Resin composition and resin sheet

By using maleimide resin and silane coupling agent in the resin composition and adding an adhesion imparting agent, the problem of low peel strength of the resin composition at low thermal curing temperature is solved, and high heat resistance and High adhesion, sealing material suitable for high temperature applications.

CN114846053BActive Publication Date: 2024-11-12LINTEC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080086301.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-13
Filing Date
2020-12-10
Publication Date
2024-11-12
Estimated Expiration
2040-12-10

AI Technical Summary

Technical Problem

The conventional resin composition has low peel strength after thermal curing, and is difficult to meet the requirements of heat resistance and adhesiveness, especially under low thermal curing temperature conditions.

Method used

A resin composition containing a maleimide resin and a silane coupling agent is used, and an adhesion imparting agent is added to the resin sheet to optimize the component ratio of the resin sheet to improve the peel strength after heat curing.

Benefits of technology

The peel strength after thermal curing of the resin composition is significantly improved and is suitable for high temperature-resistant sealing materials, especially in the applications of power semiconductor components and semiconductor components such as silicon carbide and gallium nitride.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003690475310000031
    Figure BDA0003690475310000031
  • Figure BDA0003690475310000041
    Figure BDA0003690475310000041
  • Figure BDA0003690475310000042
    Figure BDA0003690475310000042
Patent Text Reader

Abstract

The resin composition of the present invention contains (A) a thermosetting component and (B) a silane coupling agent, wherein the thermosetting component (A) contains (A1) a maleimide resin, and the silane coupling agent (B) is a compound represented by the following general formula (B1). 21 O) a (R 22 ) 3‑a Si‑L 21 ‑NH‑L 22 ‑NH‑R 23 ···(B1) (In the above general formula (B1), R 21 is an alkyl group, R 22 and R 23 are independently monovalent organic groups, L 21 and L 22 are independently divalent organic groups, and a is 1, 2 or 3. )
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition and a resin sheet. Background Art

[0002] As a sealing material for a power semiconductor element or the like, a resin composition having high heat resistance is used.

[0003] For example, Patent Document 1 discloses a resin composition containing a maleimide compound, a compound having at least one of an allyl group and an epoxy group, an amine compound, and a radical generator containing at least one of an acetophenone derivative and a tetraphenylethane derivative.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-147849 Summary of the invention

[0007] Problems to be solved by the invention

[0008] However, the resin composition described in Patent Document 1 has a problem in that the peel strength after thermal curing decreases, particularly when the thermal curing temperature is low.

[0009] An object of the present invention is to provide a resin composition and a resin sheet which are excellent in heat resistance and can improve the peel strength after thermal curing.

[0010] Solutions to the problem

[0011] A resin composition according to one embodiment of the present invention is a resin composition comprising (A) a thermosetting component and (B) a silane coupling agent, wherein the thermosetting component (A) comprises (A1) a maleimide resin, and the silane coupling agent (B) is a compound represented by the following general formula (B1).

[0012] (R 21 O) a (R 22 ) 3-a Si-L 21 -NH-L 22 -NH-R 23 ···(B1)

[0013] (In the above general formula (B1), R 21 is an alkyl group, R 22 and R 23 are independently monovalent organic groups, L 21 and L 22 are independently divalent organic groups, and a is 1, 2 or 3. )

[0014] In the resin composition of one embodiment of the present invention, the content of the (B) silane coupling agent is preferably 0.01% by mass or more and 5% by mass or less based on the total amount of solid content of the resin composition.

[0015] The resin composition according to one embodiment of the present invention further contains (E) an adhesion-imparting agent, and the (E) adhesion-imparting agent is preferably a compound having a triazine skeleton.

[0016] The resin sheet of one embodiment of the present invention is formed from the resin composition of one embodiment of the present invention described above.

[0017] In the resin sheet according to one embodiment of the present invention, when the resin sheet and copper foil are bonded together and cured at a temperature of 180° C. for 2 hours, the peel strength after curing is 2.0 N / 10 mm or more.

[0018] In the resin sheet according to one embodiment of the present invention, when the resin sheet and copper foil are bonded and cured at a temperature of 180° C. for 2 hours, the peel strength after curing is preferably 6.0 N / 10 mm or more.

[0019] In the resin sheet of one embodiment of the present invention, the resin sheet is used to seal a power semiconductor element, or is used to be sandwiched between the power semiconductor element and other electronic components.

[0020] The resin sheet of one embodiment of the present invention is preferably used to seal a semiconductor element using at least one of silicon carbide and gallium nitride, or to be sandwiched between the semiconductor element using at least one of silicon carbide and gallium nitride and other electronic components.

[0021] According to one embodiment of the present invention, a resin composition and a resin sheet which are excellent in heat resistance and can improve the peel strength after thermal curing can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The schematic cross-sectional view of a laminated body according to one embodiment.

[0023] Explanation of symbols

[0024] 1 ... laminated body, 2 ... first release material, 3 ... resin sheet, 4 ... second release material. DETAILED DESCRIPTION

[0025] [Resin composition]

[0026] First, the resin composition according to the present embodiment will be described.

[0027] The resin composition of the present embodiment contains (A) a thermosetting component and (B) a silane coupling agent. The (A) thermosetting component of the present embodiment contains (A1) a maleimide resin.

[0028] ((A) Thermosetting component)

[0029] The (A) thermosetting component (hereinafter, sometimes referred to as "(A) component") has the property of forming a three-dimensional network when heated and firmly bonding the adherend. As described above, the (A) thermosetting component in the present embodiment contains the (A1) maleimide resin (hereinafter, sometimes referred to as "(A1) component").

[0030] (A1) Maleimide resin

[0031] The (A1) maleimide resin in the present embodiment is not particularly limited as long as it contains two or more maleimide groups in one molecule.

[0032] From the viewpoint of heat resistance, the maleimide resin (A1) in the present embodiment preferably includes a benzene ring, and more preferably includes a structure in which a maleimide group is linked to a benzene ring. In addition, the maleimide compound preferably includes a structure in which two or more maleimide groups are linked to a benzene ring.

[0033] The (A1) maleimide resin in the present embodiment is preferably a maleimide resin containing two or more maleimide groups and one or more biphenyl skeletons in one molecule (hereinafter, sometimes simply referred to as a "biphenyl maleimide resin").

[0034] From the viewpoint of heat resistance and adhesiveness, the (A1) maleimide resin in the present embodiment is preferably represented by the following general formula (1).

