Hybrid metal halide luminescent material and preparation method and application thereof

By using hybrid metal halide materials containing organic matter and alkali metal ions containing heteroatom functional groups such as oxygen, nitrogen, phosphorus, sulfur, etc. in the field of X-ray imaging, the problems of toxicity, high detection limit and poor stability of existing materials are solved. New materials with excellent high-energy ray detection and imaging performance and multiple preparation methods have been realized.

CN114874767BActive Publication Date: 2024-10-29NANJING TECH UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210487457.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-06
Publication Date
2024-10-29
Estimated Expiration
2042-05-06

AI Technical Summary

Technical Problem

Existing materials in the field of X-ray imaging have problems such as high toxicity, high detection limit, poor stability, low luminous efficiency and harsh preparation conditions. It is difficult to realize non-toxic, low-cost, low detection limit and good stability metal halide scintillator. commercial applications.

Method used

Hybrid metal halide materials containing organic matter containing heteroatom functional groups such as oxygen, nitrogen, phosphorus, and sulfur combined with alkali metal ions are used to prepare crystals or films through solvent evaporation or anti-solvent assisted methods to achieve adjustable luminescence color and low-temperature preparation. and flexible applications.

Benefits of technology

A new hybrid metal halide luminescent material with excellent high-energy ray detection and imaging performance, low detection limit, adjustable luminescence color, and multiple preparation methods has been achieved. It has good environmental stability and efficient X-ray imaging capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114874767B_ABST
    Figure CN114874767B_ABST
Patent Text Reader

Abstract

The present invention discloses a hybrid metal halide luminescent material and a preparation method and application thereof. The general structural formula of the hybrid metal halide is A a B b C c X d , wherein A is an organic substance that can interact with alkali metal ions; B is an alkali metal ion; C is a metal cation; and X is a halogen anion. The preparation method of the luminescent crystal is to make raw materials A and B x X y and C x X y The precursor solution is dissolved in a good solvent, and then the hybrid metal halide crystal is obtained by solvent evaporation method or anti-solvent assisted method. The preparation method of the luminescent film is based on the precursor solution or the obtained crystal, and is prepared by spin coating, printing, scraping, pressing, melting and other methods. The obtained crystal or film has the advantages of adjustable luminescent color, flexible processing, low detection limit of high-energy rays (X-rays, α, β, γ rays, etc.), and high resolution of high-energy ray imaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention relates to hybrid metal halide materials, in particular to environmentally friendly copper, manganese, indium, zinc and other hybrid halide luminescent materials and their preparation methods and high-energy ray detection and imaging applications. Background technology:

[0002] In the field of X-ray imaging, traditional inorganic alkali metal halide scintillators (such as commercial CsI:Tl) have problems such as high toxicity and high detection limits, and usually require high-temperature preparation and are difficult to use in flexible devices (Nuclear Instruments and Methods in Physics Research Section A, 2021, 991, 164999). New organic long afterglow scintillators can be processed in solution, but have low luminescence efficiency, and the long luminescence lifetime easily leads to slow response speed of X-ray imaging (Nature Photonics 2021, 15, 187-192). In recent years, organic-inorganic lead-based halide materials have developed rapidly in the fields of photovoltaics, luminescence, and X-ray imaging due to their advantages of high absorption coefficient, high fluorescence quantum yield, high carrier mobility, low-temperature solution processing, and large-area flexible preparation (Advanced Materials 2018, 30, 1804771; Nature 2018, 562, 249; Advanced Materials 2018, 0, 1802110; Nature 2018, 561, 88-93). However, the toxicity and strong self-absorption properties of lead-based halides have greatly restricted their commercial prospects.

