Positive electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery
By adjusting the void ratio of the positive electrode composite material layer and adding carbon nanotubes, combined with an appropriate amount of polyvinylidene fluoride, the problems of lithium ion mobility and resistance are solved, and a high-capacity and low-resistance secondary battery is achieved.
Patent Information
- Application Number
- CN202080087516.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-18
- Filing Date
- 2020-12-08
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-12-08
AI Technical Summary
In the prior art, the high-density positive electrode composite material layer makes it difficult for lithium ions to move, resulting in an increase in the secondary battery resistance, and the stability of the positive electrode composite material slurry deteriorates when the content of polyvinylidene fluoride is small, and the resistance is high.
By adjusting the void ratio of the positive electrode composite layer to 23% to 50% by volume, carbon nanotubes with an aspect ratio of 100 to 1000, the number of molecules of polyvinylidene fluoride is controlled to be 0.005 in the positive electrode composite layer per unit mass. ~0.030, realize the synergistic effect between carbon nanotubes and polyvinylidene fluoride, improve the adhesion strength and electron conductivity of the positive electrode active material, and reduce resistance.
A high-capacity and low resistance secondary battery is achieved, ensuring good mobility of lithium ions between the positive electrode active material particles and the low resistance performance of the battery.
Smart Images

Figure CN114868276B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a positive electrode for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery. Background Art
[0002] In recent years, secondary batteries are increasingly required to have higher capacity. Patent Document 1 discloses a high-capacity secondary battery in which the volume ratio of the positive active material in the positive composite material is set to 97.1% to 99.6%, and the volume ratio of the voids in the positive composite material layer is set to 16% to 22%, thereby increasing the density of the positive active material in the positive composite material layer to 3.7 g / cc or more.
[0003] In addition, in the positive electrode composite material layer, by reducing the content of the binding material and increasing the content of the positive electrode active material, a high-capacity secondary battery can be obtained. Patent document 2 discloses a method of obtaining a positive electrode composite material slurry having properties suitable for the preparation of a high-capacity positive electrode composite material layer by controlling the preparation temperature to 30°C to 60°C, comprising polyvinylidene fluoride with a molecular weight of 600,000 to 1,000,000 as a binding material.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-43257
[0007] Patent Document 2: Japanese Patent No. 4263501 Summary of the invention
[0008] When the positive electrode composite material layer is densified in the manner disclosed in Patent Document 1, it becomes difficult for lithium ions to move between the particles of the positive electrode active material, and sometimes it becomes high resistance. In addition, even if polyvinylidene fluoride with a molecular weight of 600,000 to 1,000,000 is used in the manner disclosed in Patent Document 2, when the content of polyvinylidene fluoride is small, the stability of the positive electrode composite material slurry will deteriorate, and sometimes it will become high resistance. The technology disclosed in Patent Documents 1 and 2 does not take into account the battery resistance, and there is still room for improvement.
[0009] The non-aqueous electrolyte secondary battery positive electrode of one embodiment of the present disclosure has a positive electrode core and a positive electrode composite material layer formed on the surface of the positive electrode core. The porosity of the positive electrode composite material layer is 23% to 50% by volume, and the positive electrode composite material layer contains at least a positive electrode active material, carbon nanotubes as a conductive auxiliary material, and polyvinylidene fluoride as a binding material, the particle size of the carbon nanotubes is 5nm to 40nm, and the aspect ratio is 100 to 1000, and the content in the positive electrode composite material layer is 0.2% to 5% by mass, and the number of polyvinylidene fluoride molecules contained in the unit mass of the positive electrode composite material layer is 0.005 to 0.030.
[0010] A nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure includes the above-described positive electrode for a nonaqueous electrolyte secondary battery, a negative electrode, and a nonaqueous electrolyte.
