Method for producing rubber molded body
By setting specific parameters in the extrusion molding machine, the problem of the surface state of the rubber molded body falling after crosslinking in the prior art is solved, and the rubber molded body manufacturing with high productivity and excellent surface state is achieved.
Patent Information
- Application Number
- CN202080088249.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-27
- Filing Date
- 2020-12-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-12-21
AI Technical Summary
The prior art is difficult to manufacture a rubber molded body that can maintain an excellent surface state even after crosslinking at high productivity.
By using specific parameter settings in the extruder, such as the mixing amount of carbon black, DBP oil absorption value, screw diameter, screw speed and pitch number, to meet a specific range to prepare acrylic rubber compositions, ensuring that the rubber molded body is in the Maintain excellent surface condition after crosslinking.
The rubber molded body is manufactured at a high productivity and maintains an excellent surface state after crosslinking, improving production efficiency and product quality.
Smart Images

Figure CN114867591B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a rubber molded body, and more particularly to a method for producing a rubber molded body capable of producing a rubber molded body with high productivity and capable of achieving an excellent surface state even after cross-linking. Background Art
[0002] Acrylic rubber is a polymer mainly composed of units derived from (meth)acrylate monomers such as alkyl (meth)acrylate monomers and alkoxyalkyl (meth)acrylate monomers. It is generally known as a rubber with excellent heat resistance, oil resistance, and ozone resistance. It is widely used in automobile-related fields, etc. by mixing with a cross-linking agent to produce a cross-linked rubber.
[0003] The cross-linked rubber of acrylic rubber is obtained, for example, by extruding an acrylic rubber composition obtained by adding carbon black, a cross-linking agent, and the like to a rubber component containing acrylic rubber using an extruder to form a rubber molded body, and cross-linking the obtained rubber molded body (see, for example, Patent Document 1). In the technology of extruding the acrylic rubber composition, it is required to have good extrusion processability so as to produce a rubber molded body with an excellent surface state.
[0004] However, in the conventional techniques such as the technique described in Patent Document 1, no research has been conducted on producing a rubber molded body having an excellent surface state with high productivity or producing a rubber molded body capable of maintaining an excellent surface state even after crosslinking.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2002-220505. Summary of the invention
[0008] Problem that the invention aims to solve
[0009] The present invention has been made in view of such actual circumstances, and an object of the present invention is to provide a rubber molded body capable of producing a rubber molded body with high productivity and capable of achieving an excellent surface state even after crosslinking.
[0010] Solutions for solving problems
[0011] The present inventors have conducted intensive studies to achieve the above object and have found that when an acrylic rubber composition containing a rubber component including an acrylic rubber, carbon black and a crosslinking agent is molded using an extruder, the amount of carbon black contained in the acrylic rubber composition is adjusted to C. A , DBP oil absorption value C of carbon black D, the diameter S of the screw of the extruder D , extruder screw speed S S , and the total pitch number S of the screw of the extruder P The present invention has been completed because it has been found that within a specific range, the obtained rubber molded product can achieve an excellent surface state even after crosslinking, and the rubber molded product can be produced with high productivity.
[0012] That is, according to the present invention, there is provided a method for producing a rubber molded body by molding an acrylic rubber composition containing a rubber component including an acrylic rubber, carbon black, and a crosslinking agent using an extrusion molding machine to produce a rubber molded body.
[0013] When the amount of carbon black contained in the acrylic rubber composition is C A [phr], the DBP oil absorption value of the above carbon black is set as C D [cc / 100g], the diameter of the screw of the above extruder is set to S D [mm], the screw speed of the above extruder is set to S S [rpm], the total pitch of the screw of the extruder is denoted as S P In the case of the above-mentioned acrylic rubber composition being molded using the above-mentioned extrusion molding machine in a manner satisfying the following formula (1) and the following formula (2),
[0014] 6.5×10 3 ≤C A ×C D ≤1.1×10 4 (1)
[0015] 3.2×10 6 ≤C A ×S D ×S S ×S P ≤8.0×10 6 (2).
[0016] In the method for producing a rubber molded body of the present invention, it is preferred that the acrylic rubber contains a (meth)acrylic acid ester monomer unit and a crosslinking monomer unit, and the content of the (meth)acrylic acid ester monomer unit in the monomer units constituting the acrylic rubber is 50% by weight or more, and the content of the crosslinking monomer unit is 0.1% by weight or more.
[0017] In the method for producing a rubber molded product of the present invention, it is preferred that the crosslinkable monomer unit is a unit of an α,β-ethylenically unsaturated carboxylic acid monomer.
[0018] In the method for producing a rubber molded product of the present invention, it is preferred that the crosslinkable monomer unit is a unit of an α,β-ethylenically unsaturated dicarboxylic acid monoester monomer.
[0019] In the method for producing a rubber molded body of the present invention, it is preferred that the blending amount of the carbon black is C A It is 40~120phr.
[0020] In the method for producing a rubber molded body of the present invention, the extruder is preferably a uniaxial extruder.
[0021] Furthermore, according to the present invention, there is provided a method for producing a cross-linked rubber product, comprising the step of obtaining a rubber molded body according to any of the above-mentioned production methods and the step of cross-linking the rubber molded body.
[0022] Effects of the Invention
[0023] According to the present invention, it is possible to provide a rubber molded body capable of producing a rubber molded body with high productivity and capable of achieving an excellent surface state even after cross-linking. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram showing an extrusion molding machine used in a method for producing a rubber molded body according to one embodiment of the present invention.
[0025] Figure 2 It is a schematic diagram showing the screw arranged inside the extruder. DETAILED DESCRIPTION
[0026] The method for producing a rubber molded body of the present invention is a method for producing a rubber molded body by molding an acrylic rubber composition containing a rubber component including an acrylic rubber, carbon black, and a crosslinking agent using an extrusion molding machine.
[0027] When the amount of carbon black contained in the acrylic rubber composition is C A [phr], the DBP oil absorption value of the above carbon black is set as C D [cc / 100g], the diameter of the screw of the above extruder is set to S D [mm], the screw speed of the above extruder is set to S S [rpm], the total pitch of the screw of the extruder is denoted as S P In the case of the above-mentioned acrylic rubber composition being molded using the above-mentioned extrusion molding machine in a manner satisfying the following formula (1) and the following formula (2),
[0028] 6.5×10 3 ≤C A ×C D ≤1.1×104 (1)
[0029] 3.2×10 6 ≤C A ×S D ×S S ×S P ≤8.0×10 6 (2).
[0030] <Acrylic rubber>
[0031] First, the acrylic rubber used in the production method of the present invention will be described.
[0032] The acrylic rubber used in the present invention is a rubbery polymer containing (meth)acrylate monomer [meaning acrylate monomer and / or methacrylate monomer. Hereinafter, the same shall apply to methyl (meth)acrylate, etc.] units as the main component (meaning monomer units preferably accounting for 50% by weight or more of all monomer units constituting the acrylic rubber) in the molecule.
[0033] The (meth)acrylic acid ester monomer forming the (meth)acrylic acid ester monomer unit which is the main component of the acrylic rubber used in the present invention is not particularly limited, and examples thereof include alkyl (meth)acrylic acid ester monomers and alkoxyalkyl (meth)acrylic acid ester monomers.