[0003] Currently, tin-based halides (C8H 17 NH3)2SnBr4 has no self-absorption phenomenon, but the material stability is poor (ACSApplied Materials&Interfaces 2020,12,19797); double perovskite Cs2Ag 0.6 Na 0.4 In 0.85 Bi 0.15Cl6 has a low detection limit, but the luminescent color is single, and it usually needs to be prepared under harsh conditions such as high temperature and high pressure (Light: Science & Applications 2020, 9, 112). Copper-based halides such as Cs3Cu2I5 and Rb2CuBr3 have high light yields, but the detection limit still needs to be improved (Advanced Science 2020, 7, 2000195; Adv. Mater. 2019, 31, 1904711). Therefore, it is urgent to develop new metal halide scintillator materials that have the advantages of non-toxicity, low cost, low detection limit, good stability, adjustable luminescent color, and easy and flexible preparation. Summary of the invention:

[0004] The purpose of the present invention is to overcome the above-mentioned shortcomings and provide a new hybrid metal halide luminescent material with good stability, low detection limit, adjustable luminescent color, diverse film preparation methods, excellent high-energy ray detection and imaging performance, and easy flexibility.

[0005] To achieve the above object, the technical solution of the present invention is as follows:

[0006] A hybrid metal halide luminescent material, the structural formula of the hybrid metal halide material is A a B b C c X d , wherein A is an organic substance that can interact with alkali metal ions; B is an alkali metal ion; C is a metal cation; X is a halogen anion; and the hybrid metal halide material is in the form of crystal or film.

[0007] The organic compound A capable of interacting with alkali metal ions is an organic molecule containing heteroatom functional groups such as oxygen, nitrogen, phosphorus, and sulfur, including alcohols (methanol, ethanol, propanol, isopropanol, butanol), aldehydes (formaldehyde, acetaldehyde, salicylaldehyde), ketones (acetone, cyclopentanone, etc.), ethers (12-crown-4, 15-crown-5, benzo-15-crown-5, dibenzo-15-crown-5, 18-crown-6, dibenzo-18-crown-6, dicyclohexane-18-crown-6, 21-crown-7, dibenzo-21- Crown ether-7, dicyclohexane 21-crown ether-7, 24-crown ether-8, dibenzo 24-crown ether-8, dicyclohexane 24-crown ether-8, dibenzo 30-crown ether-10, aza 18-crown ether-6, tetraethylene glycol dimethyl ether), acids (p-chlorobenzoic acid, 3-chlorobenzoic acid, 2-naphthoic acid, 1-methyl-2-pyrrolecarboxylic acid, 2-pyrrolecarboxylic acid, n-valeric acid, n-butyric acid, taurine, 2-aminoethanesulfonic acid, 4-bromobenzoic acid, glutaric acid, hexanoic acid, propylphosphonic acid, n-octanoic acid, isonicotinic acid, citric acid, tetrafluoroboric acid, oxalic acid, pyromellitic acid, benzoic acid, hypophosphorous acid, n-butylboric acid, benzenesulfonic acid, propionic acid, citric acid, benzenetricarboxylic acid), esters (formates, acetates, propionates, butyrates, valerates, acrylates, methacrylates), amino acids (tryptophan, phenylalanine, aminosulfonic acid, 7-aminoheptanoic acid, glycine, 3-aminopropane-1-phosphate, aminomethanesulfonic acid, glycine, 2-aminomethylphenylacetic acid, 3-(aminosulfonyl)propionic acid, N-acetyl-L-cysteine, 3-amino-4-hydroxybenzenesulfonic acid, 4-aminobutane-1-phosphate, p-aminobenzoic acid, 6-aminocaproic acid, EDTA, 3-aminopropanesulfonic acid, 2-amino-4-sulfobutyric acid, 2-aminoethanol hydrogen sulfate, N-(2-acetylamino)-3-aminoethanesulfonic acid, γ-aminobutyric acid, 5-aminovaleric acid, lysine, alanine, 5-hydroxytryptophan, cysteine), peroxides (peracetic acid, benzoyl peroxide), amines (1,5-dimethylhexylamine, dimethylamine, 1,8-octanediamine, m-toluidine, n-butylamine, 1,4-phenylenediamine, octylamine, One or more of 1,3-propylenediamine, 3-methylaminopropylamine, N-benzylethylenediamine, cyclohexylmethylamine, 5-aminopyrimidine, 9-aminoanthracene, 3-dimethylaminopropylamine, dicyclohexylcarbodiimide, N,N-dimethylethylenediamine, 1,6-hexanediamine, tert-octylamine, aniline, ethylamine, cyclooctylamine, tri(3,6-dioxaheptyl)amine, cup[4]pyrrole, etc.), amides (formamide, acetamide, sulfonamide), phosphine oxides (tributylphosphine oxide, trioctylphosphine oxide), sulfones (dimethyl sulfone, cyclopentane sulfone), and sulfoxides (dimethyl sulfoxide, methyl phenyl sulfoxide, diphenyl sulfoxide).