[0011] According to the present disclosure, a secondary battery having high capacity and low resistance can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a perspective view of a secondary battery as an example of an embodiment, and is a view showing the internal structure of a battery case in a state where the front side of an exterior body is removed. DETAILED DESCRIPTION
[0013] A secondary battery with high capacity and high output is required. By reducing the porosity and densifying the positive electrode composite material layer, the high capacity of the secondary battery can be achieved, but lithium ions will become difficult to move between the particles of the positive electrode active material, and the secondary battery will sometimes become high resistance. The inventors and others conducted in-depth research and found that: the porosity of the positive electrode composite material layer is adjusted to an appropriate range, and a prescribed amount of carbon nanotubes with a high aspect ratio are added, so that the number of molecules of polyvinylidene fluoride contained in the unit mass positive electrode composite material layer is within a prescribed range, thereby obtaining a secondary battery that takes into account both high capacity and low resistance. Through the synergistic effect of polyvinylidene fluoride and carbon nanotubes, the dispersibility of the positive active material, polyvinylidene fluoride, and carbon nanotubes in the positive electrode composite material slurry is improved, so that uniform coating can be performed. In addition, polyvinylidene fluoride and carbon nanotubes are combined to improve the adhesion strength between the positive electrode active material and improve the electronic conductivity. Through these synergistic effects, the positive electrode and the battery can be made into low resistance. Even when the amount of polyvinylidene fluoride is small, this effect can be obtained by setting the number of polyvinylidene fluoride molecules contained per unit mass in the positive electrode mixture layer to be within a predetermined range.
[0014] Hereinafter, an example of an embodiment of the present disclosure is described in detail. In the present embodiment, a secondary battery 100 having a square metal outer casing 1 is illustrated, but the outer casing is not limited to a square shape, and may be, for example, a cylindrical shape. In addition, a wound electrode body 3 in which a positive electrode and a negative electrode are wound with the aid of a separator is illustrated, but it may also be a stacked electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one with the aid of a separator. The electrode body 3 is preferably a wound type. In addition, in both the positive electrode and the negative electrode, the case in which each composite material layer is formed on both sides of each core body is illustrated, but each composite material layer is not limited to being formed on both sides of each core body, and may also be formed on the surface of at least one of them.
[0015] like Figure 1As shown, the secondary battery 100 comprises: a wound electrode body 3 in which a positive electrode and a negative electrode are wound with a separator and formed into a flat shape having a flat portion and a pair of curved portions, an electrolyte, and an outer body 1 for accommodating the electrode body 3 and the electrolyte. The outer body 1 and the sealing plate 2 are both made of metal, preferably aluminum or an aluminum alloy.
[0016] The outer casing 1 has a bottom that is substantially rectangular when viewed from above, and a side wall portion that is erected on the periphery of the bottom. The side wall portion is formed to be perpendicular to the bottom. The size of the outer casing 1 is not particularly limited, and as an example, the horizontal length is 60 to 160 mm, the height is 60 to 100 mm, and the thickness is 10 to 40 mm.
[0017] The positive electrode is a strip having a positive electrode core body made of metal and positive electrode composite material layers formed on both sides of the core body, and a strip-shaped positive electrode core body exposed portion 4 is formed at one end of the positive electrode core body in the width direction and exposed in the length direction. Similarly, the negative electrode is a strip-shaped negative electrode core body exposed portion 5 is formed at one end of the negative electrode core body in the width direction and exposed in the length direction. The electrode body 3 has a structure in which the positive electrode and the negative electrode are wound with a separator, with the positive electrode core body exposed portion 4 of the positive electrode arranged at one end side in the axial direction and the negative electrode core body exposed portion 5 of the negative electrode arranged at the other end side in the axial direction.
[0018] The positive electrode collector 6 is connected to the laminated portion of the positive electrode core exposed portion 4 of the positive electrode, and the negative electrode collector 8 is connected to the laminated portion of the negative electrode core exposed portion 5 of the negative electrode. The ideal positive electrode collector 6 is made of aluminum or an aluminum alloy. The ideal negative electrode collector 8 is made of copper or a copper alloy. The positive terminal 7 has: a positive electrode external conductive portion 13 arranged on the battery external side of the sealing plate 2, a positive electrode bolt portion 14 connected to the positive electrode external conductive portion 13, and a positive electrode embedded portion 15 embedded in the through hole provided in the sealing plate 2, and electrically connected to the positive electrode collector 6. In addition, the negative terminal 9 has: a negative electrode external conductive portion 16 arranged on the battery external side of the sealing plate 2, a negative electrode bolt portion 17 connected to the negative electrode external conductive portion 16, and a negative electrode embedded portion 18 embedded in the through hole provided in the sealing plate 2, and electrically connected to the negative electrode collector 8.