[0034] The (meth)acrylic acid alkyl ester monomer is not particularly limited, but is preferably an ester of an alkanol having 1 to 12 carbon atoms and (meth)acrylic acid (a (meth)acrylic acid ester having an alkyl group having 1 to 12 carbon atoms), more preferably an ester of an alkanol having 1 to 8 carbon atoms and (meth)acrylic acid (a (meth)acrylic acid ester having an alkyl group having 1 to 8 carbon atoms), and still more preferably an ester of an alkanol having 2 to 6 carbon atoms and (meth)acrylic acid (a (meth)acrylic acid ester having an alkyl group having 2 to 6 carbon atoms).
[0035] Specific examples of the (meth)acrylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and cyclohexyl (meth)acrylate. Among these, ethyl (meth)acrylate and n-butyl (meth)acrylate are preferred, and ethyl acrylate and n-butyl acrylate are more preferred. These can be used alone or in combination of two or more.
[0036] The alkoxyalkyl (meth)acrylate monomer is not particularly limited, but is preferably an ester of an alkoxyalkyl alcohol having 2 to 12 carbon atoms and (meth)acrylic acid (a (meth)acrylate having an alkoxyalkyl group having 2 to 12 carbon atoms), more preferably an ester of an alkoxyalkyl alcohol having 2 to 8 carbon atoms and (meth)acrylic acid (a (meth)acrylate having an alkoxyalkyl group having 2 to 8 carbon atoms), and still more preferably an ester of an alkoxyalkyl alcohol having 2 to 6 carbon atoms and (meth)acrylic acid (a (meth)acrylate having an alkoxyalkyl group having 2 to 6 carbon atoms).
[0037] Specific examples of alkoxyalkyl (meth)acrylates include methoxymethyl (meth)acrylate, ethoxymethyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-propoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, and 4-methoxybutyl (meth)acrylate. Among these, 2-ethoxyethyl (meth)acrylate and 2-methoxyethyl (meth)acrylate are preferred, and 2-ethoxyethyl acrylate and 2-methoxyethyl acrylate are particularly preferred. These can be used alone or in combination of two or more.
[0038] In the acrylic rubber used in the present invention, it is preferred to use, as the (meth)acrylic acid ester monomer unit, a monomer unit composed of 30 to 100% by weight of an alkyl (meth)acrylate monomer unit and 70 to 0% by weight of an alkoxyalkyl (meth)acrylate monomer unit.
[0039] The content of the (meth)acrylate monomer unit in the monomer units constituting the acrylic rubber used in the present invention is preferably 50% by weight or more, more preferably 60% by weight or more, further preferably 70 to 99.9% by weight, further preferably 80 to 99.5% by weight, and particularly preferably 90 to 99% by weight. If the content of the (meth)acrylate monomer unit is too low, the weather resistance, heat resistance, and oil resistance of the obtained cross-linked rubber may be reduced.
[0040] The acrylic rubber used in the present invention may contain a crosslinking monomer unit in addition to a (meth)acrylate monomer unit as required. The crosslinking monomer forming the crosslinking monomer unit is not particularly limited, and examples thereof include α,β-ethylenically unsaturated carboxylic acid monomers, monomers having epoxy groups, monomers having halogen atoms, and diene monomers. As the crosslinking monomer, from the viewpoint of being able to further improve the scorch stability of the rubber composition of the acrylic rubber, the heat resistance of the rubber crosslinked product, and the compression set, α,β-ethylenically unsaturated carboxylic acid monomers, monomers having epoxy groups, and monomers having halogen atoms are preferred, α,β-ethylenically unsaturated carboxylic acid monomers and monomers having epoxy groups are more preferred, and α,β-ethylenically unsaturated carboxylic acid monomers are particularly preferred.
[0041] The α,β-ethylenically unsaturated carboxylic acid monomer is not particularly limited, and examples thereof include α,β-ethylenically unsaturated monocarboxylic acids, α,β-ethylenically unsaturated dicarboxylic acids, and α,β-ethylenically unsaturated dicarboxylic acid monoesters. By using an α,β-ethylenically unsaturated carboxylic acid monomer, the acrylic rubber can be made into a carboxyl group-containing acrylic rubber having a carboxyl group as a crosslinking point, thereby further improving the compression set resistance when the rubber crosslinked product is made.
[0042] The α,β-ethylenically unsaturated monocarboxylic acid is not particularly limited, but is preferably an α,β-ethylenically unsaturated monocarboxylic acid having 3 to 12 carbon atoms. Specific examples thereof include acrylic acid, methacrylic acid, α-ethylacrylic acid, crotonic acid, and cinnamic acid.
[0043] The α,β-ethylenically unsaturated dicarboxylic acid is not particularly limited, but is preferably an α,β-ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms. Specific examples thereof include butenedioic acids such as fumaric acid and maleic acid; itaconic acid; citraconic acid; and chloromaleic acid.
[0044] The α,β-ethylenically unsaturated dicarboxylic acid monoester is not particularly limited, but is preferably a monoester of an α,β-ethylenically unsaturated dicarboxylic acid having 4 to 12 carbon atoms and an alkanol having 1 to 12 carbon atoms, more preferably a monoester of an α,β-ethylenically unsaturated dicarboxylic acid having 4 to 6 carbon atoms and an alkanol having 2 to 8 carbon atoms, and still more preferably a monoester of butenedioic acid having 4 carbon atoms and an alkanol having 2 to 6 carbon atoms. Specific examples of α,β-ethylenically unsaturated dicarboxylic acid monoesters include: monomethyl fumarate, monoethyl fumarate, mono-n-butyl fumarate, monomethyl maleate, monoethyl maleate, mono-n-butyl maleate and other single-chain alkyl esters of butenedioic acid; monocyclopentyl fumarate, monocyclohexyl fumarate, monocyclohexenyl fumarate, monocyclopentyl maleate, monocyclohexyl maleate, monocyclohexenyl maleate and other butenedioic acid monoesters having an alicyclic structure; monomethyl itaconate, monoethyl itaconate, mono-n-butyl itaconate, monocyclohexyl itaconate and other itaconic acid monoesters; and the like.
[0045] Among these, α,β-ethylenically unsaturated dicarboxylic acid monoesters are preferred, butenedioic acid single-chain alkyl esters or butenedioic acid monoesters having an alicyclic structure are more preferred, fumaric acid mono-n-butyl ester, maleic acid mono-n-butyl ester, fumaric acid mono-cyclohexyl ester and maleic acid mono-cyclohexyl ester are further preferred, and fumaric acid mono-n-butyl ester is particularly preferred. These α,β-ethylenically unsaturated carboxylic acid monomers can be used alone or in combination of two or more. In addition, among the above-mentioned monomers, dicarboxylic acids also include monomers that exist as acid anhydrides.
[0046] The monomer having an epoxy group is not particularly limited, and examples thereof include epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate; and epoxy group-containing ethers such as allyl glycidyl ether and vinyl glycidyl ether.
