Thermal treatment method for battery waste and lithium recovery method

By adjusting the oxygen partial pressure and using specific ambient gases in the heat treatment furnace of lithium-ion secondary battery waste, the problem of insufficient lithium being converted into lithium carbonate was solved, the leaching rate and recovery rate of lithium were improved, and valuable metals were realized efficient recycling.

CN114845820BActive Publication Date: 2024-10-15JEX RESOURCE RECYCLING ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180006459.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-31
Filing Date
2021-03-30
Publication Date
2024-10-15
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

When thermally treating lithium-ion secondary battery waste, the lack of oxygen in a high-concentration nitrogen environment causes lithium to be insufficiently converted into lithium carbonate, reducing the recovery rate of lithium.

Method used

By adjusting the oxygen partial pressure in the heat treatment furnace, using ambient gas containing oxygen, nitrogen, carbon dioxide and water vapor, the oxygen partial pressure in the furnace is maintained in the range of 5×10-4atm to 4×10-2atm, and the heat treatment is performed. Lithium in lithium-ion battery waste is leached in weakly acidic or alkaline solutions.

Benefits of technology

Stably generate lithium carbonate, improve the leaching rate and recovery rate of lithium, avoid the problem of insufficient conversion of lithium, and improve the recovery efficiency of valuable metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114845820B_ABST
    Figure CN114845820B_ABST
Patent Text Reader

Abstract

The present invention is a method for heat treatment of battery waste, which is a method for heat treatment of battery waste containing lithium, wherein, in a heat treatment furnace equipped with the battery waste, an ambient gas containing oxygen and at least one selected from the group consisting of nitrogen, carbon dioxide and water vapor is made to flow to adjust the oxygen partial pressure in the furnace, and at the same time, the battery waste is heated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This specification discloses a technology related to a thermal treatment method of battery waste containing lithium and a lithium recovery method. Background Art

[0002] For example, hybrid vehicles, fuel cell vehicles, electric vehicles, and other vehicles are equipped with batteries that supply power to electric motors as driving sources. In order to make the batteries function effectively, as described in Patent Documents 1 to 5, a vehicle-mounted battery pack is generally used, which packages multiple electrical components such as batteries, an ECU that controls the batteries, a cooling device that cools the batteries, and various sensors that measure the battery status, and houses them inside a box.

[0003] The battery of the vehicle-mounted battery pack generally uses a secondary battery that can be charged and stored and used repeatedly, among which nickel-hydrogen batteries are generally used, but in recent years, lithium-ion secondary batteries using lithium transition metal composite oxides as positive electrodes have gradually been used. In particular, when the lithium-ion secondary battery contains valuable metals such as cobalt, and the vehicle-mounted battery pack is discarded after use, from the perspective of effective resource utilization, it is expected to easily recover the valuable metals that may be contained in such waste at a relatively low cost for reuse.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 4917307

[0007] Patent Document 2: U.S. Patent Application Publication No. 2007 / 0141454

[0008] Patent Document 3: Japanese Patent No. 4955995

[0009] Patent Document 4: Japanese Patent No. 5464357

[0010] Patent Document 5: Japanese Patent Application Publication No. 2006-179190 Summary of the invention

[0011] Problem that the invention aims to solve

[0012] In addition, when recovering lithium from battery waste such as vehicle-mounted battery pack waste containing lithium as a positive electrode, it is considered that the battery waste is heated in a heat treatment furnace for heat treatment, and then the lithium in the battery powder obtained by crushing and screening is leached into water.

[0013] Here, by heat treatment, lithium in lithium compounds such as lithium composite oxides that may be contained in battery waste can be converted into the form of lithium carbonate that is easily leached into water.

[0014] However, if it is assumed that a high-concentration nitrogen environment is set in the heat treatment furnace, and the battery waste is heat-treated in the absence of oxygen in the heat treatment furnace, the oxygen required for generating lithium carbonate is sometimes insufficient, and the lithium in the battery waste is not fully converted into lithium carbonate. In this case, when leaching is performed using water, the lithium leaching rate is reduced, thereby causing the recovery rate of lithium to also be reduced.

[0015] The present specification discloses a thermal treatment method for battery waste and a lithium recovery method capable of stably generating lithium carbonate.

