at least one of an ester group, an ether group, a carbonyl group, an amide group, a carbonate anhydride group, and an acid anhydride group. The ionic bond can be a bond including, for example, a carboxylate ion, an ammonium ion, an acyl cation group, etc.

[0048] The thickness of the shell can be, for example, about 1 nm to about 5 μm, about 1 nm to about 1 μm, about 1 nm to about 500 nm, about 1 nm to about 200 nm, about 1 nm to about 100 nm, about 1 nm to about 90 nm, about 1 nm to about 80 nm, about 1 nm to about 70 nm, about 1 nm to about 60 nm, about 1 nm to about 50 nm, about 1 nm to about 40 nm, about 1 nm to about 30 nm, about 1 nm to about 20 nm, or about 1 nm to about 10 nm. The increase in the internal resistance of a lithium battery including a composite positive active material can be suppressed by having a shell having a thickness in any range within these ranges.

[0049] The positive electrode active material may also include a third metal coated on the core or a third metal oxide coated on the core. In addition, the shell may be disposed on the coated third metal or the coated third metal oxide. For example, after the third metal is coated on the surface of the lithium transition metal oxide included in the core or the third metal oxide is coated on the surface of the lithium transition metal oxide, the shell may be disposed on the third metal and / or the third metal oxide. For example, the composite positive electrode active material may include: a core; an intermediate layer, disposed on the core; and a shell, disposed on the intermediate layer, wherein the intermediate layer may include a third metal or a third metal oxide. The third metal may be at least one metal selected from Al, Zr, W and Co, and the third metal oxide may be Al2O3, ZrO2, WO2, CoO, Co2O3 or Co3O4.

[0050] The shell included in the composite positive active material may include, for example, at least one selected from a first metal oxide and a carbonaceous material. The shell included in the composite positive active material may include, for example, at least one selected from a grinding product of graphene and a first composite, and the first metal oxide may be located in a carbonaceous material matrix (e.g., a graphene matrix). The shell may be prepared, for example, from a first composite including a first metal oxide and graphene. In addition to the first metal oxide, the first composite may also include a second metal oxide. The first composite may include, for example, at least two types of first metal oxides. The first composite may include, for example, at least two types of first metal oxides and at least two types of second metal oxides.

[0051] Based on the total weight of the composite positive active material, the content of the first composite included in the composite positive active material may be 3 wt% or less, 2.5 wt% or less, 2 wt% or less, or 1.5 wt% or less. Based on the total weight of the composite positive active material, the content of the first composite may be in the range of about 0.5 wt% to about 3 wt%, about 0.5 wt% to about 2.5 wt%, about 0.5 wt% to about 2 wt%, or about 0.5 wt% to about 1.5 wt%. When the composite positive active material includes the first composite within any of these ranges, a lithium battery including the composite positive active material may have improved cycle characteristics.

[0052] The average diameter of at least one selected from the first metal oxide and the second metal oxide included in the first composite can be in the range of about 1 nm to about 1 μm, about 1 nm to about 500 nm, about 1 nm to about 200 nm, about 1 nm to about 100 nm, about 1 nm to about 70 nm, about 1 nm to about 50 nm, about 1 nm to about 30 nm, about 3 nm to about 30 nm, about 3 nm to about 25 nm, about 5 nm to about 25 nm, about 5 nm to about 20 nm, about 7 nm to about 20 nm, or about 7 nm to about 15 nm. When the first metal oxide and / or the second metal oxide have such a nanometer-scale diameter, the first metal oxide and / or the second metal oxide can be uniformly distributed in the carbonaceous material matrix (e.g., graphene matrix) of the first composite. Therefore, the first composite can be uniformly coated on the core to form a shell. In addition, the first metal oxide and / or the second metal oxide can be more uniformly arranged on the core by having a diameter within this range. Therefore, by uniformly disposing the first metal oxide and / or the second metal oxide on the core, high voltage resistance (ie, high withstand voltage) can be more effectively exhibited.

[0053] The average diameter of the first metal oxide and the second metal oxide can be measured using a measuring device such as a laser diffraction method or a dynamic light scattering method. In this specification, the average diameter is a value measured by using, for example, a laser scattering particle size distribution instrument (e.g., Horiba LA-920), and is a median particle size (D50) corresponding to 50% of the cumulative particle size distribution curve weighted by volume from small particles.

[0054] The uniformity deviation of at least one selected from the first metal oxide and the second metal oxide included in the first composite may be 3% or less, 2% or less, or 1% or less. The uniformity can be calculated by, for example, XPS. Therefore, at least one selected from the first metal oxide and the second metal oxide included in the first composite may have a deviation of 3% or less, 2% or less, or 1% or less, and may be uniformly distributed.

[0055] The carbonaceous material included in the first composite may have a branched structure, for example, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed in the branched structure of the carbonaceous material. The branched structure of the carbonaceous material may include, for example, a plurality of carbonaceous material particles in contact with each other. The carbonaceous material may provide various conductive paths by having a branched structure.

[0056] The carbonaceous material included in the first composite may be, for example, graphene. For example, the graphene may have a branched structure, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed in the branched structure of the graphene. For example, the branched structure of the graphene may include a plurality of graphene particles in contact with each other. The graphene may provide various conductive paths by having a branched structure.

[0057] The carbonaceous material included in the first composite can have a spherical structure, for example, and at least one metal oxide selected from the first metal oxide and the second metal oxide can be distributed in the spherical structure. The size of the spherical structure of the carbonaceous material can be in the range of about 50nm to about 300nm. There can be a plurality of carbonaceous materials having a spherical structure. The carbonaceous material can have a spherical structure, and therefore, the first composite can have a firm structure.

[0058] The carbonaceous material included in the first composite may be, for example, graphene. The graphene may have, for example, a spherical structure, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed in the spherical structure. The size of the spherical structure of the graphene may be in the range of about 50 nm to about 300 nm. There may be a plurality of graphenes having a spherical structure. The graphene may have a spherical structure, and therefore, the first composite may have a firm structure.

[0059] The carbonaceous material included in the first composite may have, for example, a spiral structure in which a plurality of spherical structures are connected, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed in the spherical structure of the spiral structure. The size of the spiral structure of the carbonaceous material may be in the range of about 500 nm to about 100 μm. The carbonaceous material may have a spiral structure, and therefore, the first composite may have a strong structure.

[0060] The carbonaceous material included in the first composite may be, for example, graphene. Graphene, for example, may have a spiral structure in which a plurality of spherical structures are connected, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed in the spherical structure of the spiral structure. The size of the spiral structure of the graphene may be in the range of about 500 nm to about 100 μm. Graphene may have a spiral structure, and therefore, the first composite may have a strong structure.

[0061] The carbonaceous material included in the first composite may, for example, have a cluster structure in which a plurality of spherical structures are agglomerated, and at least one metal oxide selected from the first metal oxide and the second metal oxide may be distributed in the spherical structure of the cluster structure. The size of the cluster structure of the carbonaceous material may be in the range of about 0.5 mm to about 10 cm. The carbonaceous material may have a cluster structure, and therefore, the first composite may have a firm structure.

[0062] The carbonaceous material included in the first composite can be, for example, graphene. Graphene, for example, can have a cluster structure in which a plurality of spherical structures are agglomerated, and at least one metal oxide selected from the first metal oxide and the second metal oxide can be distributed in the spherical structure of the cluster structure. The size of the cluster structure of graphene can be in the range of about 0.5 mm to about 10 cm. Graphene can have a cluster structure, and therefore, the first composite can have a stable structure.

[0063] For example, the first composite can be a wrinkled polyhedral spherical structure, and at least one selected from the first metal oxide and the second metal oxide can be distributed inside or on the surface of the wrinkled polyhedral spherical structure. Since the first composite is such a polyhedral spherical structure, the first composite can be easily coated on the irregular surface of the core.

[0064] For example, the first composite can be a planar structure, and at least one selected from the first metal oxide and the second metal oxide can be distributed inside or on the surface of the planar structure. Since the first composite is such a two-dimensional planar structure, the first composite can be easily coated on the irregular surface of the core.