[0008] The most preferred organic matter that can interact with alkali metal ions is one or more of formic acid, acetic acid, ethyl acetate, ethyl butyrate, 15-crown-5, 18-crown-6, dimethyl sulfoxide, N,N-dimethylformamide, and methacrylate.

[0009] The alkali metal ions B include: Li + 、Na + , K + , Rb + , Cs + ;

[0010] Metal cations C include: Cu + , Cu 2+ Sn 2+ Sn 4+ , Mn 2+ 、In 3+ 、Zn 2+ etc.; the halogen anion X includes: I – Br – , Cl – 、F - .

[0011] The preparation method of the hybrid metal halide luminescent crystal comprises the following steps:

[0012] 1) Raw materials A and B x X y and C x X y The precursor solution is obtained by dissolving in a good solvent in a molar ratio of 2-6:2-4:1-2; wherein A and B x X y and C x X y The sum of the masses of the precursor solution accounts for 10-50% of the total mass;

[0013] 2) The metal halide crystals are obtained by solvent evaporation method or anti-solvent assisted method, wherein the anti-solvent assisted method refers to slowly diffusing the anti-solvent into the precursor solution or dropping the precursor solution into the anti-solvent.

[0014] The good solvent includes formamide, N,N'-dimethylformamide, dimethyl sulfoxide, tetramethylene sulfoxide, 1,3-dimethylpropylene urea, γ-butyrolactone, N-alkyl pyrrolidone, acetonitrile, dichloromethane, methanol, ethanol, isopropanol, butanol or any mixture thereof in any proportion; preferably, the good solvent is N,N'-dimethylformamide, dimethyl sulfoxide, acetonitrile;

[0015] The anti-solvent includes: one of ether, toluene, chlorobenzene, methanol, chloroform, formates, acetates, propionates, butyrates, valerates, acrylates, methacrylates, dichloromethane, petroleum ether or any mixture thereof. The preferred anti-solvent is toluene, chlorobenzene, or ether.

[0016] The preparation temperature in step 2) is 0-100°C.

[0017] The preparation method of the hybrid metal halide luminescent film is to prepare raw materials A and B x X y and C x X y The precursor solution is dissolved in a good solvent at a molar ratio of 2-6:2-4:1-2, and a rigid luminescent film is prepared on a rigid substrate by a low-temperature solution method, or a flexible luminescent film is prepared on a flexible substrate by a low-temperature solution method. The low-temperature solution method includes a spin coating method, a printing method, and the like.

[0018] The details are as follows: The first method for preparing the hybrid metal halide luminescent film is to deposit the precursor solution onto a suitable substrate by spin coating, printing or the like to obtain a rigid or flexible luminescent film; the precursor solution is raw materials A and B x X y and C x X y Dissolved in a good solvent at a molar ratio of 2-6:2-4:1-2.