[0016] Solutions to Solve Problems

[0017] The method for heat treatment of battery waste disclosed in this specification is a method for heat treatment of battery waste containing lithium, wherein, in a heat treatment furnace equipped with the battery waste, an ambient gas containing oxygen and at least one selected from the group consisting of nitrogen, carbon dioxide and water vapor is caused to flow to adjust the oxygen partial pressure in the furnace, and at the same time, the battery waste is heated.

[0018] In addition, the lithium recovery method disclosed in this specification is a method for recovering lithium from battery waste containing lithium, wherein the lithium recovery method includes: a heat treatment step, heat treating the battery waste by any of the above-mentioned battery waste heat treatment methods; and a lithium leaching step, leaching lithium in the battery powder obtained from the battery waste after the heat treatment step in any of a weak acid solution, water and an alkaline solution.

[0019] Effects of the Invention

[0020] According to the above-mentioned heat treatment method for battery waste, lithium carbonate can be stably generated. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The flowchart shows an example of a lithium recovery method including a heat treatment step performed by a battery waste heat treatment method according to an embodiment.

[0022] Figure 2 This is a graph showing the change over time in temperature when waste vehicle-mounted battery packs are heat-treated in Examples. DETAILED DESCRIPTION

[0023] Hereinafter, embodiments of the thermal treatment method for battery waste and the lithium recovery method will be described in detail.

[0024] In a method for heat treatment of battery waste according to one embodiment, a heat treatment step is performed in which an ambient gas containing oxygen and at least one selected from the group consisting of nitrogen, carbon dioxide and water vapor is flowed in a heat treatment furnace in which the battery waste is placed to adjust the oxygen partial pressure in the furnace and heat the battery waste at the same time. Here, as the battery waste, it is preferred to use a battery pack waste containing lithium and having a box body constituting an outer package and batteries surrounded by the box body.

[0025] After the heat treatment step, as Figure 1 As shown in the example, a lithium leaching step can be performed as needed, in which lithium in battery powder obtained by crushing and screening the waste vehicle battery packs as the battery waste after heat treatment is leached in water. In this way, lithium contained in the waste vehicle battery packs can be recovered.

[0026] (Battery waste)

[0027] As battery waste, battery waste for vehicle use or for people's livelihood use can be taken as the object. In this embodiment, the battery waste is, for example, waste of vehicle-mounted battery packs installed in vehicles such as hybrid vehicles, fuel cell vehicles, and electric vehicles. More specifically, it is waste of vehicle-mounted battery packs that are discarded due to vehicle scrapping, replacement of vehicle-mounted battery packs, manufacturing defects, or other reasons. By taking such waste of vehicle-mounted battery packs as the object, effective utilization of resources can be achieved. However, waste batteries used in electronic equipment or devices can also be taken as the object.

[0028] A vehicle-mounted battery pack generally includes a metal box body that forms a shell around it, and batteries and other components that are stored inside the box body and have multiple battery cells. The components inside the box body include a control device such as an ECU that controls the battery, a cooling device that circulates cooling air inside the box body to suppress the increase in battery temperature during discharge or charging of the battery, various sensors that measure temperature to observe the battery status, and other necessary electrical components.

[0029] In-vehicle battery packs have various shapes depending on the space restrictions of the vehicle on which they are mounted, such as a substantially rectangular parallelepiped shape in a plan view having a longitudinally long shape in one direction.

[0030] As the battery housed in the vehicle-mounted battery pack, a nickel-cadmium secondary battery, a nickel-hydrogen secondary battery, a lithium ion secondary battery, or the like that can be charged and used repeatedly is used.

[0031] Among them, lithium ion secondary batteries usually contain a positive electrode active material composed of one or more single metal oxides or two or more composite metal oxides of lithium, nickel, cobalt and manganese, such as a positive electrode formed by coating and fixing on an aluminum foil (positive electrode substrate) with an organic binder such as polyvinylidene fluoride (PVDF), a negative electrode composed of a carbon material, and an electrolyte such as an organic electrolyte such as ethylene carbonate or diethyl carbonate. Since valuable metals such as cobalt are particularly contained as metals constituting the positive electrode, it is preferred to recycle these valuable metals from waste in terms of effective resource utilization.

