An electronic structure and a method for manufacturing the same
By forming a cross-linked fusion of a first conductive layer with high resin and low conductive particles on the substrate and a second conductive layer with high conductive particles and low resin, the problem of poor adhesion of low-temperature conductive silver paste on the glass substrate is solved, achieving Highly adherent and solderable electronic structures.
Patent Information
- Application Number
- CN202210474056.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-04-29
AI Technical Summary
Existing low-temperature conductive silver paste is difficult to meet user requirements for high adhesion and weldability, especially when molded on glass substrates, it has poor adhesion and is easy to peel off.
The first low-temperature conductive paste is used to form a conductive layer that is in direct contact with the substrate, and the adhesion is ensured through surface drying treatment, and then the second low-temperature conductive paste with high conductive particles and low resin is used to form the pad electrode, and heat-setting treatment is performed To achieve cross-linking and fusion to form an integrated electronic structure.
It achieves high adhesion and weldability effects, ensures the bonding strength of the conductive layer and the tinning performance of the pad electrode, and meets the user's needs for high adhesion and weldability.
Smart Images

Figure CN114867206B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electronic manufacturing, and in particular relates to an electronic structure and a manufacturing method thereof. Background Art
[0002] Conductive paste is an emerging raw material for additive manufacturing of electronic circuits. It is often used to form the electronic structure required by users through printing and other methods. Compared with traditional copper foil and aluminum foil etching technology, the printed conductive paste process has the advantages of low cost, pollution-free, fast and large-scale manufacturing.
[0003] Conductive pastes are generally divided into high-temperature conductive pastes and low-temperature conductive pastes based on the sintering and curing temperature. High-temperature conductive pastes mainly use glass powder as a binder for conductive particles, and the sintering temperature generally needs to reach thousands of degrees. Even if expensive low-melting-point glass powder on the market is used, the sintering temperature must be at least 500°C. It has high energy consumption, high equipment and supporting costs, and poor versatility, and cannot meet the needs of substrates with poor temperature resistance.
[0004] Low-temperature conductive paste mainly uses resin as a binder for conductive particles. The curing temperature generally only needs to be between 100°C and 300°C. It has low energy consumption, low equipment and supporting costs, and can meet the use of most substrates. Conventional low-temperature conductive pastes, such as low-temperature conductive silver paste, are mainly a viscous blend formed by mechanical mixing of silver powder, resin (also known as adhesive), solvent and additive. During the molding and curing process, the solvent and additive will gradually evaporate, thereby forming a conductive trace composed of silver powder and resin film.
[0005] At present, the existing low-temperature conductive silver paste is difficult to meet the user requirements of high adhesion and solderability, especially when it is formed on a glass substrate, the adhesion is poor and it is easy to peel off. Summary of the invention
[0006] In view of this, an object of the present invention is to provide a method for manufacturing an electronic structure to solve the problem in the prior art that low-temperature conductive silver paste cannot simultaneously meet user requirements of high adhesion and solderability.
[0007] In some illustrative embodiments, the method for manufacturing the electronic structure includes: providing a substrate; providing a first low-temperature conductive paste containing at least a resin carrier and conductive particles, forming a first conductive layer on the substrate using the first low-temperature conductive paste, and performing a surface drying treatment on the first conductive layer; wherein the first conductive layer has at least a target area for forming a pad electrode; providing a second low-temperature conductive paste containing at least a resin carrier and conductive particles, forming a second conductive layer covering at least the target area on the first conductive layer using the second low-temperature conductive paste to obtain the pad electrode; and simultaneously performing a thermosetting treatment on the first conductive layer and the second conductive layer to obtain an electronic structure in which the first conductive layer and the second conductive layer are cross-linked and fused together; wherein the mass fraction of the resin carrier in the first low-temperature conductive paste is higher than the mass fraction of the resin carrier in the second low-temperature conductive paste, and the mass fraction of the conductive particles in the first low-temperature conductive paste is lower than the mass fraction of the conductive particles in the second low-temperature conductive paste.
[0008] In some optional embodiments, the first low-temperature conductive paste includes, by mass fraction: 55% to 65% conductive particles, 13% to 18% resin carrier, 0% to 0.5% additive, and the rest is solvent.
[0009] In some optional embodiments, the second low-temperature conductive paste includes, by mass fraction: 75% to 85% conductive particles, 7% to 10% resin carrier, 0% to 0.5% additive, and the rest is solvent.
[0010] In some optional embodiments, after obtaining the electronic structure formed by cross-linking and fusing the first conductive layer and the second conductive layer, the method further includes: providing an element; and welding the element to the welding electrode.