[0047] The monomer having a halogen atom is not particularly limited, and examples thereof include unsaturated alcohol esters of halogen-containing saturated carboxylic acids, haloalkyl (meth)acrylates, haloacyloxyalkyl (meth)acrylates, (haloacetylcarbamoyloxy)alkyl (meth)acrylates, halogen-containing unsaturated ethers, halogen-containing unsaturated ketones, halogen-containing aromatic vinyl compounds, halogen-containing unsaturated amides, and halogen-containing acetyl unsaturated monomers. In addition, as the monomer having a halogen atom, a monomer containing a chlorine atom as the halogen atom is preferred.
[0048] Specific examples of the unsaturated alcohol ester of a halogen-containing saturated carboxylic acid include vinyl chloroacetate, vinyl 2-chloropropionate, and allyl chloroacetate.
[0049] Specific examples of the haloalkyl (meth)acrylate include chloromethyl (meth)acrylate, 1-chloroethyl (meth)acrylate, 2-chloroethyl (meth)acrylate, 1,2-dichloroethyl (meth)acrylate, 2-chloropropyl (meth)acrylate, 3-chloropropyl (meth)acrylate, and 2,3-dichloropropyl (meth)acrylate.
[0050] Specific examples of the haloacyloxyalkyl (meth)acrylate include 2-(chloroacetoxy)ethyl (meth)acrylate, 2-(chloroacetoxy)propyl (meth)acrylate, 3-(chloroacetoxy)propyl (meth)acrylate, and 3-(hydroxychloroacetoxy)propyl (meth)acrylate.
[0051] Specific examples of the (haloacetylcarbamoyloxy)alkyl (meth)acrylate include 2-(chloroacetylcarbamoyloxy)ethyl (meth)acrylate and 3-(chloroacetylcarbamoyloxy)propyl (meth)acrylate.
[0052] Specific examples of the halogen-containing unsaturated ether include chloromethyl vinyl ether, 2-chloroethyl vinyl ether, 3-chloropropyl vinyl ether, 2-chloroethyl allyl ether, and 3-chloropropyl allyl ether.
[0053] Specific examples of the halogen-containing unsaturated ketone include 2-chloroethyl vinyl ketone, 3-chloropropyl vinyl ketone, and 2-chloroethyl allyl ketone.
[0054] Specific examples of the halogenated methyl group-containing aromatic vinyl compound include p-chloromethylstyrene, m-chloromethylstyrene, o-chloromethylstyrene, p-chloromethyl-α-methylstyrene and the like.
[0055] Specific examples of the halogen-containing unsaturated amide include N-chloromethyl (meth) acrylamide and the like.
[0056] Specific examples of the halogenated acetyl group-containing unsaturated monomer include 3-(hydroxychloroacetyloxy)propyl allyl ether and p-vinylbenzyl chloroacetate.
[0057] Examples of the diene monomer include conjugated diene monomers such as 1,3-butadiene, isoprene, and piperylene; non-conjugated diene monomers such as ethylidene norbornene and dicyclopentadiene; and esters of (meth)acrylic acid and enol such as dicyclopentadienyl (meth)acrylate and 2-dicyclopentadienylethyl (meth)acrylate.
[0058] The content of the crosslinkable monomer unit in the monomer units constituting the acrylic rubber used in the present invention is preferably 0.01% by weight or more, more preferably 0.01 to 20% by weight, further preferably 0.1 to 10% by weight, further preferably 0.5 to 5% by weight, and particularly preferably 1 to 3% by weight. By making the content of the crosslinkable monomer unit within the above range, the mechanical properties and heat resistance of the obtained rubber cross-linked product can be improved and the compression set resistance can be more appropriately improved.
[0059] In addition, the acrylic rubber used in the present invention may have units of other monomers copolymerizable with the (meth)acrylate monomer units and the crosslinking monomer units used as needed. Such other monomers copolymerizable with these monomers are not particularly limited, and examples thereof include aromatic vinyl monomers, α,β-ethylenically unsaturated nitrile monomers, acrylamide monomers, α,β-ethylenically unsaturated dicarboxylic acid diester monomers, and other olefin monomers.
[0060] Examples of the aromatic vinyl monomer include styrene, α-methylstyrene, and divinylbenzene.
[0061] Examples of the α,β-ethylenically unsaturated nitrile monomer include acrylonitrile and methacrylonitrile.
[0062] Examples of the acrylamide-based monomer include acrylamide and methacrylamide.
[0063] Examples of the α,β-ethylenically unsaturated dicarboxylic acid diester monomer include: dialkyl maleates having an alkyl group with 1 to 18 carbon atoms, such as dimethyl maleate and di-n-butyl maleate; dialkyl fumarates having an alkyl group with 1 to 18 carbon atoms, such as dimethyl fumarate and di-n-butyl fumarate; dicycloalkyl maleates having a cycloalkyl group with 4 to 16 carbon atoms, such as dicyclopentyl maleate and dicyclohexyl maleate; dicycloalkyl fumarates having a cycloalkyl group with 4 to 16 carbon atoms, such as dicyclopentyl fumarate and dicyclohexyl fumarate; dialkyl itaconates having an alkyl group with 1 to 18 carbon atoms, such as dimethyl itaconate and di-n-butyl itaconate; and dicycloalkyl itaconates having a cycloalkyl group with 4 to 16 carbon atoms, such as dicyclohexyl itaconate.
[0064] Examples of other olefin monomers include ethylene, propylene, vinyl chloride, vinylidene chloride, vinyl acetate, ethyl vinyl ether, and butyl vinyl ether.
[0065] The other copolymerizable monomers can be used alone or in combination of two or more. The content of the units of these other copolymerizable monomers in the monomer units constituting the acrylic rubber used in the present invention is preferably 49.9 wt % or less, more preferably 29.9 wt % or less, further preferably 15 wt % or less, further preferably 9 wt % or less, and particularly preferably 4.5 wt % or less.
[0066] The Mooney viscosity (ML1+4, 100°C) of the acrylic rubber used in the present invention is in the range of 10 to 150, preferably 20 to 100, and more preferably 25 to 70. By setting the Mooney viscosity in the above range, the processability and strength characteristics of the acrylic rubber can be well balanced.
[0067] The glass transition temperature (Tg) of the acrylic rubber used in the present invention is not particularly limited, but is preferably 0°C or less, more preferably -5°C or less, and further preferably -10°C or less. In addition, the lower limit of the glass transition temperature (Tg) is not particularly limited, but is preferably -80°C or more, more preferably -60°C or more, and further preferably -40°C or more. By setting the glass transition temperature (Tg) within the above range, the balance between heat resistance and cold resistance of the acrylic rubber can be made more excellent.
[0068] The acrylic rubber used in the present invention can be produced by copolymerizing the above-mentioned monomers (free radical polymerization) by a known method such as emulsion polymerization, suspension polymerization, solution polymerization, and bulk polymerization. Among these polymerization methods, emulsion polymerization is preferred. In the emulsion polymerization, from the viewpoint of easy production of acrylic rubber, it is preferred to polymerize at low temperature (below 100° C.) and normal pressure. In addition, in the emulsion polymerization, in addition to using an emulsifier and a polymerization initiator, commonly used polymerization auxiliary materials can also be used.