[0065] The carbonaceous material included in the first composite can extend from the first metal oxide by a distance of 10 nm or less, and can include 1 to 20 carbonaceous material layers. For example, a carbonaceous material having a total thickness of 12 nm or less can be provided on the first metal oxide by stacking a plurality of carbonaceous material layers. For example, the total thickness of the carbonaceous material can be in the range of about 0.6 nm to about 12 nm.

[0066] The carbonaceous material included in the first composite may be, for example, graphene. The graphene may extend a distance of 10 nm or less from the first metal oxide and may include at least 1 to 20 graphene layers. For example, graphene having a total thickness of 12 nm or less may be provided on the first metal oxide by stacking a plurality of graphene layers. For example, the total thickness of the graphene may be in the range of about 0.6 nm to about 12 nm.

[0067] The core included in the composite positive electrode active material may include, for example, a lithium transition metal oxide represented by Formula 1 or Formula 2:

[0068] Formula 1

[0069] Li a Ni x Co y M z O 2-b A b

[0070] Wherein, in Formula 1,

[0071] 0.9 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0. ≤ x ≤ 0.95, 0 ≤ y ≤ 0.2, 0 < z ≤ 0.2, and x + y + z = 1,

[0072] M may be manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof, and

[0073] A may be F, S, Cl, Br, or a combination thereof.

[0074] Formula 2

[0075] Li a Co x M y O 2-b A b

[0076] Wherein, in Formula 2,

[0077] 1.0 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0.9 ≤ x ≤ 1, 0 ≤ y ≤ 0.1, and x + y = 1,

[0078] M may be manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof, and

[0079] A can be F, S, Cl, Br, or a combination thereof.

[0080] The core included in the composite positive electrode active material may include, for example, a lithium transition metal oxide represented by one of Formula 3 to Formula 5, Formula 9, and Formula 10:

[0081] Formula 3

[0082] LiNi x Co y Mn z O2

[0083] Formula 4

[0084] LiNi x Co y Al z O2

[0085] Formula 5

[0086] LiNi x Co y Mn v Al w O2

[0087] Wherein, in Formulas 3 to 5, 0.8 ≤ x ≤ 0.95, 0 < y ≤ 0.2, 0 < z ≤ 0.2, 0 < v ≤ 0.2, 0 < w ≤ 0.2, x + y + z = 1, and x + y + v + w = 1.

[0088] Based on the total mole number of the transition metals, the lithium transition metal oxides of Formula 1 and Formulas 3 to 5 can have a high nickel content of 80 mol% or higher, 85 mol% or higher, or 90 mol% or higher, while providing excellent initial capacity, room temperature life characteristics, and high temperature life characteristics. For example, based on the total mole number of the transition metals, the lithium transition metal oxides of Formula 1 and Formulas 3 to 5 can have a high nickel content in the range of about 80 mol% to about 95 mol%, about 85 mol% to about 95 mol%, or about 90 mol% to about 95 mol%.

[0089] Formula 9

[0090] Li a M1 x M2 y PO 4-b X b

[0091] Wherein, in Formula 9, 0.90 ≤ a ≤ 1.1, 0 ≤ x ≤ 0.9, 0 ≤ y ≤ 0.5, 0.9 < x + y < 1.1, and 0 ≤ b ≤ 2,

[0092] M1 may be chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof, and

[0093] M2 may be magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zinc (Zn), boron (B), niobium (Nb), gallium (Ga), indium (In), molybdenum (Mo), tungsten (W), aluminum (Al), silicon (Si), chromium (Cr), vanadium (V), scandium (Sc), yttrium (Y), or a combination thereof, and X may be O, F, S, P, or a combination thereof.

[0094] Formula 10

[0095] Li a M3 z PO4

[0096] Wherein, in formula 10, 0.90≤a≤1.1 and 0.9≤z≤1.1,

[0097] M3 may be chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof.

[0098] A lithium battery according to another embodiment may include a positive electrode.

[0099] By including a positive electrode, a lithium battery may provide improved cycle characteristics, thermal stability, and energy density.

[0100] For example, a lithium battery can be manufactured by the following method, but the manufacturing is not necessarily limited to the following method and can be adjusted according to required conditions.

[0101] First, a positive electrode may be manufactured. A method of manufacturing a positive electrode may be understood by referring to the description of a method of manufacturing a positive electrode provided herein.

[0102] Next, the negative electrode can be manufactured as follows. For example, the negative electrode can be manufactured in substantially the same manner as the positive electrode except that the negative electrode active material is used instead of the composite positive electrode active material and a separate conductive agent is used. In addition, in the negative electrode active material composition, a conductive agent, a binder, and a solvent substantially the same as those in the positive electrode can be used.

[0103] For example, a negative electrode active material, a conductive agent, a binder, and a solvent may be mixed to prepare a negative electrode active material composition. The negative electrode active material composition may be directly coated on a copper current collector to prepare a negative electrode plate. In some embodiments, the negative electrode active material composition may be cast on a separate support to form a negative electrode active material film, which may then be separated from the support and laminated on a copper current collector to prepare a negative electrode plate.

[0104] In one or more embodiments, the negative electrode active material may be any suitable negative electrode active material available in the art for lithium batteries. For example, the negative electrode active material may include at least one selected from lithium metal, metals alloyable with lithium, transition metal oxides, non-transition metal oxides, and carbonaceous materials.

[0105] Examples of metals alloyable with lithium include silicon (Si), tin (Sn), aluminum (Al), germanium (Ge), lead (Pb), bismuth (Bi), antimony (Sb), Si-Y alloys (where Y is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, transition metal, rare earth element, or a combination thereof, and Y is not Si), and Sn-Y alloys (where Y is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, transition metal, rare earth element, or a combination thereof, and Y is not Sn). For example, Y may be magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), rutherfordium (Rf), vanadium (V), niobium (Nb), tantalum (Ta), dubnium (Db), chromium (Cr), molybdenum (Mo), tungsten (W), seaborgium (Sg), technetium (Tc), rhenium (Re), bohrium (Bh), iron (Fe), lead (Pb), ruthenium (Ru), osmium (Os), hassium (Hs), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), boron (B), aluminum (Al), gallium (Ga), tin (Sn), indium (In), titanium (Ti), germanium (Ge), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), polonium (Po), or a combination thereof.

[0106] For example, the transition metal oxide may be lithium titanate oxide, vanadium oxide, or lithium vanadium oxide.

[0107] The non-transition metal oxide may be, for example, SnO2, SiO x (0 < x < 2), etc.

[0108] Examples of carbonaceous materials may include crystalline carbon, amorphous carbon, and mixtures thereof. For example, crystalline carbon may be amorphous graphite, tabular graphite, flake graphite, spherical graphite, or fibrous graphite, such as natural graphite or artificial graphite. Examples of amorphous carbon may include soft carbon (carbon sintered at low temperature), hard carbon, mesophase pitch carbide, and calcined coke.

[0109] Examples of conductive agents may include: carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fibers; carbon nanotubes; powder, fiber or tubular metal materials such as copper, nickel, aluminum, silver, etc.; and conductive polymers such as polyphenylene derivatives. Any suitable conductive agent available in the art may be used.

[0110] The amounts of the negative electrode active material, the conductive agent, the binder and the solvent may be the same as those commonly used in lithium batteries in the art. Depending on the purpose and structure of the lithium battery, at least one of the conductive agent, the binder and the solvent may be omitted.

[0111] Based on the total weight of the negative electrode active material layer, the content of the binder in the negative electrode may be, for example, in the range of about 0.1wt% to about 10wt% or about 0.1wt% to about 5wt%. Based on the total weight of the negative electrode active material layer, the content of the conductive agent in the negative electrode may be, for example, in the range of about 0.1wt% to about 10wt% or about 0.1wt% to about 5wt%. Based on the total weight of the negative electrode active material layer, the content of the negative electrode active material in the negative electrode may be, for example, in the range of about 90wt% to about 99wt% or about 95wt% to about 99wt%. When the negative electrode active material is lithium metal, the negative electrode may not include a binder and a conductive agent.

[0112] Next, a separator to be provided between the positive electrode and the negative electrode is prepared.