[0035] [Chemical formula 1]

[0036]

[0037] In the above general formula (1), k is an integer greater than or equal to 1, and the average value of k is preferably greater than or equal to 1 and less than or equal to 10, more preferably greater than or equal to 1 and less than or equal to 5, and further preferably greater than or equal to 1 and less than or equal to 3. m1 and m2 are each independently an integer greater than or equal to 1 and less than or equal to 6, preferably an integer greater than or equal to 1 and less than or equal to 3, and more preferably 1. n1 and n2 are each independently an integer greater than or equal to 0 and less than or equal to 4, preferably an integer greater than or equal to 0 and less than or equal to 2, and more preferably 0. R 1 and R 2 Each of the R groups is independently an alkyl group having 1 to 6 carbon atoms, preferably an alkyl group having 1 to 3 carbon atoms, and more preferably a methyl group. 1 Same or different, multiple R 2 Same as or different from each other.

[0038] Specific examples of the maleimide resin represented by the general formula (1) in the present embodiment include compounds represented by the following general formula (2) or the following general formula (3).

[0039] [Chemical formula 2]

[0040]

[0041] [Chemical formula 3]

[0042]

[0043] In the above general formulae (2) and (3), k is the same as k in the above general formula (1). In the above general formula (2), n1, n2, R 1 and R 2 With the above general formula (1) n1, n2, R 1 and R 2 same.

[0044] Examples of products of the maleimide resin represented by the general formula (3) include "MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd.

[0045] In addition, the maleimide resin (A1) in the present embodiment is preferably a maleimide resin containing two or more maleimide groups and two or more phenylene groups in one molecule. From the viewpoint of improving solubility in solvents and improving sheet formation, it is preferred that the phenylene group has a substituent. As the substituent, for example, alkyl groups such as methyl and ethyl, and alkylene groups can be cited.

[0046] Moreover, from the viewpoint of sheet forming properties, the (A1) maleimide resin in the present embodiment is preferably a maleimide resin having an ether bond between a maleimide group and a phenylene group.

[0047] The maleimide resin containing two or more maleimide groups and two or more phenylene groups in one molecule is represented by the following general formula (4), for example.

[0048] [Chemical formula 4]

[0049]

[0050] In the above general formula (4), R 3 ~R 6 are each independently a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, L 1 is an alkylene group having 1 to 3 carbon atoms, L 2 and L 3Each of them is independently an alkylene group having 1 to 2 carbon atoms or an arylene group having 6 to 10 carbon atoms, and p and q are independently 0 or 1. 1 , L 2 and L 3 The total number of carbon atoms in is 3 or less.

[0051] The maleimide resin represented by the general formula (4) in the present embodiment is specifically represented by the following general formula (5) or the following general formula (6), for example.

[0052] [Chemical formula 5]

[0053]

[0054] [Chemical formula 6]

[0055]

[0056] In the above general formulas (5) and (6), L 1 It is an alkylene group having 1 to 3 carbon atoms.

[0057] In the above general formula (5), R 3 ~R 6 Each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.

[0058] In addition, the maleimide resin (A1) in the present embodiment preferably has two or more maleimide groups in one molecule, and a bonding group connecting at least one pair of two maleimide groups has four or more methylene groups in the main chain, from the viewpoint of flexibility and heat resistance.

[0059] Among them, from the viewpoint of flexibility, the bonding group connecting two maleimide groups preferably has 6 or more methylene groups in the main chain, more preferably has 8 or more methylene groups in the main chain, and particularly preferably has 10 or more methylene groups in the main chain. In addition, it is more preferred that these methylene groups are connected to form an alkylene group having more than 4 carbon atoms. In the alkylene group, it is preferred that at least one -CH2- is optionally substituted by -CH2-O- or -O-CH2-.

[0060] In addition, from the viewpoint of flexibility, the bonding group connecting two maleimide groups preferably has more than one side chain. As the side chain, alkyl and alkoxy etc. can be enumerated. In addition, when there are more than two side chains, the side chains can be bonded to each other and form an alicyclic structure.

[0061] In addition, such (A1) maleimide resin is preferably a maleimide resin that is liquid at a temperature of 25°C.

[0062] From the viewpoint of flexibility and heat resistance, such a maleimide resin (A1) is preferably represented by the following general formula (7).

[0063] [Chemical formula 7]

[0064]

[0065] In the general formula (7), n is an integer of 0 or more, preferably an integer of 1 or more and 10 or less, and more preferably an integer of 1 or more and 5 or less. The average value of n is preferably 0.5 or more and 5 or less, and more preferably 1 or more and 2 or less.

[0066] L 4 and L 5 Each independently represents a substituted or unsubstituted alkylene group having 4 or more carbon atoms, in which at least one -CH2- is optionally substituted by -CH2-O- or -O-CH2-. From the viewpoint of flexibility, the carbon number of the alkylene group is preferably 6 or more, more preferably 8 or more, and particularly preferably 10 or more and 30 or less. In addition, when the hydrogen of the alkylene group is substituted, the substituent is an alkyl group having 1 or more and 10 or less carbon atoms, or an alkoxy group having 1 or more and 10 or less carbon atoms. In addition, these substituents are optionally bonded to each other to form an alicyclic structure.

[0067] X is independently a group not having a substituted or unsubstituted alkylene group having more than 4 carbon atoms (including at least one -CH2- group substituted with -CH2-O- or -O-CH2-), and is preferably a divalent group having a phthalimide group. It should be noted that the phthalimide group also includes a group derived from phthalimide. As X, specifically, for example, a group represented by the following structural formula (7-1) or the following general formula (7-2) can be cited.

[0068] [Chemical formula 8]

[0069]

[0070] In the above general formula (7-2), Y 1 and Y 2 Each is independently hydrogen, methyl or ethyl, preferably methyl.

[0071] Specific examples of the maleimide resin represented by the general formula (7) in the present embodiment include compounds represented by the following general formula (7-1-1) or the following general formula (7-2-1).

[0072] [Chemical formula 9]

[0073]

[0074] In the general formulae (7-1-1) and (7-2-1), n ​​is an integer of 1 to 5. The average value of n is 1 to 2.

[0075] Examples of products of the maleimide resin represented by the general formula (7-1-1) include "BMI-1500" manufactured by Designer Molecules, Inc. and "SLK1500" manufactured by Shin-Etsu Chemical Co., Ltd.

[0076] Examples of products of the maleimide resin represented by the general formula (7-2-1) include "BMI-1700" manufactured by Designer Molecules.

[0077] As the maleimide resin (A1) in the present embodiment, specifically, for example, from the viewpoint of obtaining a cured product having high sheet-forming properties and heat resistance, preferably, the maleimide resin represented by the above general formula (3), bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, N,N'-1,3-phenylene bismaleimide, 4-methyl-1,3-phenylene bismaleimide, polyphenylmethane maleimide, or 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane; from the viewpoint of sheet-forming properties, the maleimide resin represented by the above general formula (3) or bis(3-ethyl-5-methyl-4-maleimidephenyl)methane is more preferred; from the viewpoint of reducing the complex viscosity of the resin sheet of the present embodiment at a high temperature before curing, the maleimide resin represented by the above general formula (3) is further preferred.