[0069] The emulsifier is not particularly limited, and examples thereof include: nonionic emulsifiers such as polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene alkylphenol ethers such as polyoxyethylene nonylphenyl ether, polyoxyethylene alkyl esters such as polyoxyethylene stearate, polyoxyethylene sorbitan alkyl esters, and polyoxyethylene polyoxypropylene copolymers; anionic emulsifiers such as salts of fatty acids such as myristic acid, palmitic acid, oleic acid, and linolenic acid, alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate, higher alcohol sulfate ester salts such as sodium lauryl sulfate, higher phosphate ester salts such as sodium alkyl phosphate, and alkyl sulfosuccinates; and cationic emulsifiers such as alkyltrimethylammonium chloride, dialkylammonium chloride, and benzyl ammonium chloride. The amount of the emulsifier used is preferably 0.1 to 10 parts by weight, and more preferably 0.5 to 5 parts by weight, relative to 100 parts by weight of the monomers used for polymerization.
[0070] The polymerization initiator is not particularly limited, and can be used: azo compounds such as azobisisobutyronitrile; organic peroxides such as diisopropylbenzene hydroperoxide, cumene hydroperoxide, p-terpene hydroperoxide, benzoyl peroxide; inorganic peroxides such as sodium persulfate, potassium persulfate, hydrogen peroxide, ammonium persulfate, etc. These polymerization initiators can be used alone or in combination of two or more. The amount of the polymerization initiator used is preferably 0.001 to 1.0 parts by weight relative to 100 parts by weight of the monomer used for polymerization.
[0071] In addition, the organic peroxide and inorganic peroxide as polymerization initiators are preferably used in combination with a reducing agent as a redox polymerization initiator. The reducing agent used in combination is not particularly limited, and examples thereof include: compounds containing reduced metal ions such as ferrous sulfate, sodium ferric hexamethylenediaminetetraacetate, and cuprous cyclohexane; ascorbic acid (salts) such as ascorbic acid, sodium ascorbate, and potassium ascorbate; isoascorbic acid (salts) such as isoascorbic acid, sodium isoascorbate, and potassium isoascorbate; sugars; sulfinates such as sodium hydroxymethanesulfinate; sodium sulfite, potassium sulfite, sodium bisulfite, Sulfites such as sodium bisulfite and potassium bisulfite; pyrosulfites such as sodium pyrosulfite, potassium pyrosulfite, sodium pyrosulfite and potassium pyrosulfite; thiosulfates such as sodium thiosulfate and potassium thiosulfate; phosphorous acid (salts) such as phosphorous acid, sodium phosphite, potassium phosphite, sodium hydrogen phosphite and potassium hydrogen phosphite; pyrophosphorous acid (salts) such as pyrophosphorous acid, sodium pyrophosphite, potassium pyrophosphite, sodium hydrogen pyrophosphite and potassium hydrogen pyrophosphite; sodium formaldehyde sulfoxylate, etc. These reducing agents can be used alone or in combination of two or more. The amount of the reducing agent used is preferably 0.0003 to 0.1 parts by weight relative to 100 parts by weight of the polymerization initiator.
[0072] When producing acrylic rubber, in addition to the emulsifier and the polymerization initiator, polymerization auxiliary materials commonly used in the production of acrylic rubber, such as molecular weight modifiers, particle size modifiers, chelating agents, deoxidizers, etc., can be used.
[0073] <Acrylic rubber composition>
[0074] Next, the acrylic rubber composition used in the production method of the present invention will be described.
[0075] The acrylic rubber composition used in the production method of the present invention contains a rubber component including an acrylic rubber, carbon black, and a cross-linking agent.
[0076] The content of the acrylic rubber in the rubber component may be appropriately selected depending on the intended use, and is preferably 30% by weight or more, more preferably 50% by weight or more, further preferably 70% by weight or more, further preferably 90% by weight or more, and particularly preferably 100% by weight (i.e., a rubber consisting essentially of only acrylic rubber is used as the rubber component).
[0077] The rubber other than acrylic rubber constituting the rubber component is not particularly limited, and examples thereof include natural rubber, polybutadiene rubber, polyisoprene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, silicone rubber, fluororubber, olefin elastomers, styrene elastomers, vinyl chloride elastomers, polyester elastomers, polyamide elastomers, polyurethane elastomers, and silicone elastomers.
[0078] The carbon black is not particularly limited, and furnace black, acetylene black, thermal black, channel black, graphite, etc. can be cited. Among these, furnace black is preferably used, and specific examples thereof include SAF, ISAF, ISAF-HS, ISAF-LS, IISAF-HS, HAF, HAF-HS, HAF-LS, MAF, FEF, etc. These can be used alone or in combination of two or more.
[0079] In the present invention, the amount of carbon black added to the acrylic rubber composition is C A [phr], the DBP oil absorption value of carbon black is set to C D In the case of [cc / 100g], they satisfy the conditions of the following formula (1).
[0080] 6.5×10 3 ≤C A ×C D ≤1.1×10 4 (1)
[0081] According to the present invention, by adjusting the blending amount of carbon black to C A and the DBP oil absorption value C of carbon black D The above formula (1) is satisfied, and as described later, the amount of carbon black blended when the rubber molded body is produced using the acrylic rubber composition by an extruder is C A , the diameter S of the screw of the extruder D , extruder screw speed S S , and the total pitch number S of the screw of the extruder P By satisfying the formula (2) described later, a rubber molded product that can achieve an excellent surface state even after crosslinking can be produced with high productivity.
[0082] Carbon black content C A and the DBP oil absorption value C of carbon black D It is sufficient to satisfy the above formula (1), preferably satisfy the following formula (3), and more preferably satisfy the following formula (4). If "C A ×C D If the value of "C" is too small, the surface state of the obtained rubber molded product and rubber cross-linked product will deteriorate. A ×C D If the value of " is too large, the productivity of the acrylic rubber molded product will decrease.
[0083] 6.5×10 3 ≤C A ×C D ≤1.0×10 4 (3)
[0084] 6.5×10 3 ≤C A ×C D ≤9.0×10 3 (4)
[0085] Carbon black content C A [phr; per hundred rubber] is the amount of the rubber component containing the acrylic rubber contained in the acrylic rubber composition relative to 100 parts by weight (unit: "parts by weight"), and is expressed in terms of the DBP oil absorption value C of the carbon black. D The relationship between the above formula (1) can be satisfied, and the amount of carbon black C A It is preferably 40 to 120 phr, more preferably 45 to 100 phr, and even more preferably 50 to 80 phr.
[0086] In addition, the DBP oil absorption value C of carbon black D [cc / 100g] is the amount of DBP (dibutyl phthalate) absorbed by 100g of carbon black (unit: "cc"), measured in accordance with JIS K6221. D With the amount of carbon black C A The above formula (1) may be satisfied as long as the relationship between cc / 100 and cc / 100 g is satisfied. The content of cc / 100 g is preferably 50 to 200 cc / 100 g, more preferably 70 to 180 cc / 100 g, further preferably 80 to 160 cc / 100 g, and particularly preferably 95 to 140 cc / 100 g.
[0087] The crosslinking agent is not particularly limited, and examples thereof include polyamine compounds such as diamine compounds and carbonates thereof; sulfur; sulfur donors; triazine thiol compounds; polyvalent epoxy compounds; organic carboxylic acid ammonium salts; organic peroxides; dithiocarbamic acid metal salts; polycarboxylic acids; quaternary Salts; imidazole compounds; isocyanuric acid compounds and other conventionally known crosslinking agents. These crosslinking agents can be used alone or in combination of two or more. As the crosslinking agent, it is preferred to appropriately select according to the type of the crosslinkable monomer unit.