[0019] The positive terminal 7 and the positive electrode collector 6 are fixed to the sealing plate 2 via an inner insulating member and an outer insulating member, respectively. The inner insulating member is disposed between the sealing plate 2 and the positive electrode collector 6, and the outer insulating member is disposed between the sealing plate 2 and the positive terminal 7. Similarly, the negative terminal 9 and the negative electrode collector 8 are fixed to the sealing plate 2 via an inner insulating member and an outer insulating member, respectively. The inner insulating member is disposed between the sealing plate 2 and the negative electrode collector 8, and the outer insulating member is disposed between the sealing plate 2 and the negative terminal 9.
[0020] The electrode body 3 is accommodated in the outer shell 1. The sealing plate 2 is connected to the opening edge of the outer shell 1 by laser welding or the like. The sealing plate 2 has an electrolyte injection hole 10, and after the electrolyte is injected into the outer shell 1, the electrolyte injection hole 10 is sealed by a sealing plug. The sealing plate 2 is formed with a gas discharge valve 11 for discharging gas when the pressure inside the battery reaches a predetermined value or more.
[0021] Hereinafter, the positive electrode, the negative electrode, the separator, and the non-aqueous electrolyte constituting the electrode body 3 , in particular, the positive electrode composite material layer constituting the positive electrode will be described in detail.
[0022] [positive electrode]
[0023] The positive electrode includes a positive electrode core and a positive electrode composite material layer formed on the surface of the positive electrode core. The positive electrode core can be made of a foil of a metal such as aluminum or aluminum alloy that is stable in the potential range of the positive electrode, with a thin film of the metal disposed on the surface.
[0024] The positive electrode composite material layer contains at least a positive electrode active material, carbon nanotubes (hereinafter, sometimes referred to as CNT) as a conductive auxiliary material, and polyvinylidene fluoride (hereinafter, sometimes referred to as PVdF) as a binding material. The positive electrode can be made as follows: a positive electrode composite material slurry containing a positive electrode active material, a conductive auxiliary material, and a binding material is applied to the positive electrode core, and the coating is dried and then compressed to form the positive electrode composite material layer on both sides of the positive electrode core. The thickness of the positive electrode composite material layer is, for example, 10 μm to 150 μm on one side of the positive electrode core.
[0025] The porosity of the positive electrode composite material layer is 23 volume % to 50 volume %. The porosity of the positive electrode composite material layer can be calculated by the volume density of the positive electrode composite material layer, the true density and content of each component such as the positive electrode active material, conductive auxiliary material, and binding material contained in the positive electrode composite material layer according to the following formula. By adjusting the compression rate of the positive electrode composite material layer, the volume density of the positive electrode composite material layer can be changed, so the porosity of the positive electrode composite material layer can be changed.
[0026] Porosity of positive electrode composite material layer = 1-(sum of (content / true density) of each component × volume density of positive electrode composite material layer)
[0027] Examples of the positive electrode active material contained in the positive electrode composite material layer include lithium transition metal oxides containing transition metal elements such as Co, Mn, and Ni. x CoO2、Li x NiO2、Li x MnO2、Li x Co y Ni 1-y O2、Li xCo y M 1-y O z , Li x Ni 1-y M y O z , Li x Mn2O4、Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F (M: at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0<x≤1.2, 0<y≤0.9, 2.0≤z≤2.3). These can be used alone or in combination. From the perspective of achieving a high capacity of a non-aqueous electrolyte secondary battery, the positive electrode active material preferably contains Li x NiO2、Li x Co y Ni 1-y O2、Li x Ni 1-y M y O z Lithium nickel composite oxides such as (M: at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B, 0<x≤1.2, 0<y≤0.9, 2.0≤z≤2.3).
[0028] The CNT included in the positive electrode composite material layer is a single-layer carbon nanotube (SWCNT) or a multilayer carbon nanotube (MWCNT). In addition, as MWCNT, for example, a CNT having a tubular structure formed by a graphene sheet formed by a carbon six-membered ring and wound parallel to the fiber axis, a CNT having a platelet structure formed by a graphene sheet formed by a carbon six-membered ring and arranged vertically relative to the fiber axis, and a CNT having a herringbone structure wound at an angle relative to the fiber axis by a graphene sheet formed by a carbon six-membered ring. In addition to CNT, as a conductive auxiliary material, carbon materials such as carbon black, acetylene black (AB), ketjen black, and graphite can also be included.