[0078] In addition, as the (A1) maleimide resin in the present embodiment, specifically, for example, from the viewpoint of flexibility and heat resistance, the maleimide resin represented by the general formula (7) is further preferred. It should be noted that these maleimide resins can be used alone or in combination of two or more. In addition, the maleimide resin represented by the general formula (3) and the maleimide resin represented by the general formula (7) can also be used in combination.

[0079] In the present embodiment, the content of the (A1) component in the (A) component is preferably 60% by mass or more, more preferably 65% ​​by mass or more, and particularly preferably 70% by mass or more, based on the total amount of the solid content of the (A) component (i.e., when the amount of the non-volatile components of the (A) component other than the solvent is set to 100% by mass). By making the content of the (A1) component in the (A) component such a range, the heat resistance of the resin composition of the present embodiment after curing can be improved.

[0080] (A2) Allyl resin

[0081] The (A) thermosetting component contained in the resin composition of the present embodiment preferably further contains (A2) allyl resin. The (A2) allyl resin (hereinafter, sometimes referred to as "(A2) component") is preferably liquid at room temperature. When the (A) thermosetting component contains an allyl resin, it is easier to lower the reaction temperature of the resin sheet of the present embodiment and improve the peel strength of the resin sheet after curing.

[0082] In the present embodiment, the mass ratio (A1 / A2) of the maleimide resin of the component (A1) to the allyl resin (A2) is preferably 1.5 or more, and more preferably 3 or more.

[0083] When the mass ratio (A1 / A2) is within the above range, the storage modulus E' of the cured product of the resin sheet at 250°C tends to increase.

[0084] Moreover, when the mass ratio (A1 / A2) is in the above range, the heat resistance of the resin sheet can be improved.

[0085] In addition, when the mass ratio (A1 / A2) is within the above range, the complex viscosity η of the resin sheet is appropriately adjusted to ensure the fluidity of the resin sheet when applied to the adherend, and to achieve further improvement in the heat resistance of the resin sheet after curing. In addition, when the mass ratio (A1 / A2) is within the above range, the allyl resin can also be suppressed from seeping out of the resin sheet. It should be noted that the upper limit of the mass ratio (A1 / A2) is not particularly limited. For example, the mass ratio (A1 / A2) can be less than 50, preferably less than 10.

[0086] The allyl resin (A2) in the present embodiment is not particularly limited as long as it is a resin having an allyl group. The allyl resin (A2) in the present embodiment is preferably an allyl resin containing two or more allyl groups in one molecule, for example.

[0087] The allyl resin in the present embodiment is more preferably represented by the following general formula (8), the following general formula (9), or the following general formula (10).

[0088] [Chemical formula 10]

[0089]

[0090] [Chemical formula 11]

[0091]

[0092] [Chemical formula 12]

[0093]

[0094] In the above general formula (8), R 7 and R 8Each independently is an alkyl group, preferably an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and still more preferably an alkyl group selected from a methyl group and an ethyl group.

[0095] In the general formula (9), n3 is 1 to 4, preferably 1 to 3, and more preferably 1 to 2. In the allyl resin represented by the general formula (9), the ratio of the component where n3 is 1 is preferably 90 mol% or more.

[0096] As the allyl resin (A2) in the present embodiment, specific examples include diallyl bisphenol A (2,2-bis(3-allyl-4-hydroxyphenyl)propane), the allyl phenolic resin represented by the above general formula (9), and the allyl phenolic resin represented by the above general formula (10). These allyl resins can be used alone or in combination of two or more.

[0097] (A3) Curing catalyst

[0098] In the case where the resin composition contains a thermosetting resin, the resin sheet of the present embodiment preferably further contains a curing catalyst. Thus, the curing reaction of the thermosetting resin can be effectively carried out, and the resin sheet can be well cured. Examples of curing catalysts include imidazole curing catalysts, amine curing catalysts, and phosphorus curing catalysts.

[0099] Specific examples of imidazole curing catalysts include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1,2-dimethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and 2-phenyl-4,5-di(hydroxymethyl)imidazole. From the viewpoint of reactivity, 2-ethyl-4-methylimidazole is preferably used. It should be noted that when an imidazole compound having a triazine skeleton is used as the adhesion imparting agent (E) described later, it also acts as a curing catalyst.

[0100] Specific examples of the amine-based curing catalyst include tertiary amine compounds such as 1,8-diazabicyclo[5,4,0]undec-7ene (DBU), triethylenediamine, benzyldimethylamine, and triethanolamine.

[0101] Specific examples of the phosphorus-based curing catalyst include triphenylphosphine, tributylphosphine, tri(p-methylphenyl)phosphine, and tri(nonylphenyl)phosphine.

[0102] The (A) thermosetting component of this embodiment may further contain a thermosetting resin other than the (A1) component, a curing resin other than the (A2) component, and a curing catalyst other than the (A3) component, unless the purpose of the present invention is impaired.

[0103] Thermosetting resins other than the component (A1) may be any thermosetting resin as long as they have high heat resistance, and examples thereof include epoxy resins, benzophenone resins, Oxazine resin, cyanate resin, and melamine resin. These thermosetting resins can be used alone or in combination of two or more. Among them, from the viewpoint of high heat resistance, (A) thermosetting component preferably does not substantially contain epoxy resin.

[0104] Examples of curable resins other than component (A2) include phenolic resins, resins other than component (A2) having C=C double bonds, and resins containing acid anhydride and formaldehyde. These curable resins may be used alone or in combination of two or more.

[0105] Examples of the curing catalyst other than the component (A3) include triazole compounds, thiazole compounds, etc. These curing catalysts may be used alone or in combination of two or more.

[0106] When a thermosetting resin other than component (A1), a curing resin other than component (A2), and a curing catalyst other than component (A3) are used, their content is preferably 10% by mass or less, and more preferably 5% by mass or less, based on the total amount of the solid content of component (A) (i.e., when the amount of the non-volatile components of component (A) excluding the solvent is set to 100% by mass).

[0107] In the present embodiment, the content of the (A) thermosetting component in the resin composition is preferably 2% by mass or more and 75% by mass or less, more preferably 5% by mass or more and 60% by mass or less, and particularly preferably 10% by mass or more and 40% by mass or less, based on the total amount of the solid content of the resin composition (i.e., when the total amount of the non-volatile components of the resin composition other than the solvent is set to 100% by mass), The content of the (A) thermosetting component is within the above range, the handleability of the resin sheet, the sheet shape retention, and the heat resistance of the resin composition are improved.