[0019] The spin coating speed in the spin coating method is 500-8000 rpm / s, the spin coating time is 10-60s, the annealing temperature is 20-130°C, and the annealing time is 0.1-8h;

[0020] The viscosity of the precursor solution in the printing method is 0.1-5 mPa·s, and the annealing temperature is 20-100°C.

[0021] The second method for preparing the hybrid metal halide luminescent film is as follows: firstly, the hybrid metal halide crystal is ground into powder, then mixed with polymer additive and solvent, and finally the mixture is scraped onto a rigid or flexible substrate to obtain a luminescent film. The mass ratio of the crystal powder to the polymer additive is 5%-80%; the distance between the scraper and the substrate during scraping is 0.01-10mm, and the size of the prepared film is 0.5-100cm.

[0022] The third method for preparing the hybrid metal halide luminescent film is as follows: firstly, the hybrid metal halide crystals are ground into powders, and then the powders are pressed into sheet-like films by a tablet press in the presence or absence of polymer additives.

[0023] The fourth method for preparing the hybrid metal halide luminescent film is as follows: firstly, the hybrid metal halide crystals are ground into powder, and then a luminescent film is obtained on a rigid substrate by a melting method.

[0024] The melting temperature is 100-200°C, the melting time is 0.5-10min, and the cooling rate is 5-50°C / min;

[0025] The rigid substrate includes ordinary glass, quartz glass, conductive glass (ITO, FTO), silicon wafer, metal (Au, Al, Ag), etc., and the flexible substrate includes polyethylene terephthalate (PET), polyvinyl chloride (PVC), polyvinyl alcohol (PVA), polyimide (PI), polyethylene naphthalate (PEN), paper, textile materials, etc.

[0026] The polymer additives include polyvinylidene fluoride (PVDF), polydimethylsiloxane (PDMS), polyvinyl pyrrolidone (PVP), polymethyl methacrylate (PMMA), polyethylene glycol (PEG), polystyrene (PS) and the like.

[0027] The above hybrid metal halide crystal is prepared by the following method: 1) raw materials A and B x X y and C x X y The precursor solution is obtained by dissolving in a good solvent according to a molar ratio of 2-6:2-4:1-2; 2) obtaining metal halide crystals by solvent volatilization method or anti-solvent assisted method; wherein the anti-solvent assisted method refers to slowly diffusing the anti-solvent into the precursor solution or dropping the precursor solution into the anti-solvent.

[0028] Preferred hybrid metal halide precursor B x X y , C x X y and organic matter A are dissolved in a good solvent at a mass fraction of 40% for the preparation of crystals.

[0029] Preferred hybrid metal halide precursor C x X y Cesium iodide or cesium bromide, B x X y It is cuprous iodide or manganese bromide, and the organic substance A is 15-crown-5 or 18-crown-6.

[0030] Preferably, cesium iodide, cuprous iodide and 15-crown-5 are dissolved in DMF at a molar ratio of 2:2:2, and a room temperature solvent volatilization method or an anti-solvent assisted method is used to obtain a crystal with white light emission; a molar ratio of 2:2:4, 2:2:6 or 3:2:6 is dissolved in DMF, and a room temperature solvent volatilization method or an anti-solvent assisted method is used to obtain a crystal with red light emission. Cesium iodide, cuprous iodide and 18-crown-6 are dissolved in DMF at a molar ratio of 2:2:2, and a solvent assisted method is used to obtain a crystal with blue light emission; a molar ratio of 2:2:2 is dissolved in acetonitrile, and an anti-solvent assisted method is used to obtain a crystal with orange-red light emission; a molar ratio of 2:2:3, 2:2:6 or 3:2:6 is dissolved in DMF, and a room temperature solvent volatilization method or a solvent diffusion method is used to obtain a crystal with blue-green light emission. Cesium bromide, manganese bromide and 18-crown ether-6 are dissolved in DMF at a molar ratio of 1:1:2, 2:1:2 or 2:1:4, and a crystal with green light emission can be obtained by using an anti-solvent-assisted method. Preferably, a metal halide precursor solution with a mass fraction of 15% can be prepared at room temperature by spin coating, printing and other methods to obtain a luminescent film.