[0011] In some optional embodiments, soldering the component onto the electronic structure specifically includes: printing solder paste at the location of the pad electrode, and using reflow soldering to achieve soldering between the component and the pad electrode.
[0012] In some optional embodiments, the substrate is selected from one or more composite substrates selected from PET, PI, PTFE, PC, ABS, LCP, PU, TPU, FR4, paper, wood, glass, stone, and fabric.
[0013] In some optional embodiments, the conductive particles are selected from one or more of gold, silver, copper, aluminum, zinc, nickel, and silver-coated copper.
[0014] In some optional embodiments, the resin carrier is selected from one or more of polyester resin, polyurethane resin, epoxy resin, acrylic resin, phenolic resin, alkyd resin, silicone resin, chloroacetic resin, and polyimide resin.
[0015] In some optional embodiments, the second conductive layer has a pattern consistent with that of the first conductive layer and completely covers the first conductive layer.
[0016] Another object of the present invention is to provide an electronic structure to solve the technical problems in the prior art.
[0017] In some illustrative embodiments, the electronic structure is obtained using any of the above-described methods for manufacturing an electronic structure.
[0018] Compared with the prior art, the present invention has the following advantages:
[0019] In the embodiment of the present invention, a first low-temperature conductive paste with low conductive particles and high resin is used to form a first conductive layer in direct contact with a substrate, thereby ensuring the adhesion of the first conductive layer on the substrate, and a second low-temperature conductive paste with high conductive particles and low resin is used to form a pad electrode on the first conductive layer to achieve the tinning performance of the pad electrode, thereby meeting the weldability requirements; in addition, a second conductive layer is formed after the surface of the first conductive layer is dried, and the two are thermally cured at the same time, so that the two form an integrated structure due to the cross-linking reaction, thereby ensuring the bonding strength of the second conductive layer on the first conductive layer, and achieving high adhesion and weldability effects in one. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a flow chart of a method for manufacturing an electronic structure in an embodiment of the present invention;
[0021] Figure 2 is a schematic diagram of the manufacturing process of the electronic structure in an embodiment of the present invention;
[0022] Figure 3 is a structural example 1 of the electronic structure in an embodiment of the present invention;
[0023] Figure 4 It is a flow chart of a method for manufacturing a transparent display screen in an embodiment of the present invention. DETAILED DESCRIPTION
[0024] Reference will now be made in detail to various embodiments of the present disclosure, examples of which are shown in the accompanying drawings. When described in conjunction with these embodiments, it will be understood that the embodiments are not intended to limit the present disclosure to these embodiments. On the contrary, the present disclosure is intended to cover alternatives, modifications, and equivalents that may be included within the spirit and scope of the present disclosure as defined in the appended claims. In addition, in the following specific embodiments of the present disclosure, many specific details are set forth in order to provide a thorough understanding of the present disclosure. However, it will be understood that the present disclosure may also be practiced without these specific details. In other examples, known methods, procedures, components, and circuits are not described in detail to avoid unnecessary obscurity of aspects of the present disclosure.
[0025] It should be noted that the various technical features in the embodiments of the present invention can be combined with each other without conflict.
[0026] The present invention discloses a method for manufacturing an electronic structure, specifically, Figure 1-3 As shown, Figure 1 is a flow chart of a method for manufacturing an electronic structure in an embodiment of the present invention; Figure 2 is a schematic diagram of the manufacturing process of the electronic structure in an embodiment of the present invention; Figure 3 This is a structural example 1 of the electronic structure in an embodiment of the present invention; a method for manufacturing the electronic structure includes:
[0027] Step S11, providing a substrate 10;
[0028] Step S12, providing a first low-temperature conductive paste containing at least a resin carrier and conductive particles, forming a first conductive layer 20 on the substrate using the first low-temperature conductive paste, and performing a surface drying treatment on the first conductive layer 20;
[0029] Wherein, the first conductive layer 20 has at least one target area for forming a pad electrode;
[0030] Step S13, providing a second low-temperature conductive paste containing at least a resin carrier and conductive particles, and using the second low-temperature conductive paste to form a second conductive layer 30 covering at least the target area on the first conductive layer 20 to obtain the pad electrode;
[0031] Step S14, simultaneously performing a thermosetting treatment on the first conductive layer 20 and the second conductive layer 30 to obtain an electronic structure 40 in which the first conductive layer and the second conductive layer are cross-linked and fused into one;
[0032] The mass fraction of the resin carrier in the first low-temperature conductive paste is higher than that in the second low-temperature conductive paste, and the mass fraction of the conductive particles in the first low-temperature conductive paste is lower than that in the second low-temperature conductive paste.