[0108] ((B) Silane coupling agent)

[0109] The (B) silane coupling agent (hereinafter, sometimes referred to as "component (B)") is a compound represented by the following general formula (B1). The (B) component can improve the peel strength of the resin composition after curing. It is speculated that in the (B) component, -NH-L 22 -NH-R 23 The (B) component has a non-bonding interaction with metal ions on the metal surface or organic functional groups bonded to the metal surface, thereby improving the adhesion to the metal surface. In addition, the (B) component does not have a reactive functional group (vinyl group, epoxy group, mercapto group and isocyanate group) like a common silane coupling agent, so it can be inferred that the resin composition will not be adversely affected by the reaction with other components.

[0110] (R 21 O) a (R 22 ) 3-a Si-L 21 -NH-L 22 -NH-R 23 ···(B1)

[0111] In the above general formula (B1), R 21 It is an alkyl group, preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and further preferably a methyl group.

[0112] R 22 and R 23 are independently monovalent organic groups. 22 It is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and still more preferably a methyl group. 23 It is preferably an alkyl group, an aryl group, or a pyridyl group, and more preferably an alkyl group having 1 to 8 carbon atoms, a phenyl group, or a pyridyl group.

[0113] L 21 and L 22 are independently divalent organic groups. 21 It is preferably an alkylene group, more preferably an alkylene group having 1 to 6 carbon atoms, and still more preferably an alkylene group having 2 to 4 carbon atoms. 22 Preferably, it is a divalent organic group containing oxygen or sulfur, more preferably -C b H 2b -C(=O)-C b H 2b -or-C b H 2b -C(=S)-C b H2b Here, b is 0, 1, 2 or 3.

[0114] a is 1, 2 or 3, preferably 2 or 3, more preferably 3.

[0115] Specific examples of the compound represented by the general formula (B1) in the present embodiment include compounds represented by the following structural formula (B1-1) or the following structural formula (B1-2).

[0116] [Chemical formula 13]

[0117]

[0118] In the present embodiment, the content of the silane coupling agent (B) in the resin composition is preferably 0.01% by mass and 5% by mass based on the total amount of the solid content of the resin composition (i.e., when the total amount of the non-volatile components of the resin composition other than the solvent is set to 100% by mass), more preferably 0.05% by mass and 3% by mass, further preferably 0.1% by mass and 2% by mass, and particularly preferably 0.2% by mass and 1% by mass. By making the content of the silane coupling agent (B) in the resin composition within the above range, the peel strength of the resin composition after curing can be further improved.

[0119] ((C) Adhesive component)

[0120] In the present embodiment, the resin composition preferably includes a (C) binder component (hereinafter, sometimes referred to as "(C) component") in addition to the (A) component and the (B) component. By making the resin composition of the present embodiment further include the (C) binder component, film-forming properties can be imparted, and the resin composition can be easily formed into a sheet.

[0121] The (C) adhesive component of the present embodiment is a resin component other than the (A) component, and has the function of joining the (A) component or other components. The (C) adhesive component is preferably a thermoplastic resin. The (C) component may have a functional group as long as it has the function of joining the (A) component or other components. In the case where the (C) adhesive component has a functional group like this, even if the (C) adhesive component can participate in the curing of the resin sheet due to heat, in the present invention, the (C) adhesive component is distinguished from the (A) thermosetting component.

[0122] For (C) adhesive component, whether it is an aliphatic compound or an aromatic compound, it can be widely selected. (C) Adhesive component is preferably selected from at least one of phenoxy resin, acrylic resin, methacrylic resin, polyester resin, carbamate resin, and polyamide-imide resin, and from the viewpoint of heat resistance, it is more preferably selected from at least one of phenoxy resin and polyamide-imide resin. It should be noted that the polyester resin is preferably a wholly aromatic polyester resin. In addition, as a polyamide-imide resin, from the viewpoint of improving the flexibility of the resin sheet, a rubber-modified polyamide-imide resin is preferably used. (C) Adhesive component can be used alone or in combination of two or more.

[0123] The phenoxy resin is preferably a phenoxy resin having one or more skeletons selected from a bisphenol A skeleton (hereinafter, bisphenol A may be referred to as "BisA"), a bisphenol F skeleton (hereinafter, bisphenol F may be referred to as "BisF"), a biphenyl skeleton, and a naphthalene skeleton, and more preferably a phenoxy resin having a bisphenol A skeleton and a bisphenol F skeleton.

[0124] From the viewpoint of easily adjusting the complex viscosity of the resin sheet to a desired range, the weight average molecular weight (Mw) of the adhesive component (C) is preferably 10,000 to 1,000,000, more preferably 30,000 to 800,000, and further preferably 50,000 to 100,000. The weight average molecular weight in this specification is a value converted to standard polystyrene measured by gel permeation chromatography (GPC).

[0125] In the present embodiment, based on the total solid content of the resin composition (that is, when the total amount of the non-volatile components of the resin composition other than the solvent is set to 100% by mass), the content of the (C) adhesive component in the resin composition is preferably 1.5% by mass and 50% by mass, more preferably 2% by mass and 30% by mass, and particularly preferably 2% by mass and 15% by mass. By setting the content of the (C) adhesive component in the resin composition to the above-mentioned range, it is easy to adjust the complex viscosity of the resin sheet before curing to the desired range, and the handling and sheet formation of the resin sheet are improved.

[0126] ((D) Inorganic filler)

[0127] In this embodiment, the resin composition preferably contains (D) an inorganic filler (hereinafter sometimes simply referred to as "(D) component") in addition to the (A) to (C) components. The (D) component can improve at least one of the thermal properties and mechanical properties of the resin composition.

[0128] (D) The inorganic filler includes silica fillers, alumina fillers, boron nitride fillers, etc. Among them, silica fillers are preferred.

[0129] Examples of the silica filler include fused silica and spherical silica.

[0130] (D) The inorganic filler may be used alone or in combination of two or more. The inorganic filler (D) may be subjected to a surface treatment.

[0131] The average particle size of the inorganic filler (D) is not particularly limited. The average particle size of the inorganic filler (D) is preferably 0.1 nm or more and 100 μm or less, and more preferably 10 nm or more and 10 μm or less, as measured by a conventional particle size distribution meter. In this specification, the average particle size of the inorganic filler (D) is a value measured by a dynamic light scattering method using a particle size distribution measuring device (manufactured by Nikkiso Co., Ltd., product name "Nanotrac Wave-UT151").