[0088] Among these, when the acrylic rubber used in the present invention has an α,β-ethylenically unsaturated carboxylic acid monomer unit as a crosslinkable monomer unit, it is preferable to use a polyamine compound and a carbonate thereof as the crosslinking agent.
[0089] The polyamine compound and its carbonate are not particularly limited, but preferably are polyamine compounds and their carbonates having 4 to 30 carbon atoms. Examples of such polyamine compounds and their carbonates include aliphatic polyamine compounds and their carbonates, and aromatic polyamine compounds.
[0090] The aliphatic polyamine compound and its carbonate are not particularly limited, and examples thereof include hexamethylenediamine, hexamethylenediamine carbamate, and N,N′-dicinnamylidene-1,6-hexanediamine, etc. Among these, hexamethylenediamine carbamate is preferred.
[0091] The aromatic polyamine compound is not particularly limited, and examples thereof include 4,4'-methylenedianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-(m-phenylenediisopropylidene)diphenylamine, 4,4'-(p-phenylenediisopropylidene)diphenylamine, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzanilide, 4,4'-bis(4-aminophenoxy)biphenyl, m-phenylenediamine, p-phenylenediamine, and 1,3,5-phenyltriamine. Among these, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane is preferred.
[0092] The content of the crosslinking agent in the acrylic rubber composition used in the present invention is preferably 0.001 to 20 parts by weight, more preferably 0.1 to 10 parts by weight, further preferably 0.1 to 5 parts by weight, and particularly preferably 0.2 to 4 parts by weight, relative to 100 parts by weight of the rubber component containing the acrylic rubber. By making the content of the crosslinking agent within the above range, the rubber elasticity can be sufficient and the mechanical strength of the resulting rubber cross-linked product can be excellent.
[0093] In addition, the acrylic rubber composition preferably further contains a crosslinking accelerator. The crosslinking accelerator is not particularly limited, and when the acrylic rubber has a carboxyl group as a crosslinking group and the crosslinking agent is a polyamine compound or a carbonate thereof, a guanidine compound, a diazabicycloolefin compound, an imidazole compound, a quaternary Salts, tertiary phosphine compounds, aliphatic mono-secondary amine compounds and aliphatic mono-tertiary amine compounds, etc. Among these, guanidine compounds, diazabicycloolefin compounds and aliphatic mono-secondary amine compounds are preferred, and guanidine compounds and diazabicycloolefin compounds are particularly preferred. These basic crosslinking accelerators can be used alone or in combination of two or more.
[0094] Specific examples of guanidine compounds include 1,3-di-o-tolylguanidine and 1,3-diphenylguanidine. Specific examples of diazabicycloolefin compounds include 1,8-diazabicyclo[5.4.0]undec-7-ene and 1,5-diazabicyclo[4.3.0]non-5-ene. Specific examples of imidazole compounds include 2-methylimidazole and 2-phenylimidazole. Specific examples of the salt include tetra-n-butylammonium bromide, octadecyltri-n-butylammonium bromide, etc. Specific examples of the tertiary phosphine compound include triphenylphosphine, tri-p-tolylphosphine, etc.
[0095] The aliphatic mono-secondary amine compound is a compound in which two hydrogen atoms of ammonia are replaced by aliphatic hydrocarbon groups. The aliphatic hydrocarbon group replacing the hydrogen atom is preferably an aliphatic hydrocarbon group having 1 to 30 carbon atoms. Specific examples of the aliphatic mono-secondary amine compound include dimethylamine, diethylamine, dipropylamine, diallylamine, diisopropylamine, di-n-butylamine, di-tert-butylamine, di-sec-butylamine, dihexylamine, diheptylamine, dioctylamine, dinonylamine, didecylamine, diundecylamine, didodecylamine, ditridecylamine, ditetradecylamine, dipentadecylamine, dihexadecylamine, di-2-ethylhexylamine, and dioctadecylamine.
[0096] The aliphatic mono-tertiary amine compound is a compound in which all three hydrogen atoms of ammonia are replaced by aliphatic hydrocarbon groups. The aliphatic hydrocarbon group replacing the hydrogen atom is preferably an aliphatic hydrocarbon group having 1 to 30 carbon atoms. Specific examples of the aliphatic mono-tertiary amine compound include trimethylamine, triethylamine, tripropylamine, triallylamine, triisopropylamine, tri-n-butylamine, tri-tert-butylamine, tri-sec-butylamine, trihexylamine, triheptylamine, trioctylamine, trinonylamine, tridecylamine, triundecylamine, and tridodecylamine.
[0097] The content of the crosslinking accelerator in the acrylic rubber composition is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 7.5 parts by weight, and even more preferably 1 to 5 parts by weight relative to 100 parts by weight of the rubber component containing the acrylic rubber. By setting the content of the crosslinking accelerator within the above range, the tensile strength and compression set resistance of the obtained rubber crosslink can be further improved.
[0098] In addition, the acrylic rubber composition may be blended with an antioxidant as needed. The antioxidant is not particularly limited, and examples thereof include: amine antioxidants such as phenyl-α-naphthylamine, phenyl-β-naphthylamine, p-(p-toluenesulfonamide)-diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, N,N-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, butyraldehyde-aniline condensate; imidazole antioxidants such as 2-mercaptobenzimidazole; quinoline antioxidants such as 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, etc. Among these, amine antioxidants are preferred.
[0099] The antioxidant can be used alone or in combination of two or more. The content of the antioxidant in the acrylic rubber composition is not particularly limited, but is preferably 0.01 to 15 parts by weight, more preferably 0.05 to 10 parts by weight, and further preferably 0.1 to 5 parts by weight, relative to 100 parts by weight of the rubber component containing the acrylic rubber.
[0100] In addition, the acrylic rubber composition used in the manufacturing method of the present invention can be mixed with compounding agents commonly used in the field of rubber processing in addition to the above-mentioned components. Examples of such compounding agents include reinforcing fillers such as silicon dioxide; non-reinforcing fillers such as calcium carbonate and clay; light stabilizers; anti-scorching agents; plasticizers; processing aids; adhesives; lubricants; lubricants; flame retardants; mildew inhibitors; antistatic agents; colorants, etc. The amount of these compounding agents is not particularly limited as long as it does not impair the purpose and effect of the present invention, and can be appropriately mixed in an amount corresponding to the purpose of the combination.
[0101] The acrylic rubber composition of the present invention is prepared by adding carbon black, a crosslinking agent and other various compounding agents used as needed to the rubber component containing the acrylic rubber, mixing and kneading them using an open roll mill, a Banbury mixer, various kneading machines, etc., and then further kneading them using a mixing roll.
[0102] The order of mixing the components is not particularly limited. It is preferred that the components that are not easily reacted or decomposed by heat are fully mixed, and then the crosslinking agent that is easily reacted or decomposed by heat is mixed for a short time at a temperature where it does not react or decompose.