[0113] The separator for lithium battery can be any suitable separator commonly used in lithium battery. For example, the separator can have low resistance to ion migration in the electrolyte and have electrolyte solution retention ability (electrolytic solution-retaining ability). Examples of separators can include glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), and combinations thereof, which can all be non-woven fabrics or textiles. For example, a rollable separator comprising polyethylene or polypropylene can be used for lithium ion batteries. A separator with good organic electrolyte solution retention ability can be used for lithium ion polymer batteries.

[0114] For example, a lithium battery can be manufactured by the following method, but the manufacturing is not necessarily limited to the following method and can be adjusted according to required conditions.

[0115] First, the polymer resin, filler and solvent can be mixed together to prepare a separator composition. Then, the separator composition can be directly coated on the electrode and then dried to form a separator. In some embodiments, the separator composition can be cast on a support and then dried to form a separator film, which can then be separated from the support and laminated on the electrode to form a separator.

[0116] The polymer used to make the separator may be any suitable polymer used as an electrode binder. Examples of polymer resins may include vinylidene fluoride / hexafluoropropylene copolymers, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, and mixtures thereof.

[0117] Next, an electrolyte is prepared.

[0118] The electrolyte may be, for example, an organic electrolyte solution. The organic electrolyte solution may be prepared, for example, by dissolving a lithium salt in an organic solvent.

[0119] The organic solvent can be any suitable organic solvent available in the art. For example, the organic solvent can be propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methylpropyl carbonate, ethylpropyl carbonate, isopropyl methyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, cyclopentane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether and combinations thereof.

[0120] The lithium salt may be any suitable lithium salt available in the art. For example, the lithium salt may be LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein, x and y are natural numbers), LiCl, LiI or a mixture thereof.

[0121] In some embodiments, the electrolyte may be a solid electrolyte. The solid electrolyte may be, for example, boron oxide or lithium oxynitride, but is not limited thereto. The solid electrolyte may be any suitable solid electrolyte available in the art. The solid electrolyte may be, for example, an oxide solid electrolyte or a sulfide solid electrolyte. The solid electrolyte may be formed on the negative electrode by a method such as sputtering, or a separate solid electrolyte sheet may be stacked on the negative electrode.

[0122] like Figure 1As shown in FIG. 1 , the lithium battery 1 includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, the negative electrode 2, and the separator 4 may be wound or folded to be accommodated in a battery case 5. Then, the battery case 5 is filled with an organic electrolyte solution and sealed with a cap assembly 6, thereby completing the manufacture of the lithium battery 1. The battery case 5 may be cylindrical, but the battery case 5 is not necessarily limited thereto, and for example, the battery case 5 may be square in shape, a film type, or the like.

[0123] The pouch-type lithium battery may include at least one battery structure. The separator may be between the positive electrode and the negative electrode to provide a battery assembly. After the battery structure is stacked into a dual-battery structure, the battery structure may be impregnated with an organic electrolyte solution and contained and sealed in a bag to provide a pouch-type lithium battery. In some embodiments, although not shown in the drawings, the positive electrode, the negative electrode, and the separator may be wound into an electrode assembly or folded in the form of a jelly roll and then contained in a bag. The organic electrolyte solution may then be injected into the bag and sealed to provide a pouch-type lithium battery.

[0124] Since lithium batteries may have excellent life characteristics and rate performance, lithium batteries may be used, for example, in electric vehicles (EVs) (e.g., hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs)). Lithium batteries may be suitable for use in high-power storage fields. For example, lithium batteries may be used in electric bicycles or electric tools.

[0125] A plurality of lithium batteries may be stacked to form a battery module, and a plurality of battery modules may form a battery pack. The battery pack may be used in devices requiring large capacity and high power, for example, in laptop computers, smart phones, or electric vehicles.

[0126] A battery module may include, for example, a plurality of batteries and a frame for holding the plurality of batteries. A battery pack may include, for example, a plurality of battery modules and a bus bar for connecting the battery modules. A battery module and / or a battery pack may further include a cooling device.

[0127] Multiple battery packs can be controlled by a battery management system. The battery management system can include battery packs and a battery controller connected to the battery packs.

[0128] According to an embodiment, a method for manufacturing a positive electrode may include: providing a composite positive electrode active material; preparing a positive electrode active material composition including the composite positive electrode active material and a binder; and preparing a positive electrode by providing the positive electrode active material composition or its dry matter on a positive electrode collector, wherein the positive electrode active material composition may not include a carbonaceous conductive agent.

[0129] First, a composite positive electrode active material can be provided.

[0130] Providing a composite cathode active material may include: providing a lithium transition metal oxide; providing a first composite; and mechanically grinding the lithium transition metal oxide and the first composite, wherein the first composite may include: at least one first metal oxide represented by the formula M a O b (where 0 < a ≤ 3 and 0 < b < 4, provided that a is 1, 2, or 3 and b may not be an integer); and a carbonaceous material, and the at least one first metal oxide may be disposed in a carbonaceous material matrix, and M may be at least a metal selected from Groups 2 to 13 and Groups 15 and 16 of the periodic table. The carbonaceous material may be graphene.

[0131] Then, a lithium transition metal oxide may be provided. The lithium transition metal oxide may be, for example, a compound represented by one of Formulas 1 to 3.

[0132] Providing the first composite may include, for example, providing a reaction gas including a carbon source gas to a structure including a metal oxide and performing a heat treatment.

[0133] Providing the first composite may include, for example, providing at least one second metal oxide represented by M a O c (where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2, or 3 and c may be an integer) and a reaction gas including a carbon source gas and performing a heat treatment, and M may be at least a metal selected from Groups 2 to 13 and Groups 15 and 16 of the periodic table.

[0134] The carbon source gas may be a compound represented by Formula 6 or at least one mixed gas selected from a compound represented by Formula 6, a compound represented by Formula 7, and an oxygen-containing gas represented by Formula 8:

[0135] Formula 6

[0136] C n H (2n+2-a) [OH] a

[0137] wherein, in Formula 6, n may be 1 to 20 and a may be 0 or 1;

[0138] Formula 7

[0139] C n H 2n

[0140] wherein, in Formula 7, n may be 2 to 6; and

[0141] Formula 8

[0142] C x Hy O z

[0143] Among them, in Formula 8, x can be 0 or an integer from 1 to 20, y can be 0 or an integer from 1 to 20, and z can be 1 or 2.

[0144] The compound represented by Formula 6 and the compound represented by Formula 7 can be at least one selected from the group consisting of methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by Formula 8 can include, for example, carbon dioxide (CO2) and carbon monoxide (CO), water vapor (H2O), or a mixture thereof.

[0145] After supplying a reaction gas including a carbon source gas to a second metal oxide represented by M a O c (where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2, or 3 and c can be an integer) and performing heat treatment, cooling by using at least one inert gas selected from the group consisting of nitrogen, helium, and argon can be further performed. Cooling can refer to adjusting the temperature to room temperature (20 °C to 25 °C). The carbon source gas can include at least one inert gas selected from the group consisting of nitrogen, helium, and argon.

[0146] In the method for preparing the first composite, the process of growing a carbonaceous material (e.g., graphene) by a gas-phase reaction can be performed under various conditions.

[0147] Under the first condition, for example, first, methane can be supplied to a reactor in which a second metal oxide represented by M a O c (where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2, or 3 and c can be an integer) is provided, and the temperature can be raised to the heat treatment temperature (T). The time for heating until the heat treatment temperature (T) can be in the range of about 10 minutes to about 4 hours, and the heat treatment temperature (T) can be in the range of 700 °C to 1100 °C. Heat treatment can be performed at the heat treatment temperature (T) for a reaction time. The reaction time can be, for example, in the range of about 4 hours to about 8 hours. The heat-treated product can be cooled to prepare the first composite. The time taken to cool from the heat treatment temperature (T) to room temperature can be, for example, in the range of about 1 hour to about 5 hours.