[0029] The particle size of CNT is 5nm to 40nm, and the aspect ratio is 100 to 1000. By satisfying this range, interaction with PVdF can be generated, so that the positive electrode and the battery can be made low-resistance. Here, for the particle size of CNT, a scanning electron microscope (hereinafter sometimes referred to as SEM) is used to measure the diameter of 10 CNTs and calculate based on their average value. In addition, for the length of CNT, the length of 10 CNTs is measured using SEM and calculated based on their average value. For example, CNT can be observed using SEM at an acceleration voltage of 5kV, and the diameter and length of any 10 CNTs are measured in a 50,000-fold image (number of pixels 1024×1280), and the particle size and length are calculated based on their average value. The aspect ratio is the value obtained by dividing the length by the particle size.
[0030] The content of CNT in the positive electrode composite material layer is 0.2% to 5% by mass, preferably 1.5% to 3% by mass. Within this range, the dispersibility of CNT in the positive electrode composite material slurry is improved, so a positive electrode and a battery with lower resistance can be obtained.
[0031] The number of PVdF molecules contained in the positive electrode composite material layer per unit mass is 0.005 to 0.030, preferably 0.007 to 0.011. By satisfying this range, an interaction with CNT is generated, and the positive electrode and the battery can be made low-resistance. Here, the number of PVdF molecules contained in the positive electrode composite material layer per unit mass refers to the value obtained by dividing the PVdF content (mass %) in the positive electrode composite material layer by the molecular weight (g / mole) of PVdF.
[0032] The content of polyvinylidene fluoride in the positive electrode composite material layer may be 0.3 mass % to 2.5 mass %, thereby obtaining a positive electrode and a battery with lower resistance.
[0033] The molecular weight of polyvinylidene fluoride can be 1.1 million to 1.4 million. Thus, a positive electrode and a battery with lower resistance can be obtained. In addition, in addition to PVdF, the positive electrode composite material layer may also contain fluororesins such as polytetrafluoroethylene (PTFE), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. as a binder. These resins can also be used in combination with carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), etc.
[0034] [negative electrode]
[0035] The negative electrode has a negative electrode core and a negative electrode composite material layer formed on the surface of the negative electrode core. The negative electrode core can use a foil of a metal such as copper or copper alloy that is stable within the potential range of the negative electrode, a thin film of the metal configured on the surface, etc. The negative electrode composite material layer contains a negative electrode active material and a binding material. The thickness of the negative electrode composite material layer is, for example, 10 μm to 150 μm on one side of the collector. The negative electrode can be made by coating a negative electrode composite material slurry containing a negative electrode active material, a binding material, etc. on the negative electrode core, drying the coating film, and then rolling it to form the negative electrode composite material layer on both sides of the negative electrode core.
[0036] As the negative electrode active material, there is no particular limitation as long as it can reversibly absorb and release lithium ions, and carbon materials such as graphite can usually be used. Graphite can be natural graphite such as flaky graphite, block graphite, and earthy graphite, block artificial graphite, and artificial graphite such as graphitized mesophase carbon microbeads. In addition, metals such as Si and Sn alloyed with Li, metal compounds containing Si, Sn, etc., lithium-titanium composite oxides, etc. can also be used as negative electrode active materials. For example, SiO x (0.5≤x≤1.6) represented by a Si-containing compound, or Li 2y SiO (2+y) A Si-containing compound in which Si fine particles are dispersed in a lithium silicate phase represented by (0<y<2) or the like can be used together with graphite.
[0037] The binding material included in the negative electrode composite material layer is the same as that of the positive electrode, and fluororesins such as PTFE and PVdF, PAN, polyimide, acrylic resin, polyolefin, etc. can be used, but styrene-butadiene rubber (SBR) is preferably used. In addition, the negative electrode composite material layer may also include CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc. For example, SBR, CMC or its salt may be included in the negative electrode composite material layer.
[0038] [Separator]
[0039] The separator can be a porous sheet with ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, non-woven fabrics, etc. As the material of the separator, polyolefins such as polyethylene and polypropylene, cellulose, etc. are ideal. The separator can be a single-layer structure or a laminated structure. In addition, the surface of the separator can also be provided with a resin layer with high heat resistance such as aramid resin, or a filler layer containing a filler of an inorganic compound.