[0103] <Method for producing rubber molded body>
[0104] The method for producing a rubber molded body of the present invention is to produce a rubber molded body by molding an acrylic rubber composition containing a rubber component including an acrylic rubber, carbon black and a crosslinking agent using an extruder.
[0105] When the amount of carbon black contained in the acrylic rubber composition is C A [phr], the DBP oil absorption value of the above carbon black is set as C D [cc / 100g], the diameter of the screw of the above extruder is set to S D [mm], the screw speed of the above extruder is set to S S [rpm], the total pitch of the screw of the extruder is denoted as S P In the case of the above-mentioned acrylic rubber composition, the molding of the above-mentioned acrylic rubber composition using the above-mentioned extrusion molding machine is carried out so as to satisfy the following formula (1) and the following formula (2).
[0106] 6.5×103 ≤C A ×C D ≤1.1×10 4 (1)
[0107] 3.2×10 6 ≤C A ×S D ×S S ×S P ≤8.0×10 6 (2)
[0108] Figure 1 Schematic diagram of an extrusion molding machine used in a method for producing a rubber molded body according to one embodiment of the present invention. Figure 1 In the case of the extrusion molding machine of the illustrated embodiment, a method for obtaining a rubber molded product by extrusion molding an acrylic rubber composition will be described.
[0109] like Figure 1 As shown in FIG. 1 , an extrusion molding machine 1 according to one embodiment includes a drive unit 2 and a single barrel 3 composed of 11 divided barrel blocks 31 to 41. In addition, a Figure 2 The screw 6 shown in the figure is connected to a die head 5 for molding the acrylic rubber composition kneaded in the barrel 3 into a predetermined shape on the downstream side of the barrel block 41 located at the most downstream side among the barrel blocks constituting the barrel 3, and is capable of extruding a rubber molded body having a predetermined shape. The die head 5 may have a cutter for cutting the extruded rubber molded body into a predetermined size. Figure 1 In the embodiment, as the barrel 3, a structure consisting of 11 barrel blocks 31 to 41 is exemplified, but the number of barrel blocks is not particularly limited and can be more Figure 1 The methods shown are more or more Figure 1 There are few ways shown.
[0110] Figure 2 Schematic diagram of the screw rod of the extrusion molding machine 1. Figure 2 The screw 6 shown in FIG. 1 is a single-axis extruder. The bottom end of the screw 6 is connected to a drive unit 2 (see FIG. 2 ). Figure 1 ) is used to drive the screw 6 by a motor or other driving unit in the screw rod 6, thereby keeping the screw rod 6 rotatable. The shape of the screw rod 6 is not particularly limited, and examples thereof include a full-thread type bidirectional screw rod.
[0111] In the method for producing a rubber molded body of the present invention, an acrylic rubber composition is charged into such an extruder 1, the charged acrylic rubber composition is kneaded in a barrel 3 by a shear force generated by the rotation of a screw 6 while being conveyed to the downstream side, and can be extruded into a rubber molded body having a predetermined shape through a die 5.
[0112] Then, in the method for producing a rubber molded body of the present invention, when extrusion molding is performed using such an extrusion molding machine 1, the diameter of the screw 6 of the extrusion molding machine 1 is set to S. D [mm], the rotation speed of the screw 6 of the extruder 1 is set to S S [rpm], the total pitch of the screw 6 of the extruder 1 is denoted as S P In the case of the above, the amount of carbon black contained in the acrylic rubber composition is C A The relationship of [phr] satisfies the following formula (2).
[0113] 3.2×10 6 ≤C A ×S D ×S S ×S P ≤8.0×10 6 (2)
[0114] In the present invention, as described above, by adjusting the blending amount of carbon black to C A DBP oil absorption value C of carbon black D The above formula (1) is satisfied and the amount of carbon black blended when the rubber molded body is produced using the acrylic rubber composition by the extruder 1 is C A , the diameter S of the screw 6 of the extruder 1 D , the speed S of the screw 6 of the extruder 1 S , and the total pitch number S of the screw 6 of the extruder 1 P When the above formula (2) is satisfied, a rubber molded product that can achieve an excellent surface state even after crosslinking can be produced with high productivity.
[0115] Carbon black content C A , the diameter S of the screw 6 of the extruder 1 D , the speed S of the screw 6 of the extruder 1 S , and the total pitch number S of the screw 6 of the extruder 1 P It is sufficient to satisfy the above formula (2), preferably satisfy the following formula (5), and more preferably satisfy the following formula (6). When "C A ×S D ×S S ×S P " is too small, the productivity will decrease. On the other hand, when "CA ×S D ×S S ×S P If the value of " is too large, the surface state of the obtained rubber cross-linked product may be deteriorated.
[0116] 4.5×10 6 ≤C A ×S D ×S S ×S P ≤7.6×10 6 (5)
[0117] 5.0×10 6 ≤C A ×S D ×S S ×S P ≤7.1×10 6 (6)
[0118] The diameter S of the screw 6 of the extruder 1 is D is the outer diameter of the screw 6 of the extruder 1 (the diameter of the screw rib portion of the screw 6, between the screw groove portion and the screw rib portion), so that "C A ×S D ×S S ×S P The value of " can satisfy the above formula (2), and the diameter S of the screw 6 of the extruder 1 D It is preferably 20 to 200 mm, more preferably 30 to 150 mm, further preferably 50 to 100 mm, and particularly preferably 65 to 85 mm.
[0119] The speed S of the screw 6 of the extruder 1 S The rotation speed of the screw 6 during extrusion molding of the acrylic rubber composition is preferably 5 to 60 rpm, more preferably 10 to 50 rpm, and even more preferably 15 to 45 rpm.
[0120] In addition, the total pitch number S of the screw 6 of the extruder 1 is P It is the total number of the flight portions constituting the screw 6, and is preferably 10 to 50, more preferably 15 to 45, further preferably 20 to 40, and particularly preferably 27 to 37. P When the number of flights of the screw 6 is 32, that is, the total number of flights of the screw 6 in the length direction of the screw 6 is 32.
[0121] In addition, other conditions for extrusion molding using the extrusion molding machine 1 are not particularly limited. For example, the length S of the screw 6 LIt is preferably 400 to 3000 mm, more preferably 700 to 2500 mm, further preferably 1000 to 2000 mm, and particularly preferably 1050 to 1350 mm. The groove depth of the screw 6 is not particularly limited, but is preferably 4 to 12 mm, more preferably 5 to 11 mm, and further preferably 6 to 10 mm.
[0122] In addition, the temperature of the screw 6 during extrusion molding by the extrusion molding machine 1 is not particularly limited, but is preferably 50 to 110° C., more preferably 60 to 100° C., and further preferably 70 to 100° C. The temperature of the barrel constituting the barrel 3 is preferably 50 to 110° C., more preferably 60 to 100° C., and further preferably 70 to 100° C. Furthermore, the temperature of the die head 5 is preferably 60 to 120° C., more preferably 70 to 110° C., and further preferably 80 to 110° C.
[0123] <Rubber cross-linked product>
[0124] The cross-linked rubber of the present invention is obtained by cross-linking the rubber molded body obtained by the above-mentioned production method of the present invention.