[0132] Based on the total amount of the solid content of the resin composition (that is, when the total amount of the non-volatile components of the resin composition other than the solvent is set to 100% by mass), the content of the (D) inorganic filler in the resin composition is preferably 10% by mass or more and 90% by mass or less, more preferably 20% by mass or more and 85% by mass or less, further preferably 40% by mass or more and 80% by mass or less, particularly preferably 60% by mass or more and 80% by mass or less. By setting the content of the (D) inorganic filler in the resin composition to the above range, the linear expansion coefficient of the resin composition can be reduced, and the difference between the linear expansion coefficients of the sealed objects such as silicon carbide and the resin composition or the resin sheet can be reduced.

[0133] ((E) Adhesion Imparting Agent)

[0134] In the present embodiment, the resin composition preferably contains (E) an adhesion-imparting agent in addition to the (A) component to the (D) component.

[0135] Examples of the adhesion-imparting agent include compounds having a triazine skeleton, etc. As the compound having a triazine skeleton, an imidazole compound having a triazine skeleton is preferred.

[0136] Examples of the imidazole compound having a triazine skeleton include compounds represented by the following general formula (11).

[0137] [Chemical formula 14]

[0138]

[0139] In the above general formula (11), R 11 and R 12Each of them is independently a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a hydroxymethyl group or a phenyl group, preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. 13 It is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, a phenyl group, or an allyl group, preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms. 6 It is an alkylene group having 1 to 5 carbon atoms, preferably an alkylene group having 2 to 4 carbon atoms, and more preferably an ethylene group.

[0140] Specific examples of the imidazole compound having a triazine skeleton in the present embodiment include 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine, 2,4-diamino-6-[2-(2-ethyl-4-methyl-1-imidazolyl)ethyl]-1,3,5-triazine, and 2,4-diamino-6-[2-(2-undecyl-1-imidazolyl)ethyl]-1,3,5-triazine. Among these compounds, 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine or 2,4-diamino-6-[2-(2-ethyl-4-methyl-1-imidazolyl)ethyl]-1,3,5-triazine is preferred from the viewpoint of the peel strength of the resin composition and the resin sheet and the reaction temperature.

[0141] In the present embodiment, the content of the adhesion imparting agent (E) in the resin composition is preferably 0.01% by mass and 5% by mass, more preferably 0.03% by mass and 3% by mass, based on the total amount of the solids of the resin composition (i.e., when the total amount of the non-volatile components of the resin composition other than the solvent is set to 100% by mass). When the content of the adhesion imparting agent is within the above range, the peel strength of the resin composition after curing can be further improved.

[0142] As an example of the resin composition of the present embodiment, there can be listed: a resin composition containing only the (A) component, the (B) component and the (C) component, a resin composition containing only the (A) component, the (B) component, the (C) component and the (D) component, and a resin composition containing only the (A) component, the (B) component, the (C) component, the (D) component and the (E) component.

[0143] As another example of the resin composition of the present embodiment, there can be mentioned a resin composition containing components (A), (B), (C), (D), and (E), and components other than components (A) to (E), as described below.

[0144] (Other ingredients)

[0145] In this embodiment, the resin composition may further include other components. Examples of other components include at least any component selected from a crosslinking agent, a pigment, a dye, a defoamer, a leveling agent, a UV absorber, a foaming agent, an antioxidant, a flame retardant, an ion trapping agent, and an ion scavenger.

[0146] For example, the resin composition may further contain a crosslinking agent in order to adjust the initial adhesiveness and cohesiveness of the resin sheet before curing.

[0147] Examples of the crosslinking agent include organic polyisocyanate compounds and amino resins. The crosslinking agent may be used alone or in combination of two or more.

[0148] Examples of the organic polyisocyanate compound include aromatic polyisocyanate compounds, aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds, trimers of these polyisocyanate compounds, and isocyanate-terminated urethane prepolymers obtained by reacting these polyisocyanate compounds with a polyol compound.

[0149] More specific examples of the organic polyisocyanate compound include toluene-2,4-diisocyanate, toluene-2,6-diisocyanate, 1,3-phenylenediisocyanate, 1,4-xylene diisocyanate, diphenylmethane-4,4'-diisocyanate, diphenylmethane-2,4'-diisocyanate, 3-methyldiphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, and lysine isocyanate, etc. The organic polyisocyanate compound can be used alone or in combination of two or more.

[0150] As the amino resin, urea resin, melamine resin, guanamine resin, and co-condensed resins thereof can be used.

[0151] The crosslinking agent is usually blended in a ratio of 0.01 to 12 parts by mass, preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the (C) binder component.

[0152] In the present embodiment, when the resin sheet is formed by coating, the resin composition preferably contains a solvent. As the solvent, in addition to common solvents such as toluene, ethyl acetate, and methyl ethyl ketone, cyclohexanone (boiling point: 155.6°C), dimethylformamide (boiling point: 153°C), dimethyl sulfoxide (boiling point: 189.0°C), ethers of ethylene glycol (cellosolve) (boiling point: about 120 to 310°C), o-xylene (boiling point: 144.4°C) and other high boiling point solvents can also be listed.

[0153] [Resin sheet]

[0154] The resin sheet of the present embodiment is formed from the resin composition of the present embodiment described above. The resin sheet of the present embodiment can further improve flexibility while maintaining heat resistance.

[0155] The resin sheet is preferably formed only from the resin composition of the present embodiment from the viewpoint of the ability to follow the unevenness of the adherend when used for sealing the semiconductor element or when sandwiched between the semiconductor element and other electronic components. That is, the resin sheet is preferably not a composite material such as a material in which the resin composition and a fiber sheet are combined, such as a prepreg.

[0156] The resin sheet of the present embodiment has a peel strength after thermal curing of preferably 2.0 N / 10 mm or more, more preferably 3.0 N / 10 mm or more and 50 N / 10 mm or less, further preferably 4.0 N / 10 mm or more and 50 N / 10 mm or less, particularly preferably 6.0 N / 10 mm or more and 40 N / 10 mm or less.

[0157] When the resin sheet of the present embodiment has a peel strength of 2.0 N / 10 mm or more after thermal curing, the resin sheet can maintain high adhesiveness to an adherend when the resin sheet is used as a sealing material.

[0158] The peel strength of the resin sheet of the present embodiment after thermal curing can be adjusted to the above range by, for example, selecting the components used in the resin composition, preferably by adding at least one selected from an allyl resin and an adhesion-imparting agent to the resin composition and adjusting the type and amount thereof.

[0159] The peel strength of the resin sheet of the present embodiment after thermal curing is obtained by performing a peel test at a peel angle of 90 degrees between the thermally cured resin sheet and an adherend using a measuring method described below. Specifically, a test piece is prepared and the peel test is performed as follows.