[0031] The preparation principle of the above crystals and films is based on the self-assembly behavior of ions in solution. In the solution, cesium ions combine with crown ethers in a coordinated form, and at the same time, based on Coulomb interactions, they self-assemble with copper halide anion clusters to obtain a series of hybrid metal halide crystals or films with adjustable luminescent colors. The advantage of this method is that the tolerance of the raw material ratio is very large, and it is easy to obtain the expected pure phase crystals or films. However, under conditions beyond the above precursor ratio range, such as C x X y When the molar ratio of C:A is greater than 1:1, the luminescent material with the expected structure cannot be obtained. x X y When the molar ratio of :A is less than 1:3, by-products are easily generated while the expected material is formed.

[0032] Preferably, the crystal powder and the polymer are uniformly mixed in a mass ratio of 1:1 or 2:3, and then a wet film is obtained by a doctor blade method. Next, the film is vacuumed for 45 minutes at room temperature to remove bubbles in the film, and finally dried at 110° C. for 2 hours to obtain a luminescent film.

[0033] Preferably, 200 mg of the crystal powder is placed on a glass substrate preheated to 185° C., and immediately cooled to room temperature after melting for 10 seconds to obtain a luminescent film.

[0034] Preferably, 100 mg of crystal powder is placed in a tablet press and pressed for 15 min under a pressure of 15 MPa to obtain a circular flake with a diameter of 3 cm and a thickness of 100 μm. The hybrid metal halide luminescent crystal or film can be applied to X-ray imaging.

[0035] The hybrid metal halide luminescent material of the present invention can be used in high-energy ray detection and imaging, wherein the high-energy rays include α, β, γ and X-rays. The specific method of X-ray imaging is to place the object to be detected between the X-ray source and the scintillator, and then use a CCD camera on the other side of the scintillator to capture the imaging result of the object to be detected. The application fields of X-ray imaging of this material include medicine, pharmacy, industry, agriculture, national defense, aerospace, jewelry, archaeology, etc.

[0036] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0037] 1. A new hybrid metal halide crystal structure is formed by introducing organic matter containing specific functional groups. Compared with the inorganic metal halide Cs3Cu2I5 crystal, it has better environmental stability.

[0038] 2. The luminescent color of the material of the present invention is adjustable.

[0039] 3. The material of the present invention can be prepared into thin films through various methods and can be made flexible.

[0040] 4. The material of the present invention has excellent high-energy ray detection and imaging capabilities: low detection limit, high imaging resolution, and flexible and large-area preparation. Description of the drawings:

[0041] Figure 1 Crystalline diagram of Cs2(18C6)3-[Cu2I4]

[0042] Figure 2 Schematic diagram of the crystal structure of Cs2(18C6)3-[Cu2I4]

[0043] Figure 3 Photoluminescence spectrum (PL) of Cs2(18C6)3-[Cu2I4] crystal

[0044] Figure 4 Photoexcitation spectra (PLE) of Cs2(18C6)3-[Cu2I4] crystals at different wavelengths

[0045] Figure 5 Thermogravimetric analysis and differential scanning calorimetry analysis curves of Cs2(18C6)3-[Cu2I4] crystals

[0046] Figure 6 The upper part is the X-ray diffraction pattern of Cs2(18C6)3-[Cu2I4] crystal. Figure 6 The lower part is the X-ray diffraction pattern of Cs2(15C5)4-[Cu2I4] crystal

[0047] Figure 7The light intensity-dependent fluorescence emission spectrum of Cs2(18C6)3-[Cu2I4] crystal

[0048] Figure 8 Transient fluorescence spectrum of Cs2(18C6)3-[Cu2I4] crystal

[0049] Fig. 9 This is the fluorescence quantum efficiency diagram of Cs2(18C6)3-[Cu2I4] crystal