[0148] Under the second condition, for example, first, hydrogen can be supplied to a reactor in which a second metal oxide represented by M a O cA reactor for a second metal oxide represented by (where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2, or 3 and c can be an integer), and the temperature can be raised to a heat treatment temperature (T). The time for heating up to the heat treatment temperature (T) can be in the range of about 10 minutes to about 4 hours, and the heat treatment temperature (T) can be in the range of 700 °C to 1100 °C. After heat-treating for a certain reaction time at the heat treatment temperature (T), methane gas can be supplied, and heat treatment can be further carried out during the remaining reaction time. The reaction time can be, for example, in the range of about 4 hours to about 8 hours. The heat-treated product can be cooled to prepare a first composite. During cooling, nitrogen gas can be supplied to it. The time taken to cool from the heat treatment temperature (T) to room temperature can be, for example, in the range of about 1 hour to about 5 hours.

[0149] Under the third condition, for example, first, hydrogen gas can be supplied to a reactor in which there is provided a second metal oxide represented by M a O c A reactor for a second metal oxide represented by (where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2, or 3 and c can be an integer), and the temperature can be raised to a heat treatment temperature (T). The time for heating up to the heat treatment temperature (T) can be in the range of about 10 minutes to about 4 hours, and the heat treatment temperature (T) can be in the range of 700 °C to 1100 °C. After heat-treating for a certain reaction time at the heat treatment temperature (T), a mixed gas of methane and hydrogen can be supplied, and heat treatment can be further carried out during the remaining reaction time. The reaction time can be, for example, in the range of about 4 hours to about 8 hours. The heat-treated product can be cooled to prepare a first composite. During cooling, nitrogen gas can be supplied to it. The time taken to cool from the heat treatment temperature (T) to room temperature can be, for example, in the range of about 1 hour to about 5 hours.

[0150] In the preparation of the first composite, when the carbon source gas contains water vapor, a first composite with excellent conductivity can be obtained. The content of water vapor in the gas mixture is not limited. For example, based on 100 volume% of the total carbon source gas, the content of water vapor in the gas mixture is in the range of about 0.01 volume% to about 10 volume%. The carbon source gas can be, for example: methane; a mixed gas containing methane and an inert gas; or a mixed gas containing methane and an oxygen-containing gas.

[0151] The carbon source gas can be, for example: methane; a mixed gas containing methane and carbon dioxide; or a mixed gas containing methane, carbon dioxide and water vapor. In the mixed gas of methane and carbon dioxide, the molar ratio of methane to carbon dioxide can be in the range of about 1:0.20 to about 1:0.50, about 1:0.25 to about 1:0.45 or about 1:0.30 to about 1:0.40. In the mixed gas of methane, carbon dioxide and water vapor, the molar ratio of methane to carbon dioxide to water vapor can be in the range of about 1:0.20 to about 0.50:0.01 to about 1.45, about 1:0.25 to about 0.45:0.10 to about 1.35 or about 1:0.30 to about 0.40:0.50 to about 1.0.

[0152] The carbon source gas can be, for example, carbon monoxide or carbon dioxide. The carbon source gas can be, for example, a mixed gas of methane and nitrogen. In the mixed gas of methane and nitrogen, the molar ratio of methane to nitrogen can be in the range of about 1:0.20 to about 1:0.50, about 1:0.25 to about 1:0.45 or about 1:0.30 to about 1:0.40. The carbon source gas may not include inert gases such as nitrogen.

[0153] The heat treatment pressure can be selected considering the heat treatment temperature, the composition of the gas mixture and the required amount of carbon coating. The heat treatment pressure can be controlled by adjusting the amount of the inflowing gas mixture and the amount of the outflowing gas mixture. The heat treatment pressure can be, for example, 0.5 atm or higher, 1 atm or higher, 2 atm or higher, 3 atm or higher, 4 atm or higher or 5 atm or higher.

[0154] The heat treatment time is not particularly limited and can be appropriately adjusted according to the heat treatment temperature, the pressure during heat treatment, the composition of the gas mixture and the required amount of carbon coating. For example, the reaction time at the heat treatment temperature can be, for example, about 10 minutes to about 100 hours, about 30 minutes to about 90 hours or about 50 minutes to about 40 hours. For example, as the heat treatment time increases, the amount of deposited carbon (e.g., graphene) can increase, thus improving the electrical properties of the first composite. However, this trend may not necessarily be proportional to the time. For example, after a predetermined time, carbon deposition (e.g., graphene deposition) may no longer occur, or the deposition rate may decrease.

[0155] Through the gas-phase reaction of the above carbon source gas, even at a relatively low temperature, by adding to M a O c (where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2 or 3 and c can be an integer) represents the second metal oxide and its reduction product (by M a Ob (where 0 < a ≤ 3 and 0 < b < 4, provided that a is 1, 2, or 3 and b may not be an integer) at least one of the first metal oxides represented) provides a uniform carbonaceous material coating (e.g., graphene coating) to obtain a first composite.

[0156] The first composite may include, for example: a carbonaceous material matrix (e.g., graphene matrix) having at least one structure selected from a spherical structure, a helical structure in which a plurality of spherical structures are connected, a cluster structure in which a plurality of spherical structures agglomerate, and a sponge structure; and M a O c (where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2, or 3 and c may be an integer) at least one of the second metal oxides represented and its reduction products (by M a O b (where 0 < a ≤ 3 and 0 < b < 4, provided that a is 1, 2, or 3 and b may not be an integer) at least one of the first metal oxides represented), in the carbonaceous material matrix.

[0157] Next, the lithium transition metal oxide and the first composite can be mechanically ground to form a composite cathode active material. During grinding, a Nobilta mixer or the like can be used. The number of rotations of the mixer during grinding can be, for example, 1000 rpm to 2500 rpm. When the grinding rate is less than 1000 rpm, the shear force applied to the lithium transition metal oxide and the first composite may be weak, so it is difficult to form a chemical bond between the lithium transition metal oxide and the first composite. When the grinding rate is too high, since the first composite may proceed in too short a time, it may be difficult for the first composite to uniformly coat the lithium transition metal oxide to form a uniform and continuous shell. The grinding time can be, for example, about 5 minutes to about 100 minutes, about 5 minutes to about 60 minutes, or about 5 minutes to about 30 minutes. When the grinding time is too short, it may be difficult to coat the first composite on the lithium transition metal oxide to form a uniform and continuous shell. When the grinding time is too long, the production efficiency may decrease. Based on the total weight of the lithium transition metal oxide and the first composite, the content of the first composite can be 3 wt% or less, 2.5 wt% or less, 2 wt% or less, or 1.5 wt% or less. For example, based on 100 parts by weight of the mixture of the lithium transition metal oxide and the first composite, the content of the first composite can be in the range of about 0.5 parts by weight to about 3 parts by weight, about 0.5 parts by weight to about 2.5 parts by weight, about 0.5 parts by weight to about 2 parts by weight, or about 0.5 parts by weight to about 1.5 parts by weight.

[0158] An average diameter (D50) of the first composite used in the mechanical milling of the lithium transition metal oxide and the first composite may be, for example, in the range of about 1 μm to about 20 μm, about 3 μm to about 15 μm, or about 5 μm to about 10 μm.

[0159] Next, a positive active material composition including a composite positive active material and a binder may be prepared, and the positive active material composition or a dry matter thereof may be provided on a positive current collector to prepare a positive electrode.

[0160] For example, the positive electrode can be manufactured by the following method, but the manufacturing is not necessarily limited to the following method and can be adjusted according to required conditions.

[0161] First, the composite positive active material, binder and solvent prepared above can be mixed to form a positive active material composition. The prepared positive active material composition can be directly coated on an aluminum current collector and dried to prepare a positive plate having a formed positive active material layer. Alternatively, the positive active material composition can be cast on a separate support, which can then be separated from the support and laminated on an aluminum current collector to prepare a positive plate having a formed positive active material layer. In addition to the composite positive active material, the positive active material composition may not include a separate carbonaceous conductive agent.

[0162] The positive electrode active material composition may or may not further include a metal-based conductive agent and / or a conductive polymer. Examples of metal-based conductive agents include metal powders, metal fibers or metal tubes of copper, nickel, aluminum or silver. Examples of conductive polymers may be polyphenylene derivatives, but embodiments are not limited thereto. Any suitable metal-based conductive agent and / or conductive polymer available in the art may be used.