[0040] [Non-aqueous electrolyte]
[0041] The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent can use, for example, esters, ethers, nitriles such as acetonitrile, formamides such as dimethylformamide, and mixed solvents of more than two of these. The non-aqueous solvent can also contain a halogen substituted product obtained by replacing at least a portion of the hydrogen of these solvents with a halogen atom such as fluorine. As the halogen substituted product, fluorinated cyclic carbonates such as fluorinated chain carbonates, fluorinated chain carboxylates such as fluoromethyl propionate (FMP), etc. can be cited.
[0042] Examples of the above-mentioned esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate, chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate, cyclic carboxylates such as γ-butyrolactone (GBL) and γ-valerolactone (GVL), and chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate.
[0043] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether. , dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether and other chain ethers, etc.
[0044] The electrolyte salt is preferably a lithium salt. Examples of lithium salts include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1<x<6, n is 1 or 2), LiB 10 Cl 10, LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, Li2B4O7, Li(B(C2O4)F2) and other borates, LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1 SO2) {l, m is an integer greater than 0} and other imide salts. As for the lithium salt, these can be used alone or in combination. Among these, LiPF6 is preferably used from the viewpoints of ion conductivity and electrochemical stability. The concentration of the lithium salt is, for example, 0.8 mol to 1.8 mol per 1L of the non-aqueous solvent.
[0045] <Example>
[0046] Hereinafter, the present disclosure will be further described by way of examples, but the present disclosure is not limited to these examples.
[0047] <Example 1>
[0048] [Production of positive electrode]
[0049] As the positive electrode active material, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A lithium transition metal oxide represented by O2. As a conductive auxiliary material, CNT (hereinafter referred to as CNT-A) having a particle size of 10 nm and an aspect ratio of 100 to 1000 is used. PVdF with a molecular weight of 1.1 million is used. The positive electrode active material, CNT, and PVdF are mixed in a mass ratio of 97.3:0.2:2.5, and N-methyl-2-pyrrolidone (NMP) is added while kneading to prepare a positive electrode composite material slurry. Next, leaving a portion connected to the positive electrode core lead formed by aluminum foil, the positive electrode composite material slurry is applied to both sides, and the coating is dried. Then, the coating is rolled with a roller in such a way that the porosity of the positive electrode composite material layer becomes 50% by volume, and then cut into a specified electrode size, thereby producing a positive electrode having a positive electrode composite material layer formed on both sides of the positive electrode core.
[0050] [Production of negative electrode]
[0051] Graphite, sodium salt of CMC, and dispersion of SBR as negative electrode active materials are mixed in a solid content mass ratio of 99 / 0.6 / 0.4, and water is added in an appropriate amount to prepare a negative electrode composite material slurry. Next, the negative electrode core formed by copper foil is left with a portion connected to the lead, and the negative electrode composite material slurry is applied to dry the coating. Then, the coating is rolled with a roller and cut into a specified electrode size to produce a negative electrode with a negative electrode composite material layer formed on both sides of the negative electrode core. The packing density of the negative electrode composite material layer is 1.17g / cm 3.
[0052] [Preparation of non-aqueous electrolyte]
[0053] A non-aqueous electrolyte was prepared by adding 1 part by mass of vinylene carbonate (VC) to 100 parts by mass of a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 25:35:40, and dissolving LiPF6 at a ratio of 1.15 mol / L.
[0054] [Production of test battery cells]
[0055] Leads were attached to the negative electrode and the positive electrode to produce a laminated electrode body in which each electrode was alternately laminated one by one with the aid of a separator. A single-layer polypropylene separator was used as the separator. The produced electrode body and the nonaqueous electrolyte were placed in a square battery case to produce a test battery cell.