[0160] (i) Method for preparing test piece

[0161] Adhesive: Copper foil (size 50mm×10mm, thickness 150μm, JIS H 3100 standard)

[0162] ·Laminating equipment: "V-130" manufactured by Nikko Materials

[0163] · Pressing conditions: Lamination temperature 130°C, maximum pressure 200Pa, time 40 seconds

[0164] Thermal curing conditions of the resin sheet: thermal curing temperature 180°C, thermal curing time 2 hours

[0165] (ii) Peel test method

[0166] · Equipment used: Tensile testing machine ("Autograph AG-100NXplus" manufactured by Shimadzu Corporation)

[0167] ·Peeling method: Peel the cured resin sheet off the adherend

[0168] Peeling speed: 50mm / min

[0169] Peeling angle: 90 degrees

[0170] ·Measurement environment: 23℃ 50% relative humidity

[0171] The resin sheet of the present embodiment is formed into a sheet from the resin composition, so that application to an adherend becomes easy, and particularly, lamination becomes easy when the adherend has a large area.

[0172] When the resin composition is in sheet form, it is preformed into a shape suitable for the shape after the sealing process, so it can be supplied as a sealing material that ensures a certain degree of uniformity only by application. In addition, when the resin composition is in sheet form, it has no fluidity and is therefore excellent in operability.

[0173] From the viewpoint of improving the heat resistance of the cured product of the resin sheet, the storage modulus E' of the resin sheet of the present embodiment at 250°C after thermal curing is preferably 150 MPa or more, more preferably 300 MPa or more, and further preferably 500 MPa or more. The storage modulus E' of the resin sheet at 250°C after thermal curing is a value obtained by measuring a test piece obtained by curing the resin sheet at 200°C for 4 hours.

[0174] The method of forming the resin composition into a sheet can adopt the existing known method of forming a sheet, which is not particularly limited. In the case of forming a resin sheet by the resin composition through the coating of the resin composition containing a solvent, the solvent can be completely volatilized in the drying process after coating, or a part of the solvent can be left in the resin sheet. The resin sheet of the present embodiment can be a strip-shaped sheet, or it can be provided in a state of being wound into a roll. The resin sheet of the present embodiment wound into a roll can be sent out from the roll and cut into a desired size, etc. for use.

[0175] The thickness of the resin sheet of the present embodiment is, for example, preferably 10 μm or more, more preferably 20 μm or more, and preferably 500 μm or less, more preferably 400 μm or less, and further preferably 300 μm or less.

[0176] The resin sheet of this embodiment is preferably used for a semiconductor element. Specifically, the resin sheet of this embodiment is preferably used for sealing a semiconductor element. In addition, the resin sheet of this embodiment is preferably used for being sandwiched between a semiconductor element and other electronic components.

[0177] The semiconductor element is preferably a power semiconductor element.

[0178] The resin sheet of the present embodiment has excellent heat resistance and can therefore be used to seal a power semiconductor element that is expected to operate at a high temperature of 200° C. or higher, or to be sandwiched between a power semiconductor element and other electronic components.

[0179] In addition, the resin sheet of this embodiment is preferably applied to multiple semiconductor elements at one time. For example, when the resin composition is in sheet form, it can be used for so-called panel-level packaging, which is to apply a resin sheet to a structure in which semiconductor elements are arranged in each gap of a frame having multiple gaps, and the frame and the semiconductor elements are sealed together.

[0180] In addition, the resin sheet of the present embodiment is preferably used to seal a semiconductor element using any one or more of silicon carbide and gallium nitride. Alternatively, the resin sheet of the present embodiment is preferably used to be sandwiched between a semiconductor element using any one or more of silicon carbide and gallium nitride and other electronic components. Examples of other electronic components include printed wiring boards and lead frames.

[0181] The upper limit of the operating temperature of a silicon semiconductor element is about 175° C., and therefore, a semiconductor element using one or more of silicon carbide and gallium nitride that can operate at high temperatures is preferably used as a power semiconductor element.

[0182] The resin sheet of this embodiment has excellent heat resistance and can therefore be used in semiconductor elements using any one or more of silicon carbide and gallium nitride that are intended to operate at high temperatures above 200°C, or can be used to be sandwiched between semiconductor elements using any one or more of silicon carbide and gallium nitride and other electronic components.

[0183] (Thermal curing conditions)

[0184] In the thermal curing conditions of the resin sheet of the present embodiment, the heating temperature is preferably 50° C. or higher and 300° C. or lower, and more preferably 100° C. or higher and 250° C. or lower.

[0185] In the thermal curing conditions of the resin sheet of the present embodiment, the heating time is preferably 10 minutes to 10 hours, and more preferably 20 minutes to 7 hours.

[0186] By setting the thermal curing conditions of the resin sheet to be within the above-mentioned range, thermal curing of the resin sheet can be achieved.

[0187] [Laminated body]

[0188] Figure 1 A schematic cross-sectional view of the laminated body 1 according to the present embodiment is shown.

[0189] The laminated body 1 of this embodiment has the 1st release material 2, the 2nd release material 4, and the resin sheet 3 provided between the 1st release material 2 and the 2nd release material 4. The resin sheet 3 is the resin sheet of this embodiment.

[0190] The first release material 2 and the second release material 4 preferably have release properties, and there is a difference between the release force of the first release material 2 with respect to the resin sheet 3 and the release force of the second release material 4 with respect to the resin sheet 3. The materials of the first release material 2 and the second release material 4 are not particularly limited. The ratio (P2 / P1) of the release force P2 of the second release material 4 to the release force P1 of the first release material 2 is preferably 0.02≤P2 / P1<1 or 1<P2 / P1≤50.

[0191] The first release material 2 and the second release material 4 are, for example, members that have release properties themselves, or members that have been subjected to a release treatment, or members that have a release agent layer laminated thereon, etc. When the first release material 2 and the second release material 4 are not subjected to a release treatment, the materials of the first release material 2 and the second release material 4 may include, for example, olefin resins, fluororesins, etc.

[0192] The first peeling material 2 and the second peeling material 4 can be made into a peeling material having a peeling substrate and a peeling agent layer formed on the peeling substrate. By making the peeling material having a peeling substrate and a peeling agent layer, the operation becomes easy. In addition, the first peeling material 2 and the second peeling material 4 can have a peeling agent layer only on one side of the peeling substrate, or can have a peeling agent layer on both sides of the peeling substrate. The formation of the peeling agent can be carried out by coating the peeling agent, for example.

[0193] Examples of the release substrate include paper substrates, laminated paper on which a thermoplastic resin such as polyethylene is laminated, and plastic films. Examples of the paper substrate include glassine paper, coated paper, and cast-coated paper. Examples of the plastic film include polyester films (e.g., polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate), and polyolefin films (e.g., polypropylene and polyethylene). Among them, polyester films are preferred.