[0163] Vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures thereof or styrene butadiene rubber polymers can be used as adhesives. N-methyl pyrrolidone (NMP), acetone or water can be used as solvents, but embodiments are not limited thereto. Any suitable adhesive and solvent available in the art can be used.

[0164] It is also possible to form pores inside the electrode plate by adding a plasticizer or a pore former to the positive electrode active material composition.

[0165] The amount of the composite positive active material, binder and solvent used in the positive electrode may be in the range commonly used in lithium batteries. Depending on the purpose and structure of the lithium battery, at least one of the binder and the solvent may be omitted. Based on the total weight of the positive active material layer, the content of the binder in the positive electrode may be in the range of about 0.1wt% to about 10wt% or about 0.1wt% to about 5wt%. Based on the total weight of the positive active material layer, the content of the positive active material in the positive electrode may be, for example, in the range of about 90wt% to about 99wt% or about 95wt% to about 99wt%.

[0166] In addition, in addition to the above-mentioned composite positive electrode active material, the positive electrode may also include other commonly used positive electrode active materials.

[0167] The commonly used positive electrode active material may be any suitable positive electrode active material available in the art, and may be, for example, a lithium-containing metal oxide. For example, at least one composite oxide of a metal selected from cobalt, manganese, nickel, and a combination thereof and lithium may also be used. Examples thereof include compounds represented by any of the following: Li a A 1-b B b D2 (where 0.9≤a≤1 and 0≤b≤0.5); Li a E 1-b B b O 2-c D c (where 0.90≤a≤1, 0≤b≤0.5, and 0≤c≤0.05); LiE 2- b B b O 4-c D c (where 0≤b≤0.5 and 0≤c≤0.05); Li a Ni 1-b-c Co b B c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b-c Co b B c O 2-α F α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Co b B c O 2-αF2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b- c Mn b B c O 2-α F α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni b E c G d O2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, and 0.001≤d≤0.1); Li a Ni b Co c Mn d G e O2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, and 0.001≤e≤0.1); Li a NeG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a CoG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a MnG b O2 (where 0.90≤a≤1 and 0.001≤b≤0.1); Li a Mn b O4 (where 0.90≤a≤1 and 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2);Li (3-f) Fe2(PO4)3(0≤f≤2); and LiFePO4:

[0168] In the above formula, A can be selected from nickel (Ni), cobalt (Co), manganese (Mn) and combinations thereof; B can be selected from aluminum (Al), Ni, Co, Mn, chromium (Cr), iron (Fe), magnesium (Mg), strontium (Sr), vanadium (V), rare earth elements and combinations thereof; D can be selected from oxygen (O), fluorine (F), sulfur (S), phosphorus (P) and combinations thereof; E can be selected from Co, Mn and combinations thereof; F can be selected from F, S, P and combinations thereof; G can be selected from Al, Cr, Mn, Fe, Mg, lanthanum (La), cerium (Ce), Sr, V and combinations thereof; Q can be selected from titanium (Ti), molybdenum (Mo), Mn and combinations thereof; I can be selected from Cr, V, Fe, scandium (Sc), yttrium (Y) and combinations thereof; and J can be selected from V, Cr, Mn, Co, Ni, copper (Cu) and combinations thereof.

[0169] Compounds added with a coating formed on one of these compounds can also be used, and mixtures of these compounds and compounds added with coatings can also be used. In one or more embodiments, the coating added on the surface of these compounds may include at least one compound of a coating element selected from the group consisting of an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, and a hydroxycarbonate of a coating element. In one or more embodiments, these compounds constituting the coating may be amorphous or crystalline. In one or more embodiments, the coating element included in the coating may be magnesium (Mg), aluminum (Al), cobalt (Co), potassium (K), sodium (Na), calcium (Ca), silicon (Si), titanium (Ti), vanadium (V), tin (Sn), germanium (Ge), gallium (Ga), boron (B), arsenic (As), zirconium (Zr), or a mixture thereof. The method for forming the coating can be selected within the range that does not affect the physical properties of the positive active material. The coating method may be, for example, a spraying method or an impregnation method. Because the method is easily understood by a person of ordinary skill in the art, a detailed description of the coating method is omitted herein.

[0170] Hereinafter, exemplary embodiments will be described in detail with reference to examples and comparative examples. These embodiments are provided for illustrative purposes only and are not intended to limit the scope of the inventive concept.

[0171] (Preparation of the First Composite)

[0172] Preparation Example 1: Al2O3@Gr first composite

[0173] Place Al2O3 particles (with an average diameter of approximately 20 nm) in a reactor. Supply CH4 to the reactor at approximately 300 sccm and 1 atm for approximately 30 minutes, and then raise the internal temperature in the reactor to 1000 °C.

[0174] Then, perform a heat treatment at this temperature for 7 hours. Then, adjust the internal temperature of the reactor to room temperature (20 °C to 25 °C) to obtain a first composite in which Al2O3 particles and their reduction product Al2O z (0 < z < 3) particles are embedded in graphene.

[0175] The content of alumina in the first composite is 60 wt%.

[0176] Comparative Preparation Example 1: SiO2@Gr first composite

[0177] Place SiO2 particles (with an average diameter of approximately 15 nm) in a reactor. Supply CH4 to the reactor at approximately 300 sccm and 1 atm for approximately 30 minutes, and then raise the internal temperature in the reactor to 1000 °C.

[0178] Then, perform a heat treatment at this temperature for 7 hours. Then, adjust the internal temperature of the reactor to room temperature (20 °C to 25 °C) to obtain a first composite in which SiO2 particles and their reduction product SiO y (0 < y < 2) particles are embedded in graphene.

[0179] (Preparation of composite cathode active material)

[0180] Manufacturing Example 1: 1.2 wt% of Al2O3@Gr first composite (0.72 wt% of alumina) coated on NCA91

[0181] By using a Nobilta mixer (Hosokawa, Japan), grind LiNi 0.91 Co 0.05 Al 0.04 O2 (hereinafter referred to as NCA91) and the first composite prepared in Preparation Example 1 for about 5 to 30 minutes to obtain a composite cathode active material.

[0182] The mixing weight ratio of NCA91 to the first composite prepared in Preparation Example 1 is 98.8:1.2.

[0183] Manufacturing Example 2: 0.8 wt% of Al2O3@Gr first composite (0.48 wt% of alumina) coated on NCA91

[0184] A composite positive active material was manufactured in the same manner as in Manufacturing Example 1, except that the mixing weight ratio of NCA91 to the first composite prepared in Manufacturing Example 1 was adjusted to 99.2:0.8.

[0185] Manufacturing Example 3: 1.0 wt% Al2O3@Gr first composite (alumina 0.6 wt%) coated NCA91

[0186] A composite positive active material was manufactured in the same manner as in Manufacturing Example 1, except that the mixing weight ratio of NCA91 to the first composite prepared in Manufacturing Example 1 was adjusted to 99.0:1.0.

[0187] Comparative manufacturing example 1: bare NCA91

[0188] NCA91 was used as the positive electrode active material.

[0189] Comparative manufacturing example 2: 0.4wt% Al2O3@Gr first composite (alumina 0.24wt%) coated NCA91

[0190] A composite positive active material was manufactured in the same manner as in Manufacturing Example 1, except that the mixing weight ratio of NCA91 to the first composite prepared in Manufacturing Example 1 was adjusted to 99.6:0.4.

[0191] (Manufacturing of lithium batteries (half-cells))

[0192] Example 1: 1.2wt% Al2O3@Gr first composite coated with NCA91 + 0wt% conductive agent

[0193] (Manufacturing of positive electrode)

[0194] A mixture of the composite positive active material, carbon conductive agent and polyvinylidene fluoride (PVdF) prepared in manufacturing example 1 with a weight ratio of 98:0:2 was mixed with N-methylpyrrolidone (NMP) in an agate mortar with a pestle to make a slurry. That is, a separate carbonaceous conductive agent is not used. The slurry rod is applied to an aluminum current collector having a thickness of 15 μm, then dried at room temperature, and dried again in a vacuum at a temperature of 120 ° C. Then, hot pressing and stamping are performed to complete the manufacture of a positive plate having a thickness of 55 μm.