[0033] In the embodiment of the present invention, a first low-temperature conductive paste with low conductive particles and high resin is used to form a first conductive layer in direct contact with a substrate, thereby ensuring the adhesion of the first conductive layer on the substrate, and a second low-temperature conductive paste with high conductive particles and low resin is used to form a pad electrode on the first conductive layer to achieve the tinning performance of the pad electrode, thereby meeting the weldability requirements; in addition, a second conductive layer is formed after the surface of the first conductive layer is dried, and the two are thermally cured at the same time, so that the two form an integrated structure due to the cross-linking reaction, thereby ensuring the bonding strength of the second conductive layer on the first conductive layer, and achieving high adhesion and weldability effects in one.
[0034] The substrate in the embodiment of the present invention is selected from one or more composite substrates selected from PI, PTFE, PC, LCP, FR4, wood, glass, stone, and fabric.
[0035] The first low-temperature conductive paste and the second low-temperature conductive paste in the embodiment of the present invention are at least composed of a resin carrier and conductive particles, and in some embodiments, may further include: a solvent and / or an additive, etc. On the other hand, the first low-temperature conductive paste and the second low-temperature conductive paste in the embodiment of the present invention are low-temperature conductive pastes, which means that they mainly rely on the resin carrier as an adhesive, rather than glass powder used in a high-temperature environment, and when the glass powder is not used as an adhesive (i.e., the melting temperature of the glass powder is not reached), the low-temperature conductive paste may also include glass powder.
[0036] Preferably, in order to ensure that the first conductive layer has good conductivity, the mass fraction of the conductive particles of the first low-temperature conductive paste in the embodiment of the present invention must be no less than 55%, and in order to improve the adhesion of the first low-temperature conductive paste, the mass fraction of the resin carrier must be no less than 13%, thereby ensuring both the conductivity and adhesion of the first conductive layer.
[0037] Those skilled in the art should understand that, when the conductivity of the first conductive layer is not taken into consideration or the requirements for the conductivity are low, the mass fraction of the conductive particles in the first low-temperature conductive paste can be appropriately reduced.
[0038] Furthermore, a low-temperature conductive paste is proposed in an embodiment of the present invention, which is suitable for use as the first low-temperature conductive paste in the embodiment of the present invention. Calculated by mass fraction, the low-temperature conductive paste includes: 55% to 65% conductive particles, 13% to 18% resin carrier, 0% to 0.5% additives, and the rest is solvent.
[0039] The conductive particles in this embodiment may be selected from metal conductive particles, including but not limited to one or more of gold, silver, copper, aluminum, zinc, nickel, silver-coated copper, gallium, indium, tin, bismuth, gallium-based alloys, indium-based alloys, bismuth-based alloys, and tin-based alloys.
[0040] Preferably, the conductive particles in the embodiment of the present invention can be selected from gold powder, silver powder, and silver-coated copper powder. Compared with copper, aluminum, zinc, nickel, gallium, indium, tin, bismuth, gallium-based alloys, indium-based alloys, bismuth-based alloys, and tin-based alloys, these conductive particles are relatively stable in nature under the micron-sized structure, are not easy to form oxides, and have good conductivity; among them, the conductive particles can be selected from one or more of spherical, rod-shaped, flake-shaped, and branch-shaped.
[0041] Preferably, the conductive particles in the low-temperature conductive paste can be in a sheet structure. The conductive particles in this embodiment are in a sheet structure, and the conductive particles in the sheet structure have a wider overlap area, so the conductive paste of the conductive particles has better conductivity, and under the same conductivity, the demand for conductive particles is lower, so more resin carriers can be mixed in under the premise of ensuring the conductive performance, thereby improving the adhesion of the conductive paste.
[0042] The size of the conductive particles in this embodiment may range from 2 μm to 10 μm.
[0043] The resin carrier in this embodiment can be selected from one or more of polyester resin, polyurethane resin, epoxy resin, acrylic resin, phenolic resin, alkyd resin, silicone resin, chlorovinyl resin, and polyimide resin. The applicant has found that the adhesion of the low-temperature conductive paste to the substrate mainly depends on the type of resin. When the substrate is a glass substrate, preferably, the low-temperature conductive paste can use epoxy resin as the resin carrier, which can greatly improve the adhesion of the low-temperature conductive paste on the glass substrate.
[0044] The additives and solvents in this embodiment are conventionally selected in the art and will not be described in detail here.