[0194] Examples of the release agent include: silicone-based release agents composed of silicone resins; long-chain alkyl compound-containing release agents composed of compounds containing long-chain alkyl groups, such as polyvinyl carbamate and alkyl urea derivatives; alkyd resin-based release agents composed of alkyd resins (e.g., non-modified alkyd resins and modified alkyd resins); olefin resin-based release agents composed of olefin resins (e.g., polyethylene (e.g., high-density polyethylene, low-density polyethylene, and linear low-density polyethylene), propylene homopolymers having an isotactic structure or a syndiotactic structure, and crystalline polypropylene resins such as propylene-α-olefin copolymers); rubber-based release agents composed of rubbers such as natural rubber and synthetic rubber (e.g., butadiene rubber, isoprene rubber, styrene-butadiene rubber, methyl methacrylate-butadiene rubber, and acrylonitrile-butadiene rubber); and acrylic resin-based release agents composed of acrylic resins such as (meth)acrylate copolymers. These release agents may be used alone or in combination of two or more. Especially, when a phenoxy resin or a polyamide-imide resin is used as the (C) adhesive component of the resin composition contained in the resin sheet 3, when a conventional silicone-based release agent is used, there is a risk that the release material may be accidentally released before the resin sheet 3 is used, so it is preferred to use an alkyd resin-based release agent.

[0195] The thickness of the first release material 2 and the second release material 4 is not particularly limited, but is usually 1 μm or more and 500 μm or less, and preferably 3 μm or more and 100 μm or less.

[0196] The thickness of the release agent layer is not particularly limited. When the release agent layer is formed by applying a solution containing a release agent, the thickness of the release agent layer is preferably 0.01 μm to 3 μm, and more preferably 0.03 μm to 1 μm.

[0197] The manufacturing method of the laminate 1 is not particularly limited. For example, the laminate 1 can be manufactured through the following steps. First, a resin composition containing a solvent is applied to the first release material 2 to form a coating film. Next, the coating film is dried to form a resin sheet 3. Next, the laminate 1 is obtained by bonding the resin sheet 3 to the second release material 4 at room temperature. It should be noted that in this case, when the types of release materials of the first release material 2 and the second release material 4 are the same, there is a high possibility that the ratio of the release force P2 of the second release material 4 to the release force P1 of the first release material 2 (P2 / P1) is P2 / P1<1. Even if the release materials of the first release material 2 and the second release material 4 are different, since it is the first release material 2 that is coated with the resin composition, there is a tendency for the value of P2 / P1 to decrease.

[0198] [Effects of Embodiment]

[0199] According to the resin composition and the resin sheet of the present embodiment, it is possible to obtain a resin composition and a resin sheet that have heat resistance and can improve the peel strength after thermal curing.

[0200] As described above, the resin sheet of the present embodiment can be suitably used for a power semiconductor element. In other words, in the semiconductor device of the present embodiment, the semiconductor element is preferably a power semiconductor element. The power semiconductor element is assumed to operate at a high temperature of 200°C or above. Therefore, the material used in the semiconductor device having the power semiconductor element requires heat resistance. The resin sheet of the present embodiment has excellent heat resistance, and therefore, can be suitably used to cover the power semiconductor element in the semiconductor device, or to be sandwiched between the power semiconductor element and other components.

[0201] As described above, the resin sheet of the present embodiment can be suitably used for semiconductor elements using any one or more of silicon carbide and gallium nitride. In other words, in the semiconductor device of the present embodiment, the semiconductor element is preferably a semiconductor element using any one or more of silicon carbide and gallium nitride. Semiconductor elements using any one or more of silicon carbide and gallium nitride have different characteristics from silicon semiconductor elements, and therefore can be preferably used for power semiconductor elements, high-output power devices for base stations, sensors, detectors, and Schottky barrier diodes. In these uses, the heat resistance of semiconductor elements using any one or more of silicon carbide and gallium nitride is also considered. Since the resin sheet of the present embodiment has excellent heat resistance, it can be suitably used in combination with semiconductor elements using any one or more of silicon carbide and gallium nitride.

[0202] [Variations of Embodiments]

[0203] The present invention is not limited to the above-described embodiments, and modifications and improvements within the scope that can achieve the object of the present invention are included in the present invention.

[0204] In the above embodiment, a laminate having a first release material, a second release material, and a resin sheet provided between the first release material and the second release material has been described. Alternatively, a laminate having a release material only on one surface of a resin sheet may be used.

[0205] In addition, the semiconductor sealing application is described in the above-mentioned embodiment of the semiconductor device. In addition, the resin sheet of the present invention can also be used as an insulating material for a circuit substrate (for example, a hard printed wiring board material, a flexible wiring substrate material, and an interlayer insulating material for a laminated substrate, etc.), an adhesive film for lamination, and an adhesive, etc.

[0206] Example

[0207] Hereinafter, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to these Examples.

[0208] [Preparation of resin composition]

[0209] The resin compositions of Examples 1 to 5 and Comparative Examples 1 and 2 were prepared by dissolving or dispersing the components in a solvent at the blending ratios (mass % (ratio converted into solid content)) shown in Tables 1 and 2.

[0210] The materials used in the preparation of the resin composition are as follows.

[0211] (Thermosetting component)

[0212] Maleimide resin-1: a maleimide resin having a biphenyl group (a maleimide resin represented by the above general formula (3), "MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd.)

[0213] Maleimide resin-2: long-chain alkyl maleimide resin (maleimide resin represented by the above general formula (7-2-1), "BMI-1700" manufactured by Designer Molecules Co., Ltd.)

[0214] · Maleimide resin-3: long-chain alkyl maleimide resin ("SLK1500" manufactured by Shin-Etsu Chemical Co., Ltd.)

[0215] ·Allyl resin: diallyl bisphenol A ("DABPA" manufactured by Yamato Chemical Industry Co., Ltd.)

[0216] Curing catalyst (adhesion-imparting agent): 2,4-diamino-6-[2-(2-ethyl-4-methyl-1-imidazolyl)ethyl]-1,3,5-triazine ("2E4MZ-A" manufactured by Shikoku Chemical Industry Co., Ltd.)

[0217] (Silane coupling agent)

[0218] Silane coupling agent-1: a silane coupling agent represented by the above structural formula (B1-1) ("X-12-989MS" manufactured by Shin-Etsu Chemical Co., Ltd.)

[0219] Silane coupling agent-2: a silane coupling agent represented by the above structural formula (B1-2) ("X-12-1116" manufactured by Shin-Etsu Chemical Co., Ltd.)