[0195] (Manufacture of button batteries)

[0196] A button cell was fabricated by using the prepared positive plate, lithium metal as a counter electrode, a PTFE separator, and a solution in which 1.3 M LiPF6 was dissolved in ethylene carbonate (EC) + ethyl methyl carbonate (EMC) + dimethyl carbonate (DMC) (volume ratio of 3:4:3).

[0197] Example 2: 0.8wt% Al2O3@Gr first composite coated with NCA91 + 0wt% conductive agent

[0198] A button cell was manufactured in the same manner as in Example 1, except that the composite positive electrode active material prepared in Manufacturing Example 2 was used instead of the composite positive electrode active material prepared in Manufacturing Example 1.

[0199] Example 3: 1.0wt% Al2O3@Gr first composite coated with NCA91 + 0wt% conductive agent

[0200] A button cell was manufactured in the same manner as in Example 1, except that the composite positive electrode active material prepared in Manufacturing Example 3 was used instead of the composite positive electrode active material prepared in Manufacturing Example 1.

[0201] Comparative Example 1: Bare NCA91 + 2wt% conductive agent

[0202] (Manufacturing of positive electrode)

[0203] A mixture of the positive active material, carbon conductive agent (Denkablack, conductive acetylene black) and polyvinylidene fluoride (PVdF) prepared in comparative manufacturing example 1 with a weight ratio of 96:2:2 was mixed with N-methylpyrrolidone (NMP) in an agate mortar with a pestle to make a slurry. The slurry rod was coated on an aluminum current collector having a thickness of 15 μm, then dried at room temperature, and dried again in a vacuum at a temperature of 120 ° C. Then, hot pressing and stamping were performed to complete the manufacture of a positive plate having a thickness of 55 μm.

[0204] (Button battery manufacturing)

[0205] A button cell was manufactured in the same manner as in Example 1.

[0206] Comparative Example 2: Bare NCA91 + 0wt% conductive agent

[0207] A positive electrode and a button cell were manufactured in the same manner as in Example 1, except that the positive electrode active material prepared in Comparative Manufacturing Example 1 was used instead of the composite positive electrode active material prepared in Manufacturing Example 1.

[0208] Comparative Example 3: 0.4wt% Al2O3@Gr first composite (alumina 0.24wt%) coated with NCA91+0wt% conductive agent

[0209] A positive electrode and a button cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material prepared in Comparative Manufacturing Example 2 was used instead of the composite positive electrode active material prepared in Manufacturing Example 1.

[0210] Comparative Example 4: 1.2wt% Al2O3@Gr first composite coated with NCA91+2wt% conductive agent

[0211] The positive electrode and button cell were manufactured in the same manner as in Example 1, except that the composite positive electrode active material, carbon conductive agent (conductive acetylene black) and polyvinylidene fluoride (PVdF) prepared in Manufacturing Example 1 were mixed in a weight ratio of 96:2:2, and the content of the conductive agent was changed from 0wt% to 2wt%.

[0212] Evaluation Example 1: XPS Spectrum Evaluation

[0213] During the preparation of the first composite prepared in Preparation Example 1, the XPS spectrum was measured over time using Quantum 2000 (Physical Electronics). The XPS spectra of the C1s orbital and the Al 2p orbital were measured before each sample was heated, after 1 minute of heating, after 5 minutes of heating, after 30 minutes of heating, after 1 hour of heating, and after 4 hours of heating. In the initial stage of heating, only the peak of the Al 2p orbital was displayed, and the peak of the C1s orbital was not displayed. After 30 minutes, the peak of the C 1s orbital was clearly displayed, and the size of the peak of the Al 2p orbital was significantly reduced.

[0214] After 30 minutes, the peaks of the C 1s orbital due to C═C bonding and CC bonding due to graphene growth are clearly shown around 284.5 eV.

[0215] As the reaction time increases, the oxidation number of aluminum decreases and the peak position of the Al 2p orbital moves toward a lower binding energy (eV).

[0216] Therefore, it was confirmed that as the reaction proceeded, graphene grew on the Al2O3 particles and Al2O3 was generated as a reduction product of Al2O3. x (0 <x<3)。

[0217] The average contents of carbon and aluminum were measured by XPS analysis results of 10 regions of the first composite sample prepared in Preparation Example 1. For the measurement results, the deviation of the aluminum content in each region was calculated. The deviation of the aluminum content was expressed as a percentage of the average value, and this value is called uniformity. The percentage of the average value of the deviation of the aluminum content (i.e., the uniformity of the aluminum content) was 1%. Therefore, it was confirmed that aluminum oxide was uniformly distributed in the first composite prepared in Preparation Example 1.

[0218] Evaluation Example 2: Scanning Electron Microscopy (SEM), High-Resolution Transmission Electron Microscopy (HR-TEM), and SEM-Energy Dispersive X-ray Spectroscopy (EDAX) Analysis

[0219] SEM, HR-TEM, and EDX analyses were performed on the first composite prepared in Preparation Example 1, the composite cathode active material prepared in Manufacturing Example 1, and the bare NCA91 of Comparative Manufacturing Example 1. For the SEM-EDAX analysis, the FEI Titan 80-300 available from Philips was used.

[0220] It was found that the first composite prepared in Preparation Example 1 had a structure in which Al2O3 particles and their reduction product Al2O z (where 0 < z < 3) particles were embedded in graphene. It was confirmed that graphene layers were provided on the outer surfaces of at least one kind of particles selected from the Al2O3 particles and Al2O z (where 0 < z < 3) particles. The at least one kind of particles selected from the Al2O3 particles and Al2O z (where 0 < z < 3) particles were uniformly dispersed in the graphene matrix. The diameter of at least one of the Al2O3 particles and Al2O z (where 0 < z < 3) particles was about 20 nm. The diameter of the first composite prepared in Preparation Example 1 was in the range of about 100 nm to about 200 nm.

[0221] In the composite cathode active material prepared in Manufacturing Example 1, a shell formed of the first composite including graphene was provided on the NCA91 core.

[0222] SEM-EDAX analysis was performed on the bare NCA91 of Comparative Manufacturing Example 1 and the composite cathode active material prepared in Manufacturing Example 1.

[0223] Compared with the surface of the bare NCA91 cathode active material of Comparative Manufacturing Example 1, it was found that the concentration of aluminum (Al) distributed on the surface of the composite cathode active material of Manufacturing Example 1 was increased. Therefore, it was found that the first composite prepared in Preparation Example 1 was uniformly coated to form a shell on the NCA91 core of the composite cathode active material of Manufacturing Example 1.

[0224] Evaluation Example 3: SEM Analysis of the Cross-Section of the Cathode

[0225] SEM analysis was performed on the cross-sections of the cathodes of each of Example 1 and Comparative Example 4.

[0226] Figure 2 The cross-section of the cathode manufactured in Example 1 is shown.

[0227] Figure 3A cross section of the positive electrode manufactured in Comparative Example 4 is shown.

[0228] like Figure 2 As shown in , since the positive electrode of Example 1 does not include a conductive agent, voids exist between the composite positive electrode active material particles.

[0229] like Figure 3 As shown in , since the positive electrode of Comparative Example 1 includes the conductive agent, the conductive agent exists between the composite positive electrode active material particles.

[0230] Therefore, in the lithium battery including the cathode of Example 1 and the liquid electrolyte, the electrolyte solution may be present in the gaps between the composite cathode active material particles to improve ion conductivity.

[0231] In contrast, in the battery including the positive electrode and the liquid electrolyte of Comparative Example 4, the conductive agent is filled in the space between the composite positive electrode active material particles. Therefore, the content of the electrolyte solution in the space between the positive electrode active material particles may be reduced.

[0232] Therefore, the lithium battery including the positive electrode of Comparative Example 4 may have reduced ion conductivity, increased internal resistance of the lithium battery, and thus deteriorate the cycle characteristics of the lithium battery, compared to the lithium battery including the positive electrode of Example 1. In addition, as the thickness of the positive electrode increases, the difference in cycle characteristics due to the difference in ion conductivity may be more significant.