[0125] The rubber cross-linked product of the present invention can be produced by heating the rubber molded body obtained by the above-mentioned manufacturing method of the present invention to carry out a cross-linking reaction and solidify the shape into a rubber cross-linked product. The cross-linking temperature is usually 130 to 220°C, preferably 150 to 190°C, and the cross-linking time is usually 2 minutes to 10 hours, preferably 3 minutes to 5 hours. As the heating method, oven heating, steam heating, microwave heating, hot air heating and other methods that can be used for rubber cross-linking can be appropriately selected. For example, in the case where the rubber molded body is in the shape of a hose, a mandrel can be inserted into the inner side of the hose-shaped rubber molded body, and heating can be performed in the state where the mandrel is inserted, thereby making a rubber cross-linked product.
[0126] In addition, the cross-linked rubber of the present invention may be further heated to perform secondary cross-linking depending on the shape and size of the cross-linked rubber. The secondary cross-linking varies depending on the heating method, cross-linking temperature, shape, etc., but is preferably performed for 1 to 48 hours. The heating method and heating temperature may be appropriately selected.
[0127] The rubber cross-linked product of the present invention thus obtained can be preferably used for various hoses such as oil hoses, ATF hoses, brake hoses and the like, turbo air hoses, transmission control hoses, exhaust hoses and the like air hoses, radiator hoses, heater hoses, air conditioning hoses and the like.
[0128] Example
[0129] The present invention will be described in detail below with reference to Examples and Comparative Examples. Unless otherwise specified, "parts" are based on weight. Tests and evaluations were performed as follows.
[0130] <Monomer Composition of Acrylic Rubber>
[0131] Regarding the composition of each monomer unit contained in acrylic rubber, 1 The content of the carboxyl group in the acrylic rubber was confirmed by H-NMR measurement, and the content of the carboxyl group in the acrylic rubber was calculated by dissolving the acrylic rubber in acetone and performing potentiometric titration with a potassium hydroxide solution.
[0132] <Mooney viscosity (ML1+4, 100°C)>
[0133] The Mooney viscosity (ML1+4, 100° C.) of the acrylic rubber at a measurement temperature of 100° C. was measured in accordance with the Mooney viscosity test of uncrosslinked rubber physical testing methods of JIS K6300.
[0134] <Surface Condition of Rubber Molded Articles and Rubber Cross-linked Products>
[0135] The surface conditions of the rubber molded product and the rubber cross-linked product were visually observed and evaluated according to the following criteria.
[0136] ○: The surface is smooth and glossy.
[0137] △: Neither irregularities nor small wrinkles were observed on the surface, but there was no gloss.
[0138] ×: Concavities and convexities or small wrinkles were observed on the surface.
[0139] <Extrusion volume of extrusion molding>
[0140] The extrusion weight (g / 20 seconds) of every 20 seconds when the acrylic rubber composition is used for extrusion molding is measured as the extrusion amount. The larger the value of the extrusion amount, the more excellent the productivity can be judged. In addition, the extrusion amount is shown as a relative value when the value of Comparative Example 2 is taken as 100.
[0141] <Discharge Temperature of Rubber Molded Body>
[0142] When the acrylic rubber composition is extruded, the temperature of the rubber molded body discharged from the die 5 is measured with a contact thermometer.
[0143] <Production Example 1>
[0144] (Manufacture of acrylic rubber)
[0145] 200 parts of water, 2 parts of sodium dodecyl sulfate, 64 parts of ethyl acrylate and 34.6 parts of n-butyl acrylate were added to a polymerization reactor equipped with a thermometer and a stirring device. After three times of degassing and nitrogen substitution to fully remove oxygen, 1.4 parts of mono-n-butyl fumarate and 0.006 parts of terpene hydroperoxide were added, and emulsion polymerization was started at normal pressure and temperature 20°C. The reaction was allowed to proceed for 5 hours until the polymerization conversion rate reached about 90%. Then, the obtained emulsion polymerization liquid was coagulated with a calcium chloride solution, washed with water, and dried to obtain an acrylic rubber. The polymer composition of the obtained acrylic rubber was 64.0% by weight of ethyl acrylate units, 34.6% by weight of n-butyl acrylate units, and 1.4% by weight of mono-n-butyl fumarate units. In addition, the Mooney viscosity (ML1+4, 100°C) of the obtained acrylic rubber was 33.
[0146] <Example 1>
[0147] (Preparation of acrylic rubber composition)
[0148] Using a Banbury mixer, 65 parts of HAF carbon black (trade name "Seast3", manufactured by Tokai Carbon Co., Ltd., DBP oil absorption value: 101cc / 100g), 5 parts of a plasticizer (trade name "ADKCIZER RS735", manufactured by ADEKA), 2 parts of stearic acid, 1 part of an ester wax (product name "Greg G-8205", manufactured by Dainippon Ink & Chemicals Co., Ltd., lubricant), 2 parts of 4,4'-bis(α,α-dimethylbenzyl)diphenylamine (trade name "NocracCD", manufactured by Ouchi Shinko Chemical Co., Ltd., antioxidant) and 1 part of a primary alkylamine (trade name "lipomin 18D", manufactured by Lion Specialty Chemicals Co., Ltd.) were added to 100 parts of the acrylic rubber obtained in Production Example 1, and mixed at 50°C for 5 minutes. Next, the obtained mixture was transferred to a roll mixer at 50°C. 0.5 parts of hexamethylenediamine carbamate (trade name "Diak#1", manufactured by DuPont Dow Elastomers, aliphatic polyamine compound) as a crosslinking agent and 2 parts of 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) (trade name "RHENOGRAN XLA-60", manufactured by Rhein Chemie, DBU 60% (including the portion that becomes dialkyl diphosphonic acid zinc salt)) as a crosslinking accelerator were added thereto, and kneaded to obtain an acrylic rubber composition.
[0149] Next, the acrylic rubber composition obtained above was subjected to Figure 1The single-screw extruder 1 (trade name "EMR-V75D16", manufactured by EM Giken Co., Ltd.) was used to perform extrusion molding, thereby continuously producing a hose-shaped rubber molded body. The extrusion molding conditions were as follows.
[0150] Carbon black content C A :65phr
[0151] DBP oil absorption value C of carbon black D : 101cc / 100g
[0152] The diameter S of the screw 6 of the extruder 1 is D : 75mm
[0153] The speed S of the screw 6 of the extruder 1 S : 30rpm
[0154] The total pitch number S of the screw 6 of the extruder 1 P :32
[0155] Shape of the screw 6 of the extruder 1: Full-thread type bidirectional screw
[0156] Groove depth of screw 6 of extruder 1: 7.5 mm
[0157] The thread pitch of the screw 6 of the extruder 1: 75 mm
[0158] The length S of the screw 6 of the extruder 1 L : 1200mm
[0159] Temperature of screw 6 of extruder 1: 80°C
[0160] Temperature of the barrel constituting the barrel 3 of the extruder 1: 80°C
[0161] Temperature of die head 5 of extruder 1: 90°C
[0162] Die head diameter of die head 5: 33mm
[0163] Nozzle diameter of die head 5: 30mm
[0164] Then, the extrusion amount during extrusion molding and the surface condition of the obtained hose-shaped rubber molded body were evaluated according to the above-mentioned method.