[0056] [Measurement of composite material layer resistance and interface resistance]
[0057] The composite material layer resistance (Ω·cm) which is the resistance of the composite material layer as a whole and the interface resistance (Ω·cm) which is the resistance between the positive electrode core and the positive electrode composite material layer were measured for the positive electrode before being assembled into the test battery cell. 2 ). The increase in the resistance of the composite material layer and the increase in the interface resistance were calculated by subtracting the measurement result of the positive electrode prepared as described above from the measurement result of the positive electrode taken out after immersing the positive electrode in dimethyl carbonate (DMC) at 80°C for 18 hours. The composite material layer resistance and interface resistance were measured using an electrode resistance measuring device (device name: XF057) manufactured by Hioki Electric Co., Ltd.
[0058] [Evaluation of DC resistance]
[0059] The test battery cell was charged at a constant current of 0.3C at 25°C until the state of charge (SOC) reached 50%. After reaching SOC 50%, it was charged at a constant voltage until the current value reached 0.02C. After that, it was discharged at a constant current of 50C for 10 seconds. As shown in the following formula, the DC resistance was calculated by dividing the difference between the open circuit voltage (OCV) and the closed circuit voltage (CCV) after 10 seconds of discharge by the discharge current after 10 seconds of discharge.
[0060] DC resistance = [OCV-CCV (after 10 seconds of discharge)] / discharge current (after 10 seconds of discharge)
[0061] <Examples 2 to 14, Comparative Examples 1 to 21>
[0062] As shown in Tables 1 and 2, except for changing the content of the positive electrode active material, the type and content of the conductive auxiliary agent, the content and molecular weight of PVdF, and the porosity of the positive electrode composite material layer, the positive electrode and the test battery cell were prepared and evaluated in the same manner as in Example 1. It should be noted that the CNT-B of the conductive auxiliary material is a CNT with a particle size of 150 nm and an aspect ratio of 10 to 70.
[0063] Tables 1 and 2 summarize the results of the increase in resistance of the composite material layer, the increase in interface resistance, and the DC resistance of the embodiments and comparative examples. In addition, Tables 1 and 2 also record the composition of the positive electrode composite material layer formed by the positive electrode active material, the conductive auxiliary material, and the PVdF, and the porosity of the positive electrode composite material layer.
[0064] [Table 1]
[0065]
[0066] [Table 2]
[0067]
[0068] According to Tables 1 and 2, the positive electrodes and batteries of Examples 1 to 14 have lower resistance than Comparative Examples 1 to 21. In addition, in Examples 1 to 14, the content of the positive electrode active material in the positive electrode composite material layer is 90 mass % or more, and a high-capacity positive electrode and battery can be produced.
[0069] Description of Reference Numerals
[0070] 1 outer body
[0071] 2 Sealing plate
[0072] 3 Electrode body
[0073] 4. Positive electrode core exposed part
[0074] 5 Negative electrode core exposed part
[0075] 6. Positive electrode collector
[0076] 7 Positive terminal
[0077] 8 Negative electrode collector
[0078] 9 Negative terminal
[0079] 10 Electrolyte injection hole
[0080] 11 Gas exhaust valve
[0081] 13 Positive electrode external conductive part
[0082] 14 Positive electrode bolt
[0083] 15 Positive electrode embedding part
[0084] 16 Negative electrode external conductive part
[0085] 17 Negative electrode bolt
[0086] 18 Negative electrode embedding part
[0087] 100 Secondary batteries
Claims
1. A positive electrode for a non-aqueous electrolyte secondary battery, comprising a positive electrode core and a positive electrode composite material layer formed on the surface of the positive electrode core, The porosity of the positive electrode composite material layer is 31 volume % to 50 volume %, The positive electrode composite material layer at least comprises a positive electrode active material, carbon nanotubes as a conductive auxiliary material, and polyvinylidene fluoride as a binding material. The particle size of the carbon nanotubes is 5 nm to 40 nm, the aspect ratio is 100 to 1000, and the content of the carbon nanotubes in the positive electrode composite material layer is 0.2 mass % to 5 mass %. The number of polyvinylidene fluoride molecules contained in the positive electrode composite material layer per unit mass is 0.005 to 0.
030. The molecular weight of polyvinylidene fluoride is 1.1 million to 1.4 million.
2. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein The content of polyvinylidene fluoride in the positive electrode composite material layer is 0.3 mass % to 2.5 mass %. 3 . A non-aqueous electrolyte secondary battery comprising the positive electrode for a non-aqueous electrolyte secondary battery according to claim 1 , a negative electrode, and a non-aqueous electrolyte.