[0233] Evaluation Example 4: Evaluation of charge / discharge characteristics at room temperature

[0234] Each lithium battery manufactured in Examples 1 to 3 and Comparative Examples 1 to 4 was charged at a constant current of 0.1C rate at 25°C until a voltage of about 4.4V (relative to Li), and maintained at a constant voltage of 4.4V (constant voltage mode) until a cut-off current of 0.05C rate. Subsequently, the lithium battery was discharged at a constant current of 0.1C rate until the voltage reached 3.0V (relative to Li) (formation cycle).

[0235] Each lithium battery undergoing the formation cycle was charged at a constant current of 0.2C rate at 25°C until the voltage reached 4.25V (relative to Li), and a constant voltage of 4.25V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at a constant current of 0.2C rate until the voltage reached 3.0V (relative to Li) (1st cycle).

[0236] Each lithium battery undergoing the first cycle was charged at 1.0C constant current at 25°C until the voltage reached 4.25V (relative to Li), and a constant voltage of 4.25V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at 1.0C constant current until the voltage reached 3.0V (relative to Li) (2nd cycle). These cycles were repeated under the same conditions until the 50th cycle (50 cycles).

[0237] Some results of the charge / discharge test at room temperature are shown in Table 1. The capacity retention rate at the 50th cycle can be defined by Equation 1. The initial efficiency during the formation process can be defined by Equation 2.

[0238] Equation 1

[0239] Capacity retention rate (%) = (discharge capacity at the 50th cycle / discharge capacity at the 1st cycle) × 100%

[0240] Equation 2

[0241] Initial efficiency (%) = (discharge capacity during formation cycle / charge capacity during formation cycle) × 100%

[0242] Table 1

[0243] Capacity retention rate (%) Initial efficiency (%) Example 1 95.1 90.8 Example 2 93.4 90.5 Example 3 94.2 90.7 Comparative Example 1 92.9 91.1 Comparative Example 2 32.4 89.7 Comparison Example 3 12.7 90.1 Comparison Example 4 Not measured 90.7

[0244] As shown in Table 1, compared with the lithium batteries of Comparative Examples 1 to 3, it was found that the lithium batteries of Examples 1 to 3 had improved lifespan characteristics at room temperature.

[0245] Compared with the lithium batteries of Comparative Examples 2 and 3 that did not include a conductive agent, the lithium batteries of Examples 1 to 3 were found to have significantly improved lifespan characteristics at room temperature.

[0246] Furthermore, the lithium battery of Example 1 not including the conductive agent was found to have improved initial efficiency compared to the lithium battery of Comparative Example 4 including the conductive agent.

[0247] Evaluation Example 5: Evaluation of high voltage charge / discharge characteristics at high temperature

[0248] Each lithium battery manufactured in Examples 1 to 3 and Comparative Examples 1 to 4 was charged at a constant current of 0.1C rate at 45°C until a voltage of about 4.3V (relative to Li), and maintained at a constant voltage of 4.3V (constant voltage mode) until a cut-off current of 0.05C rate. Subsequently, the lithium battery was discharged at a constant current of 0.1C rate until the voltage reached 3.0V (relative to Li) (formation cycle).

[0249] Each lithium battery undergoing the formation cycle was charged at 45°C at a constant current rate of 0.2C until the voltage reached 4.3V (relative to Li), and a constant voltage of 4.3V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at a constant current rate of 0.2C until the voltage reached 3.0V (relative to Li) (1st cycle).

[0250] Each lithium battery undergoing the first cycle was charged at 1.0C constant current at 45°C until the voltage reached 4.3V (relative to Li), and a constant voltage of 4.3V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at 1.0C constant current until the voltage reached 3.0V (relative to Li) (2nd cycle). These cycles were repeated under the same conditions until the 100th cycle (100 cycles).

[0251] Some results of the charge / discharge test at high temperature are shown in Table 2. The capacity retention rate at the 100th cycle can be defined by Equation 3. The initial efficiency during the formation process can be defined by Equation 2.

[0252] Equation 3

[0253] Capacity retention rate (%) = (discharge capacity at the 100th cycle / discharge capacity at the 1st cycle) × 100%

[0254] Equation 2

[0255] Initial efficiency (%) = (discharge capacity during formation cycle / charge capacity during formation cycle) × 100%

[0256] Table 2

[0257] Capacity retention rate (%) Initial efficiency (%) Example 1 79.9 90.8 Example 2 76.9 90.7 Example 3 78.8 90.8 Comparative Example 1 76.3 91.1 Comparative Example 2 2.9 89.7 Comparison Example 3 1.5 90.1 Comparison Example 4 Not measured 90.4

[0258] As shown in Table 2, compared with the lithium batteries of Comparative Examples 1 to 3, it was found that the lithium batteries of Examples 1 to 3 had improved lifespan characteristics at high temperatures.

[0259] Compared with the lithium batteries of Comparative Examples 2 and 3 that do not include a carbonaceous conductive agent, the lithium batteries of Examples 1 to 3 were found to have significantly improved lifespan characteristics at high temperatures.

[0260] Furthermore, the lithium battery of Example 1 not including the conductive agent was found to have improved initial efficiency compared to the lithium battery of Comparative Example 4 including the conductive agent.

[0261] Evaluation Example 6: Rate Performance Characteristics

[0262] Each lithium battery manufactured in Examples 1 to 3 and Comparative Examples 1 to 3 was charged at a constant current of 0.1C rate at 25°C until a voltage of about 4.4V (relative to Li), and maintained at a constant voltage of 4.4V (constant voltage mode) until a cut-off current of 0.05C rate. Subsequently, the lithium battery was discharged at a constant current of 0.1C rate until the voltage reached 3.0V (relative to Li) (formation cycle).

[0263] Each lithium battery undergoing the formation cycle was charged at a constant current of 0.2C rate at 25°C until the voltage reached 4.4V (relative to Li), and a constant voltage of 4.4V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at a constant current of 0.2C rate until the voltage reached 3.0V (relative to Li) (1st cycle).

[0264] Each lithium battery undergoing the first cycle was charged at a constant current of 0.2C at 25°C until the voltage reached 4.4V (relative to Li), and a constant voltage of 4.4V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at a constant current of 0.5C until the voltage reached 3.0V (relative to Li) (second cycle).

[0265] Each lithium battery undergoing the second cycle was charged at a constant current of 0.2C at 25°C until the voltage reached 4.4V (relative to Li), and a constant voltage of 4.4V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at a constant current of 1.0C until the voltage reached 3.0V (relative to Li) (the third cycle).

[0266] Each lithium battery undergoing the third cycle was charged at a constant current of 0.2C at 25°C until the voltage reached 4.4V (relative to Li), and a constant voltage of 4.4V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at a constant current of 2.0C until the voltage reached 3.0V (relative to Li) (the fourth cycle).

[0267] Each lithium battery undergoing the 4th cycle was charged at a constant current of 0.2C rate at 25°C until the voltage reached 4.4V (relative to Li), and a constant voltage of 4.4V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at a constant current of 3.0C rate until the voltage reached 3.0V (relative to Li) (5th cycle).

[0268] Each lithium battery undergoing the 5th cycle was charged at a constant current of 0.2C rate at 25°C until the voltage reached 4.4V (relative to Li), and a constant voltage of 4.4V was maintained (constant voltage mode) until the cut-off current of 0.05C rate was reached. Subsequently, each lithium battery was discharged at a constant current of 4.0C rate until the voltage reached 3.0V (relative to Li) (6th cycle).

[0269] During all these charge / discharge cycles, the evaluation was suspended for 10 minutes after one charge / discharge cycle.

[0270] Some results of the charge / discharge test at room temperature are shown in Table 3. The rate capability can be defined by Eq.

[0271] Equation 4

[0272] Rate performance (%) = (discharge capacity at the nth cycle / discharge capacity at the first cycle) × 100%

[0273] Table 3

[0274]

[0275] As shown in Table 3, compared with the lithium batteries of Comparative Examples 1 to 3, the lithium batteries of Examples 1 to 3 were found to have improved rate performance.