[0045] Specifically, the mass fraction of the conductive particles in the low-temperature conductive paste can be 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64% or 65%. The mass fraction of the resin carrier in the low-temperature conductive paste can be 13%, 14%, 15%, 16%, 17% or 18%. The mass fraction of the auxiliary agent in the low-temperature conductive paste can be 0, 0.1%, 0.2%, 0.3%, 0.4% or 0.5%.
[0046] Preferably, in order to ensure that the second conductive layer has good tinning performance, the mass fraction of the conductive particles in the second low-temperature conductive paste in the embodiment of the present invention must be no less than 75%, and in order to ensure the printability of the second low-temperature conductive paste, the mass fraction of the resin carrier must be no less than 7%, thereby ensuring the printability and solderability of the second conductive layer at the same time.
[0047] Furthermore, a low-temperature conductive paste is proposed in an embodiment of the present invention, which is suitable for use as the second low-temperature conductive paste in the embodiment of the present invention. Calculated by mass fraction, the low-temperature conductive paste includes: 75% to 85% conductive particles, 7% to 10% resin carrier, 0% to 0.5% additives, and the rest is solvent.
[0048] The conductive particles in this embodiment may be selected from metal conductive particles, including but not limited to one or more of gold, silver, copper, aluminum, zinc, nickel, silver-coated copper, gallium, indium, tin, bismuth, gallium-based alloys, indium-based alloys, bismuth-based alloys, and tin-based alloys.
[0049] Preferably, the conductive particles in the embodiment of the present invention can be selected from gold powder, silver powder, and silver-coated copper powder. Compared with copper, aluminum, zinc, nickel, gallium, indium, tin, bismuth, gallium-based alloys, indium-based alloys, bismuth-based alloys, and tin-based alloys, these conductive particles are relatively stable in nature under the micron-sized structure, are not easy to form oxides, and have good conductivity; among them, the conductive particles can be selected from one or more of spherical, rod-shaped, flake-shaped, and branch-shaped.
[0050] Preferably, the conductive particles in the low-temperature conductive paste can be spherical. The conductive particles in this embodiment are spherical, and the conductive particles have a larger specific surface area. Therefore, the conductive paste of the conductive particles has more area to react with tin and is easier to form an alloy.
[0051] In addition, the smaller the particle size, the lower the melting point of the conductive particles, which can further enhance the reaction with tin. Specifically, the size range of the conductive particles is not greater than 2 μm, but the manufacturing cost of the conductive particles is higher if the size is too small. Therefore, the conductive particles are selected in the size range of 0.5 μm to 2 μm, which is more cost-effective in terms of cost and tinning performance.
[0052] The resin carrier in this embodiment can be selected from one or more of polyester resin, polyurethane resin, epoxy resin, acrylic resin, phenolic resin, alkyd resin, silicone resin, chlorovinyl resin, polyimide resin. Preferably, the resin carrier in this embodiment can be selected from polyester resin, which takes into account both heat resistance and electrical conductivity.
[0053] The additives and solvents in this embodiment are conventionally selected in the art and will not be described in detail here.
[0054] Specifically, the mass fraction of the conductive particles in the low temperature conductive paste can be 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84% or 85%. The mass fraction of the resin carrier in the low temperature conductive paste can be 7%, 8%, 9% or 10%. The mass fraction of the auxiliary agent in the low temperature conductive paste can be 0, 0.1%, 0.2%, 0.3%, 0.4% or 0.5%.
[0055] Preferably, the mass fraction of the conductive particles in the low-temperature conductive paste can be 80% to 85%, thereby further improving the tinning performance of the low-temperature conductive paste. In the conductive paste in this embodiment, the mass fraction of the conductive particles can be 80% to 85%. During the tinning process, there is sufficient contact area between the conductive particles and the solder paste, and the solder paste is not easy to separate from the conductive particles.
[0056] Preferably, the first low-temperature conductive paste in the embodiment of the present invention is an epoxy resin system, and the second low-temperature conductive paste is a polyester resin system, so that the electronic structure formed by the combination of the two has good adhesion, temperature resistance, conductivity and tinning performance on the glass substrate.
[0057] Optionally, after obtaining the electronic structure formed by cross-linking and fusing the first conductive layer and the second conductive layer, the method further includes: providing a component; and welding the component to the welding electrode. The component in this embodiment is not limited to components such as chips, LEDs, diodes, transistors, resistors, capacitors, inductors, and wires.
[0058] Preferably, soldering the component onto the electronic structure specifically includes: printing solder paste at the location of the pad electrode, and utilizing reflow soldering to achieve soldering between the component and the pad electrode.