[0220] Silane coupling agent-3: 3-glycidoxypropyltriethoxysilane

[0221] (Binder component)

[0222] Binder resin: BisA type phenoxy resin ("YX7200B35" manufactured by Mitsubishi Chemical Corporation)

[0223] (Inorganic filler)

[0224] Silica filler: fused silica (epoxysilane modified, average particle size 0.5 μm, maximum particle size 2.0 μm)

[0225] <Evaluation of resin composition and resin sheet>

[0226] [Production of Laminated Body Including Resin Sheet]

[0227] A resin varnish (a coating solution prepared by dissolving or dispersing the components of the resin composition in a mixed solvent of cyclohexanone and methyl ethyl ketone, with a solid content concentration of 60% by mass) was applied to a first release material (a polyethylene terephthalate film having a release layer formed by an alkyd resin release agent, manufactured by Lintec Corporation, PET38AL-5, with a thickness of 38 μm) using a knife coater, and dried at 90°C for 1 minute, and then dried at 115°C for 1 minute. The thickness of the dried resin composition was 25 μm. Immediately after being taken out of the drying oven, the dried resin composition and the second release material (a polyethylene terephthalate film having a release layer formed by a silicone release agent, manufactured by Lintec Corporation, SP-PET382150, with a thickness of 38 μm) were laminated at room temperature to produce a laminated body in which the first release material, the resin sheet formed by the resin composition, and the second release material were laminated in this order.

[0228] [Determination of peel strength]

[0229] One side of the resin sheet in the obtained laminate was subjected to reduced pressure and pressure bonding at a lamination temperature of 130°C, and thus bonded (laminating device: "V-130" manufactured by Nikko Materials; conditions: reaching pressure 100Pa, time 60 seconds) to a wafer (thickness 800μm) pre-cut into 4 equal parts by a 6-inch Si wafer, and then, a copper foil (size 50mm×10mm, thickness 350μm, JIS H 3100 specification) was subjected to reduced pressure and pressure bonding under the same conditions as above, and thus bonded to the other side of the resin sheet. It should be noted that the second stripping material and the first stripping material of the resin sheet in the laminate were peeled off before being attached to the Si wafer and the copper plate, respectively. Then, the resin composition was cured under a temperature of 180°C and a thermal curing condition of 2 hours to prepare a sample. For this sample, the copper foil was peeled off from the cured resin sheet using a tensile testing machine ("Autograph AG-IS" manufactured by Shimadzu Corporation) at a peeling speed of 50 mm / min and a peeling angle of 90 degrees, and the peel strength (unit: N / 10 mm) between the copper foil and the cured resin sheet was measured. The measurement was carried out under an environment of 23°C and a relative humidity of 50%. For Examples 1 to 3 and Comparative Example 1, the results obtained are shown in Table 1. In addition, for Examples 4 and 5 and Comparative Example 2, the results obtained are shown in Table 2.

[0230] [Measurement of elastic modulus at 250°C]

[0231] The obtained resin composition was coated on a release material, dried at 90°C for 1 minute, and dried at 110°C for 1 minute to prepare a resin sheet with a thickness of 25 μm. 8 sheets of the resin sheet were stacked to a thickness of 200 μm, and then peeled from the release material to prepare a sample. The sample was cured under a thermal curing condition of a temperature of 200°C and 4 hours to prepare a measurement sample. For the measurement sample, the storage modulus E' (unit: MPa) at 250°C was measured using "DMA Q800" manufactured by TA INSTRUMENTS under the conditions of a heating rate of 3°C / min, a temperature range of 0 to 300°C, and a frequency of 11 Hz. It should be noted that the larger the storage modulus at 250°C, the better the heat resistance. For Examples 1 to 3 and Comparative Example 1, the results obtained are shown in Table 1. In addition, for Examples 4 and 5 and Comparative Example 2, the results obtained are shown in Table 2.

[0232] [Table 1]

[0233]

[0234] It can be seen that for the resin compositions of Examples 1 to 3, all evaluations of peel strength and elastic modulus at 250°C were good. In addition, Comparative Example 1 is different from Example 1 and the like in that a silane coupling agent other than the compound represented by the general formula (B1) is used, and it can be seen that the peel strength result is poor compared with Example 1 and the like. This confirms that the resin compositions of Examples 1 to 3 have excellent heat resistance and can improve the peel strength after thermal curing.

[0235] [Table 2]

[0236]

[0237] It can be seen that for the resin compositions of Examples 4 and 5, all evaluations of peel strength and elastic modulus at 250°C were good. In addition, Comparative Example 2 is different from Example 4 and the like in that a silane coupling agent other than the compound represented by the general formula (B1) is used, and it can be seen that the result of peel strength is poor compared with Example 4 and the like. This confirms that the resin compositions of Examples 4 and 5 have excellent heat resistance and can improve the peel strength after thermal curing.

Claims

1. A resin composition comprising (A) a thermosetting component, (B) a silane coupling agent and (D) an inorganic filler, wherein: The (A) thermosetting component contains (A1) a maleimide resin, The (B) silane coupling agent is a compound represented by the following general formula (B1), (R 21 O) a (R 22 ) 3-a Si-L 21 -NH-L 22 -NH-R 23 ···(B1) In the general formula (B1), R 21 is an alkyl group, R 22 and R 23 are independently monovalent organic groups, L 21 is a divalent organic group, L 22 is -C(=O)- or -C(=S)-, a is 1, 2 or 3, The content of the (A) thermosetting component is 10% by mass or more and 40% by mass or less, and the content of the (B) silane coupling agent is 0.01% by mass or more and 5% by mass or less, based on the total solid content of the resin composition.

2. The resin composition according to claim 1, further comprising (E) an adhesion-imparting agent, The (E) adhesion-imparting agent is a compound having a triazine skeleton. 3 . A resin sheet formed from the resin composition according to claim 1 .

4. The resin sheet according to claim 3, wherein When the resin sheet and copper foil are bonded to each other and cured at a temperature of 180° C. for 2 hours, the peel strength after curing is 2.0 N / 10 mm or more.

5. The resin sheet according to claim 3, wherein When the resin sheet and the copper foil were bonded together and cured at a temperature of 180° C. for 2 hours, the peel strength after curing was 6.0 N / 10 mm or more. 6 . The resin sheet according to claim 3 , which is used for sealing a power semiconductor element or for being sandwiched between the power semiconductor element and other electronic components.

7. The resin sheet according to any one of claims 3 to 5, which is used to seal a semiconductor element using one or more of silicon carbide and gallium nitride, or to be sandwiched between the semiconductor element using one or more of silicon carbide and gallium nitride and other electronic components.