[0276] Compared with the lithium battery of Comparative Example 1 including the conductive agent, the lithium battery of Example 1 was found to have improved rate performance.

[0277] Evaluation Example 7: Measurement of compacted density

[0278] The compaction density of each of the composite positive electrode active material alone and the mixture of the composite positive electrode active material and the conductive agent used in the manufacture of the positive electrodes of Examples 1 to 3 and Comparative Examples 1 to 4 was measured. The results are shown in Table 4.

[0279] 3.0 g of each of the composite positive electrode active material alone and the mixture of the composite positive electrode active material and the conductive agent was dried at a temperature of 80° C., and a pressure of 2.6 Torr was applied thereto for 30 seconds. Then, the compaction density was measured.

[0280] Table 4

[0281] <![CDATA[Compaction density (g / cm 3 )]]> Example 1 3.60 Example 2 3.58 Example 3 3.58 Comparative Example 1 3.47 Comparative Example 2 3.56 Comparison Example 3 3.59 Comparison Example 4 3.49

[0282] As shown in Table 4, it was found that the positive electrodes of Examples 1 to 3 not including a conductive agent had significantly improved compaction density compared to the positive electrodes of Comparative Examples 1 and 4 including a conductive agent.

[0283] Therefore, the lithium batteries of Examples 1 to 3 including the positive electrodes not including the conductive agent were found to have improved energy density compared to the lithium batteries of Comparative Examples 1 and 4 including the positive electrodes including the conductive agent.

[0284] It is clear from the foregoing description that since the positive electrode may include such a composite positive electrode active material: the composite positive electrode active material includes a shell containing a first metal oxide and a carbonaceous material, and in the positive electrode, the carbonaceous conductive agent may be present only in the shell, the lithium battery may have improved life characteristics at room temperature and high temperatures and improved energy density.

[0285] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for limiting purposes. The description of features or aspects within each embodiment should generally be considered applicable to other similar features or aspects in other embodiments. Although one or more embodiments have been described with reference to the accompanying drawings, it will be understood by those of ordinary skill in the art that various changes in form and detail may be made therein without departing from the spirit and scope of the disclosure as defined by the appended claims.

Claims

1. A positive electrode, the positive electrode comprising a positive electrode current collector and a positive electrode active material layer on the positive electrode current collector, in, The positive electrode active material layer comprises a composite positive electrode active material and a binder, The composite positive electrode active material comprises: a core comprising a lithium transition metal oxide; and a shell disposed on the surface of the core and conformal with the surface of the core, The shell includes: at least one first metal oxide represented by the formula M a O b where 0 < a ≤ 3 and 0 < b < 4, provided that a is 1, 2 or 3 and b is not an integer; at least one second metal oxide represented by the formula M a O c where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2 or 3 and c is an integer; and a carbonaceous material, The at least one first metal oxide is disposed in a carbonaceous material matrix, M is at least one selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se, The second metal oxide comprises the same metal as the metal of the first metal oxide, The ratio c / a of a to c in the second metal oxide is greater than the ratio b / a of a to b in the first metal oxide, The positive electrode active material layer further comprises a carbonaceous conductive agent, and the carbonaceous conductive agent is only present in the shell, and In the total content of the composite positive electrode active material, the content of the first metal oxide is 0.3 wt% or higher.

2. The positive electrode according to claim 1, wherein In the total content of the composite positive electrode active material, the content of the first metal oxide is in the range of 0.3 wt% to 1.8 wt%.

3. The positive electrode according to claim 1, wherein Void spaces are provided between the composite positive electrode active materials.

4. The positive electrode according to claim 1, wherein The first metal oxide is at least one selected from the following substances: Al2O z , where 0 < z < 3; NbO x , where 0 < x < 2.5; MgO x , where 0 < x < 1; Sc2O z , where 0 < z < 3; TiO y , where 0 < y < 2; ZrO y , where 0 < y < 2; V2O z , where 0 < z < 3; WO y , where 0 < y < 2; MnO y , where 0 < y < 2; Fe2O z , where 0 < z < 3; Co3O w , where 0 < w < 4; PdO x , where 0 < x < 1; CuO x , where 0 < x < 1; AgO x , where 0 < x < 1; ZnO x , where 0 < x < 1; Sb2O z , where 0 < z < 3; and SeO y , where 0 < y < 2.

5. The positive electrode according to claim 4, wherein The second metal oxide is selected from Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2.

6. The positive electrode according to claim 4, wherein The first metal oxide is a reduction product of the second metal oxide.

7. The positive electrode according to claim 1, wherein The thickness of the shell is in the range of 1 nm to 5 μm.

8. The positive electrode according to claim 1, the positive electrode further comprising a third metal coated on the core or a third metal oxide coated on the core, in, The shell is disposed on the third metal or the third metal oxide, and The third metal oxide is an oxide of the third metal, and the third metal is selected from Al, Zr, W, and Co.

9. The positive electrode according to claim 1, wherein The shell comprises a first composite, the first composite comprising the first metal oxide and the carbonaceous material.

10. The positive electrode according to claim 9, wherein The first composite further comprises a second metal oxide having a composition different from the composition of the first metal oxide.

11. The positive electrode according to claim 10, wherein The average diameter of at least one selected from the first metal oxide and the second metal oxide is in the range of 1 nm to 1 μm.

12. The positive electrode according to claim 9, wherein The carbonaceous material has a branched structure, and the first metal oxide is distributed in the branched structure, and The branched structure comprises a plurality of carbonaceous material particles in contact with each other.

13. The positive electrode according to claim 1, wherein The lithium transition metal oxide is represented by Formula 1: Formula 1 Li m Ni x Co y D z O 2-n A n Wherein, in Formula 1, 0.9 ≤ m ≤ 1.2, 0 ≤ n ≤ 0.2, 0.8 ≤ x ≤ 0.95, 0 ≤ y ≤ 0.2, 0 < z ≤ 0.2, and x + y + z = 1, D is manganese, niobium, vanadium, magnesium, gallium, silicon, tungsten, molybdenum, iron, chromium, copper, zinc, titanium, aluminum, boron, or a combination thereof, and A is F, S, Cl, Br or a combination thereof.

14. A lithium battery comprising the positive electrode according to any one of claims 1 to 13.

15. A method for manufacturing a positive electrode, the method comprising the following steps: Providing composite positive electrode active materials; preparing a positive electrode active material composition comprising a composite positive electrode active material and a binder; as well as The positive electrode is prepared by providing the positive electrode active material composition or a dry substance thereof on a positive electrode current collector, Wherein, the positive electrode active material composition does not include a carbonaceous conductive agent, The step of providing the composite positive electrode active material comprises the following steps: Providing lithium transition metal oxides; providing a first composite; and mechanically grinding the lithium transition metal oxide and the first composite, Among them, the first composite includes: at least one first metal oxide represented by the formula M a O b where 0 < a ≤ 3 and 0 < b < 4, provided that a is 1, 2 or 3 and b is not an integer; at least one second metal oxide represented by the formula M a O c where 0 < a ≤ 3 and 0 < c ≤ 4, provided that a is 1, 2 or 3 and c is an integer; and a carbonaceous material, and The at least one first metal oxide is disposed in a carbonaceous material matrix, M is at least one selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb and Se, The step of providing the first composite comprises the following steps: providing the second metal oxide and a reaction gas including a carbon source gas and performing a heat treatment, The second metal oxide includes the same metal as the metal of the first metal oxide, and A ratio of a to c in the second metal oxide, c / a, is greater than a ratio of a to b in the first metal oxide, b / a.

16. The method according to claim 15, wherein: The average diameter of the first complex is in the range of 1 μm to 20 μm, and the content of the first complex is 3 wt % or less in the total content of the lithium transition metal oxide and the first complex.

Citation Information

Patent Citations

  • Vibration control method of bidet

    KR1020210014324A

  • Positive electrode active material, preparation method of positive electrode active material, positive electrode sheet and lithium ion battery

    CN106299371A

  • Lithium secondary battery

    JP2002117832A

  • Composite cathode active material, lithium battery including the same, and preparation method thereof

    US20150037680A1