[0032] (Heat treatment step)

[0033] The above-mentioned waste vehicle-mounted battery packs have a strong structure with the periphery protected by a metal box, etc., so it is not easy to dismantle them. In addition, when dismantling them, there is a risk of electric shock caused by residual voltage.

[0034] Therefore, in the heat treatment step, the waste vehicle battery pack is not disassembled, but the heat treatment step of heating the waste vehicle battery pack is performed while maintaining the structure of the battery and the like surrounded by the box body. This can reduce the time required for the disassembly work. In addition, even if the waste vehicle battery pack is not discharged by immersing it in a predetermined liquid, there is no possibility of electric shock during the heat treatment.

[0035] In particular, when the waste vehicle battery packs disposed in the heat treatment furnace are heat treated, an atmosphere containing oxygen and at least one selected from the group consisting of nitrogen, carbon dioxide and water vapor is flowed into the heat treatment furnace to adjust the oxygen partial pressure in the furnace. The inert gas containing a relatively small amount of oxygen is preferably mainly nitrogen in order to make the properties of the battery powder after the heat treatment uniform when the treatment scale is expanded.

[0036] By flowing an ambient gas mainly containing nitrogen, carbon dioxide and / or water vapor into the heat treatment furnace, the oxygen partial pressure in the furnace is maintained at a certain low level. As a result, the explosive combustion of the flammable organic electrolyte present in the box of the vehicle battery waste can be prevented, so the rupture of the vehicle battery waste can be prevented, and the vehicle battery waste can be controlled at a desired temperature. As a result, the melting of aluminum such as aluminum foil can be effectively prevented. In the case of aluminum melting, valuable metals such as cobalt and nickel may be mixed into the molten aluminum, and then separated and removed together with the solidified aluminum in the following screening step, but since this situation can be prevented here, the recovery rate of valuable metals can be improved.

[0037] In addition, if the temperature can be controlled while making the oxygen partial pressure in the furnace relatively low, the generation of powdered lithium aluminate caused by the reaction of aluminum and lithium oxide can be suppressed. Furthermore, compared with lithium carbonate, the solubility of lithium aluminate in water is lower, so the generation of lithium aluminate promoted at high temperature and high oxygen partial pressure will lead to a decrease in the leaching rate of lithium in the following lithium leaching step. Aluminum foil that has not reacted to lithium aluminate can be easily separated in the screening step. In the case of generating lithium aluminate, the aluminum foil becomes brittle and is easily mixed into the battery powder in the screening step of the later stage, so it is important to perform heat treatment under conditions that lithium aluminate is not generated as much as possible.

[0038] Furthermore, the low oxygen partial pressure in the furnace during heat treatment can suppress the formation of nickel oxide and cobalt oxide and promote the formation of metal cobalt and nickel that are more soluble in acid, thereby effectively suppressing a decrease in the recovery rate of valuable metals.

[0039] On the other hand, when the oxygen partial pressure in the furnace is extremely low, the generation of lithium carbonate under heat treatment cannot be promoted. If lithium carbonate that is easily leached into water cannot be fully generated, the lithium leaching rate in the lithium leaching step is reduced, and then the recovery rate of lithium is reduced. It is speculated that the generation of lithium carbonate under heat treatment is carried out by the reaction of carbon contained in the negative electrode of oxygen, lithium ion secondary battery, etc. and lithium. Oxygen may also be contained in the oxide of the positive electrode, but its amount is small, and it is difficult to say that it is enough to make a large amount of lithium in the vehicle-mounted battery pack waste become lithium carbonate. In contrast, in this embodiment, the oxygen partial pressure in the furnace is adjusted by making the ambient gas contain a relatively small amount of oxygen, and the generation of lithium carbonate can be promoted.

[0040] Specifically, it is preferred to maintain the oxygen partial pressure in the furnace at 5×10 -4 atm~4×10 -2 Atm. By maintaining the oxygen partial pressure in the furnace within this range, the recovery rate of valuable metals can be improved as described above, and the generation of lithium carbonate can be further promoted. In order to generate lithium carbonate, the oxygen partial pressure in the furnace during heating can be set to at least higher than 0atm.