[0059] Optionally, the second conductive layer in the embodiment of the present invention has the same pattern as the first conductive layer and completely covers the first conductive layer. The second conductive layer in this embodiment not only constitutes a welding electrode, but also enhances the overall conductivity and overall weldability of the first conductive layer.
[0060] The present invention also discloses an electronic structure which can be obtained by any of the above-mentioned methods for making an electronic structure. The electronic structure can be applied to electronic circuits such as PCB, FPC, smart wearables, transparent displays and other fields.
[0061] The embodiment of the present invention discloses a method for manufacturing a transparent display screen, comprising:
[0062] Step S21, providing a glass substrate;
[0063] Step S22, printing a first conductive layer on the glass substrate using a first low-temperature conductive paste;
[0064] Step S23, performing surface drying treatment on the first conductive layer;
[0065] Step S24, printing a second conductive layer on the first conductive layer using a second low-temperature conductive paste;
[0066] Step S25, simultaneously performing a thermosetting treatment on the first conductive layer and the second conductive layer to obtain an electronic structure in which the first conductive layer and the second conductive layer are cross-linked and fused into one;
[0067] Step S26, printing solder paste on the pad electrodes of the obtained electronic structure;
[0068] Step S27, mounting LED lamp beads and performing reflow soldering to obtain a transparent display screen.
[0069] The transparent display screen specifically comprises: a glass substrate, an electronic structure formed by cross-linking a first conductive layer and a second conductive layer which are printed successively to form an integrated structure, and LED lamp beads which are mounted and welded on the electronic structure.
[0070] In addition, the glass substrate in this embodiment may also be other transparent substrates to meet the production requirements of film screens and soft film screens.
[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for manufacturing an electronic structure, characterized in that: include: providing a substrate; Providing a first low-temperature conductive paste containing at least a resin carrier and conductive particles, forming a first conductive layer on the substrate using the first low-temperature conductive paste, and performing a surface drying treatment on the first conductive layer; wherein the first conductive layer has at least one target area for forming a pad electrode; Providing a second low-temperature conductive paste containing at least a resin carrier and conductive particles, and using the second low-temperature conductive paste to form a second conductive layer covering at least the target area on the first conductive layer to obtain the pad electrode; Simultaneously, the first conductive layer and the second conductive layer are subjected to a thermosetting treatment to obtain an electronic structure in which the first conductive layer and the second conductive layer are cross-linked and fused into one; The mass fraction of the resin carrier in the first low-temperature conductive paste is higher than that in the second low-temperature conductive paste, and the mass fraction of the conductive particles in the first low-temperature conductive paste is lower than that in the second low-temperature conductive paste.
2. The method for manufacturing an electronic structure according to claim 1, characterized in that: Calculated by mass fraction, the first low-temperature conductive paste includes: 55% to 65% conductive particles, 13% to 18% resin carrier, 0% to 0.5% additive, and the rest is solvent.
3. The method for manufacturing an electronic structure according to claim 1, characterized in that: Calculated by mass fraction, the second low-temperature conductive paste includes: 75% to 85% conductive particles, 7% to 10% resin carrier, 0% to 0.5% additive, and the rest is solvent.
4. The method for manufacturing an electronic structure according to claim 1, characterized in that: After obtaining the electronic structure formed by cross-linking and fusing the first conductive layer and the second conductive layer, the method further comprises: providing a component; The component is soldered onto the pad electrode.
5. The method for manufacturing an electronic structure according to claim 4, characterized in that: The step of welding the component onto the electronic structure specifically includes: Solder paste is printed at the pad electrode position, and reflow soldering is used to achieve soldering between the component and the pad electrode.
6. The method for manufacturing an electronic structure according to claim 1, characterized in that: The substrate is selected from one or more composite substrates selected from PI, PTFE, PC, LCP, FR4, wood, glass, stone, and fabric.
7. The method for manufacturing an electronic structure according to claim 1, characterized in that: The conductive particles are selected from one or more of gold, silver, copper, aluminum, zinc, nickel, silver-coated copper, gallium, indium, tin, bismuth, gallium-based alloy, indium-based alloy, bismuth-based alloy, and tin-based alloy.
8. The method for manufacturing an electronic structure according to claim 1, characterized in that: The resin carrier is selected from one or more of polyester resin, polyurethane resin, epoxy resin, acrylic resin, phenolic resin, alkyd resin, silicone resin, chloroacetic acid resin, and polyimide resin.
9. The method for manufacturing an electronic structure according to claim 1, characterized in that: The second conductive layer has a pattern consistent with that of the first conductive layer and completely covers the first conductive layer.
10. An electronic structure, characterized in that Obtained by the method for manufacturing an electronic structure according to any one of claims 1 to 9.