[0165] Next, the obtained hose-shaped rubber molded body was cut into 50 mm lengths, and a 30 mm φ SUS metal rod (mandrel) was inserted into the inner surface of the cut hose-shaped rubber molded body, and the hose-shaped rubber cross-linked body was heated in an oven at 170° C. for 1 hour with the SUS metal rod inserted, thereby obtaining a hose-shaped rubber cross-linked body. Then, the surface state of the obtained rubber cross-linked body was evaluated according to the above method. The results are shown in Table 1.
[0166] <Example 2, Example 3>
[0167] The blending amount of HAF carbon black is C A and the speed S of the screw 6 of the extruder 1 S A rubber molded product and a rubber cross-linked product were obtained in the same manner as in Example 1, except that one of the above was changed as shown in Table 1, and were evaluated in the same manner.
[0168] <Comparative Examples 1 to 6>
[0169] The blending amount of HAF carbon black is C A and the speed S of the screw 6 of the extruder 1 S A rubber molded product and a rubber cross-linked product were obtained in the same manner as in Example 1, except that one or both of the above were changed as shown in Table 1, and were evaluated in the same manner.
[0170] [Table 1]
[0171]
[0172] <Example 4>
[0173] A rubber molded body and a rubber cross-linked product were obtained in the same manner as in Example 1, except that 50 parts of MAF carbon black (trade name "Seast 116", manufactured by Tokai Carbon Co., Ltd., DBP oil absorption value: 135 cc / 100 g) was used instead of 65 parts of HAF carbon black, and the results were evaluated in the same manner.
[0174] <Examples 5 to 8>
[0175] The blending amount of MAF carbon black is C A and the speed S of the screw 6 of the extruder 1 S A rubber molded product and a rubber cross-linked product were obtained in the same manner as in Example 4, except that one or both of the above were changed as shown in Table 2, and were evaluated in the same manner.
[0176] <Comparative Examples 7 to 12>
[0177] The blending amount of MAF carbon black is C A and the speed S of the screw 6 of the extruder 1 SA rubber molded product and a rubber cross-linked product were obtained in the same manner as in Example 4, except that one or both of the above were changed as shown in Table 2, and were evaluated in the same manner.
[0178] [Table 2]
[0179]
[0180] <Example 9>
[0181] A rubber molded body and a rubber cross-linked product were obtained in the same manner as in Example 1, except that 65 parts of FEF carbon black (trade name "Seast SO", manufactured by Tokai Carbon Co., Ltd., DBP oil absorption value: 115 cc / 100 g) was used instead of 65 parts of HAF carbon black, and were evaluated in the same manner. The results are shown in Table 3.
[0182] <Example 10, Example 11>
[0183] The amount of FEF carbon black added is C A and the speed S of the screw 6 of the extruder 1 S A rubber molded product and a rubber cross-linked product were obtained in the same manner as in Example 9, except that one or both of the above were changed as shown in Table 3, and were evaluated in the same manner.
[0184] <Comparative Examples 13 to 18>
[0185] The amount of FEF carbon black added is C A and the speed S of the screw 6 of the extruder 1 S A rubber molded product and a rubber cross-linked product were obtained in the same manner as in Example 9, except that one or both of the above were changed as shown in Table 3, and were evaluated in the same manner.
[0186] [Table 3]
[0187]
[0188] <Comparative Example 19>
[0189] 50 parts of SRF carbon black (trade name "Seast S", manufactured by Tokai Carbon Co., Ltd., DBP oil absorption value: 68 cc / 100 g) were used instead of 65 parts of HAF carbon black, and the rotation speed S of the screw 6 of the extruder 1 was increased to 1. S The rubber molded body and the rubber cross-linked product were obtained in the same manner as in Example 1 except that the rotation speed was changed to 15 rpm, and were evaluated in the same manner.
[0190] <Comparative Examples 20 to 27>
[0191] The blending amount of SRF carbon black is C Aand the speed S of the screw 6 of the extruder 1 S A rubber molded product and a rubber cross-linked product were obtained in the same manner as in Comparative Example 19, and evaluated in the same manner. The results are shown in Table 4.
[0192] [Table 4]
[0193]
[0194] As shown in Tables 1 to 4, when the acrylic rubber composition is extruded using an extruder, the 3 ≤C A ×C D ≤1.1×10 4 " conditions and "3.2×10 6 ≤C A ×S D ×S S ×S P ≤8.0×10 6 When extrusion molding is performed under the conditions of ", the surface conditions of the obtained rubber molded body and the rubber cross-linked product are excellent, and the extrusion amount during extrusion molding is also large, and the productivity is excellent (Examples 1 to 11).
[0195] On the other hand, for the acrylic rubber composition, when extrusion molding is performed using an extruder, if the "6.5×10 3 ≤C A ×C D ≤1.1×10 4 " conditions and "3.2×10 6 ≤C A ×S D ×S S ×S P ≤8.0×10 6 ", as a result, the surface condition of one or both of the obtained rubber molded product and the rubber cross-linked product is poor, or the extrusion amount during extrusion molding is small and the productivity is poor (Comparative Examples 1 to 27).
[0196] Description of Reference Numerals
[0197] 1: Extruder;
[0198] 2: Drive unit;
[0199] 3: Barrel;
[0200] 31-41: barrel block;
[0201] 5: Die head;
[0202] 6: Screw.
Claims
1. A method for producing a rubber molded body, comprising molding an acrylic rubber composition containing a rubber component including an acrylic rubber, carbon black and a crosslinking agent using a uniaxial extruder to produce a rubber molded body, When the amount of carbon black contained in the acrylic rubber composition is C A , the DBP oil absorption value of the carbon black is set to C D , the diameter of the screw of the extruder is set to S D , the screw speed of the extruder is set to S S , the total pitch number of the screw of the extruder is set to S P In the case of the above-mentioned, the above-mentioned acrylic rubber composition is molded using the above-mentioned extrusion molding machine in a manner satisfying the following formula (1) and the following formula (2), The C A The unit is phr, the C D The unit is cc / 100g, the S D The unit is mm, the S S The unit is rpm, The DBP oil absorption value is measured based on JIS K6221. 6.5×10 3 ≤C A ×C D ≤1.1×10 4 (1) 3.2×10 6 ≤C A ×S D ×S S ×S P ≤8.0×10 6 (2)。 2. The method for producing a rubber molded body according to claim 1, in, The acrylic rubber contains (meth)acrylate monomer units and cross-linking monomer units. The content of the (meth)acrylic acid ester monomer unit in the monomer units constituting the acrylic rubber is 50% by weight or more, and the content of the crosslinking monomer unit is 0.1% by weight or more.
3. The method for producing a rubber molded body according to claim 2, in, The crosslinking monomer unit is a unit of an α,β-ethylenically unsaturated carboxylic acid monomer.
4. The method for producing a rubber molded body according to claim 3, in, The crosslinking monomer unit is a unit of an α,β-ethylenically unsaturated dicarboxylic acid monoester monomer.
5. The method for producing a rubber molded body according to any one of claims 1 to 3, in, The amount of carbon black blended C A It is 40~120phr. 6 . A method for producing a rubber cross-linked product, comprising the steps of obtaining a rubber molded body according to the production method according to claim 1 , and cross-linking the rubber molded body.