[0041] Furthermore, when the oxygen partial pressure in the furnace during heating is set to 1×10 -2 Atm or less, the embrittlement of aluminum in the battery waste can be suppressed. If aluminum becomes embrittled during heat treatment, the separation of aluminum during the following sieving may be deteriorated.

[0042] Furthermore, the oxygen partial pressure in the furnace can be measured by a zirconia oxygen concentration meter. The above range of the oxygen partial pressure in the furnace means that the measured value of the oxygen partial pressure in the furnace measured at least during the period in which the oxygen partial pressure in the furnace can be measured is within the range. For example, when the organic electrolyte volatilizes, there is a situation where the oxygen partial pressure cannot be measured, but there is no particular limitation on the oxygen partial pressure in the furnace during such a period in which the oxygen partial pressure cannot be measured.

[0043] In addition, from the viewpoint of improving the recovery rate of valuable metals and promoting the production of lithium carbonate, when the inert gas is introduced into the heat treatment furnace, the oxygen concentration is preferably set to 0.05 volume % to 4.00 volume %.

[0044] Furthermore, the flow rate of the atmosphere gas in the heat treatment furnace is preferably set to 6 m 3 / hr~60m 3 / hr. If the flow rate of the inert gas is too high, the temperature distribution during the heat treatment may become larger, and the heat treatment may not be performed at the optimal temperature. On the other hand, if the flow rate of the inert gas is too low, there is a possibility that the oxygen partial pressure distribution during the heat treatment may become larger, and the heat treatment may not be performed at the optimal oxygen partial pressure. From this point of view, the flow rate of the ambient gas is preferably set to 6m / hr. 3 / hr~60m 3 / hr.

[0045] In the heat treatment furnace, when the inert gas is flowed and the oxygen partial pressure in the furnace is adjusted and the vehicle battery waste is heated at the same time, the maximum temperature reached by the vehicle battery waste is preferably set to 500°C to 650°C. When the maximum temperature reached by the vehicle battery waste is too low, there are concerns that the decomposition of the lithium metal oxide in the vehicle battery waste and the reduction of the nickel oxide and cobalt oxide obtained after the decomposition become insufficient; the formation of lithium carbonate is not promoted as expected; the removal of the organic electrolyte and the decomposition of polyvinylidene fluoride or polypropylene-polyethylene are not sufficiently carried out. On the other hand, when the maximum temperature reached by the vehicle battery waste is too high, it cannot be denied that aluminum may be melted and lithium aluminate may be formed.

[0046] For example, the heating rate until the above-mentioned maximum temperature is reached is preferably set to 50°C / hr to 150°C / hr. If the temperature rises too slowly, the heat treatment takes a lot of time, the treatment cannot proceed, and the equipment becomes larger. On the other hand, if the temperature rises too quickly, generally, the gasification of the electrolyte, PVDF, and the thermal decomposition gas of PE and PP used as separators will be generated all at once, which can be predicted to cause the rupture of the unit.

[0047] In addition, the time for maintaining the above-mentioned highest reached temperature is preferably set to 4 hours to 8 hours. The subsequent cooling can be natural cooling, but for example, by water cooling, or by using a water cooling jacket, making a large amount of inactive gas flow, etc., for forced cooling, there is an advantage that the equipment can be miniaturized.

[0048] In the heat treatment step as described above, as a heat treatment furnace, for example, if it is a batch type, an atmosphere type electric furnace or an atmosphere type muffle furnace can be used, or if it is a continuous type, a roller hearth kiln or a mesh belt kiln can be used. Among them, the roller hearth kiln is preferred in that it is suitable for large-scale treatment.

[0049] Furthermore, the combustible organic electrolyte evaporated and removed from the inside of the case of the waste vehicle battery pack is preferably introduced into a secondary combustion furnace, where it is burned by a burner or the like to be rendered harmless.

[0050] (crushing step; crushing and pulverizing step; screening step)

[0051] After the heat treatment step, a crushing step, a pulverizing step, a pulverizing step, and a subsequent screening step may be performed as necessary.

[0052] Crushing is to remove the battery from the box of the vehicle-mounted battery pack waste, destroy the shell of the battery, and selectively separate the positive electrode active material from the aluminum foil coated with the positive electrode active material. Here, various known devices or equipment can be used. As a specific example, an impact crusher that can cut the vehicle-mounted battery pack waste or battery and simultaneously apply impact to crush it can be listed, such as a sample mill, a hammer mill, a pin mill, a wing mill, a cyclone mill, a hammer crusher, etc. Furthermore, a screen can be set at the outlet of the crusher, so that if the battery is crushed to a size that can pass through the screen, it is discharged from the crusher through the screen.

[0053] After crushing, the crushed battery is slightly pulverized into powder, and then sieved using a sieve with an appropriate mesh. The separation of the positive electrode active material fixed on the aluminum foil from the aluminum foil is improved by crushing and pulverizing. As a result, aluminum, copper, etc., for example, remain on the sieve, and battery powder containing lithium, cobalt, nickel, etc., from which aluminum, copper, etc. have been removed to some extent, can be obtained under the sieve.

[0054] (Lithium Leaching Step)

[0055] The battery powder obtained after the heat treatment step and optionally the crushing and screening step is contacted with any one of a weak acid solution, water and an alkaline solution in the lithium dissolution step, so that the lithium contained in the battery powder is dissolved in the solution. The preferred pH value is 2 < pH value < 13, and more preferably 3 < pH value < 12.

[0056] In the above-mentioned heat treatment step, the lithium contained in the waste of vehicle-mounted battery packs has been fully converted into lithium carbonate. Therefore, in the lithium leaching step, the lithium carbonate contained in the battery powder can be easily leached into any one of a weak acid solution, water and an alkaline solution. On the other hand, other metals that may be contained in the battery powder are almost insoluble in a weak acid solution, and even less soluble in water or an alkaline solution. Therefore, in the lithium leaching step, the lithium contained in the battery powder can be effectively separated from other metals.

[0057] As the weak acid solution in contact with the battery powder, the type of acid is not particularly limited, but generally a sulfuric acid solution is used. As for the alkaline solution in contact with the battery powder, the type of alkali is also not particularly limited, and generally sodium hydroxide and calcium hydroxide are used. In the treatment of waste LIB, lithium hydroxide may also be used. In addition, as for the water in contact with the battery powder, specifically tap water, industrial water, distilled water, purified water, ion exchange water, pure water, ultrapure water, etc.

[0058] The pH of the lithium solution obtained after the lithium is dissolved becomes high due to the dissolution of lithium, but an acid such as sulfuric acid may be added to the water to adjust the pH of the lithium solution to 7 to 10. The acid may be added before, during, and / or after the lithium is dissolved. It is preferred that the pH of the lithium solution finally obtained be 7 to 10.

[0059] This is because, if the pH value of the lithium solution is less than 7, metals such as Co may be eluted, and if it exceeds 10, aluminum may be eluted.

[0060] As a method for contacting the battery powder with water, there are various methods such as spraying, immersion, and passing liquid. However, from the viewpoint of reaction efficiency, a method of immersing the battery powder in water and stirring is preferred.

[0061] The liquid temperature when the battery powder contacts water can be 10 to 60° C. The slurry concentration can be 50 to 150 g / L. The slurry concentration refers to the ratio of the dry weight (g) of the battery powder to the amount (L) of water in contact with the battery powder.

[0062] In the lithium dissolution step, the leaching rate of lithium into water is preferably 30% to 70%, and more preferably 45% to 55%.

[0063] The lithium concentration of the lithium solution is preferably 1.0 g / L to 3.0 g / L, and more preferably 1.5 g / L to 2.5 g / L. The lithium solution may contain 0 mg / L to 1000 mg / L of sodium and 0 mg / L to 500 mg / L of aluminum.

[0064] The lithium in the lithium solution can be recovered as lithium carbonate by subjecting the lithium solution obtained in the lithium leaching step to treatments such as solvent extraction, neutralization, and carbonation. Furthermore, the lithium carbonate thus obtained can be purified as needed to reduce impurity components.

[0065] The water-insoluble residue remaining in the battery powder can be taken out by solid-liquid separation and then subjected to acid leaching, neutralization, solvent extraction, and other treatments by known methods to recover various metals such as cobalt and nickel contained therein.

[0066] Example

[0067] Next, the above-mentioned heat treatment method for waste vehicle battery packs was experimentally implemented and its effect was confirmed, so it is described below. However, the purpose of the description here is only to illustrate and is not intended to be limiting.

[0068] Under the conditions shown in Table 1, waste battery packs for vehicles having a case and a lithium ion secondary battery as a battery were heated and heat treated. Here, the heat treatment was performed while an atmosphere mainly containing nitrogen and also containing oxygen was flowed into the heat treatment furnace. In Examples 1 to 3, only the oxygen concentration and oxygen partial pressure in the furnace were substantially changed. The conditions are shown in Table 1.

[0069] Table 1

[0070]

[0071] The electrolyte in the lithium ion secondary batteries of any of Examples 1 to 3 did not enter an uncontrollable combustion state during the heat treatment, but was evaporated and removed to be harmless.

[0072] Then, the battery powder obtained by crushing, pulverizing / powdering and screening was brought into contact with water, and lithium leaching was performed in two stages at a slurry concentration of 50 g / L to 90 g / L. As a result, the lithium leaching rate of any of Examples 1 to 3 was as high as about 50% to 60%. It can be inferred that in Examples 1 to 3, the lithium in the waste of vehicle-mounted battery packs has been fully converted into lithium carbonate through the above-mentioned heat treatment.

[0073] Furthermore, the residue from the lithium leaching is then subjected to acid leaching, neutralization and solvent extraction in sequence to collect cobalt and nickel. Since the cobalt and nickel in the lithium-ion secondary battery have been fully reduced from the oxides during the above-mentioned heat treatment, any of Examples 1 to 3 has a relatively high collection rate of cobalt and nickel. However, in Example 3, since the oxygen partial pressure in the furnace during the heat treatment is slightly high, the aluminum in the lithium-ion battery becomes brittle, resulting in a slight deterioration in the separation of aluminum during screening, which needs to be removed, but the Co and Ni collection rates are only slightly reduced. Therefore, in Table 1, the improvement in the Co and Ni collection rates of Example 3 is recorded as "○", and the more preferred oxygen concentration is 0.1% to 1.0%.

Claims

1. A method for heat treatment of battery waste, which is a method for heat treatment of battery waste containing lithium, wherein: In a heat treatment furnace in which the battery waste is disposed, an atmosphere gas containing oxygen and at least one selected from the group consisting of nitrogen, carbon dioxide and water vapor is flowed to adjust the oxygen partial pressure in the furnace, and at the same time, the battery waste is heated at a maximum temperature of 650° C. or less, The oxygen partial pressure in the furnace during heating was maintained at a level higher than 0 atm and 4 × 10 -2 Below atm.

2. The method for thermal treatment of battery waste according to claim 1, wherein: The oxygen partial pressure in the furnace during heating was maintained at 5×10 -4 atm~4×10 -2 within the range of atm.

3. The method for thermal treatment of battery waste according to claim 1 or 2, wherein: The oxygen concentration of the atmosphere when introduced into the heat treatment furnace is set to 0.05 volume % to 4.00 volume %.

4. The method for thermal treatment of battery waste according to claim 1 or 2, wherein: The oxygen concentration of the atmosphere when introduced into the heat treatment furnace is set to 0.1 volume % to 1.0 volume %.

5. The method for thermal treatment of battery waste according to claim 1 or 2, wherein: The maximum temperature reached by the battery waste during heating is set to 500°C to 650°C.

6. The method for thermal treatment of battery waste according to claim 1 or 2, wherein: The battery waste is vehicle-mounted battery pack waste including a case body constituting an outer package and batteries surrounded by the case body.

7. A lithium recovery method, which is a method for recovering lithium from battery waste containing lithium, wherein: The lithium recovery method comprises: a heat treatment step of heat-treating the battery waste by the heat treatment method for battery waste according to any one of claims 1 to 6; and The lithium leaching step is to leach lithium in the battery powder obtained from the battery waste after the heat treatment step in any one of a weak acid solution, water and an alkaline solution.