[0050] Fig.10 C s2 Emission spectrum of (18C6)3-[Cu2I4] crystal under X-ray irradiation

[0051] Fig.11 Absorption spectrum of Cs2(18C6)3-[Cu2I4] crystal in the photon energy range

[0052] Fig.12 This is the X-ray photoelectron spectrum of Cs2(18C6)3-[Cu2I4] crystal

[0053] Fig.13 Dose rate diagram of Cs2(18C6)3-[Cu2I4] crystal excited by X-ray

[0054] Fig.14 Photostability of Cs2(18C6)3-[Cu2I4] crystals subjected to repeated cycles of X-ray excitation at 50 kV with a time interval of 5 s

[0055] Fig.15 Crystalline diagram of Cs2(15C5)4-[Cu2I4]

[0056] Fig.16 Schematic diagram of the crystal structure of Cs2(15C5)4-[Cu2I4]

[0057] Fig.17 Photoluminescence spectrum of Cs2(15C5)4-[Cu2I4] crystal

[0058] Fig.18 Photoexcitation spectra of Cs2(15C5)4-[Cu2I4] crystal at different wavelengths

[0059] Fig.19 Thermogravimetric analysis and differential scanning calorimetry curves of Cs2(15C5)4-[Cu2I4] crystals

[0060] Fig. 20 The light intensity-dependent fluorescence emission spectrum of Cs2(15C5)4-[Cu2I4] crystal

[0061] Fig.21 Transient fluorescence spectrum of Cs2(15C5)4-[Cu2I4] crystal

[0062] Fig. 22 This is the fluorescence emission spectrum of Cs2(15C5)4-[Cu2I4] crystal under X-ray irradiation

[0063] Fig.23 Crystalline diagram of Cs2(18C6)2-[MnBr4]

[0064] Fig.24 Schematic diagram of the crystal structure of Cs2(18C6)2-[MnBr4]

[0065] Fig.25 Photoemission spectrum of Cs2(18C6)2-[MnBr4] crystal

[0066] Fig.26 Photoexcitation spectra of Cs2(18C6)2-[MnBr4] crystal at different wavelengths

[0067] Fig. 27 X-ray diffraction pattern of Cs2(18C6)2-[MnBr4] crystal

[0068] Fig.28 This is the fluorescence emission spectrum of Cs2(18C6)2-[MnBr4] crystal under X-ray irradiation

[0069] Fig.29 Shown is the photostability of Cs2(18C6)3-[MnBr4] subjected to repeated cycles of X-ray excitation at 50 kV with a time interval of 5 s.

[0070] Fig.30 Photoemission spectrum of the crystal prepared when the ratio exceeds the optimal range

[0071] Fig.31 Photoemission spectrum of the crystals prepared when the solvent is out of the optimal range

[0072] Fig.32 Schematic diagram of Cs2(18C6)3-[Cu2I4] flexible film under 302nm UV light

[0073] Fig.33 The imaging results of Cs2(18C6)3-[Cu2I4] flexible film under X-ray

[0074] Fig.34 The calculated results of the resolution test of the prepared Cs2(18C6)3-[Cu2I4] flexible film under X-ray

[0075] Fig.35 Schematic diagram of Cs2(18C6)3-[Cu2I4] molten film under 302nm UV lamp

[0076] Fig.36 The imaging result of Cs2(18C6)3-[Cu2I4] molten film under X-ray

[0077] Fig.37 Schematic diagram of Cs2(18C6)3-[Cu2I4] pressed film under 302nm UV lamp

[0078] Fig.38 Schematic diagram of Cs2(18C6)3-[Cu2I4] spin-coated film under 302nm UV lamp Specific implementation method:

[0079] The present invention is explained below by means of specific embodiments:

[0080] Example 1

[0081] 1. The preparation process of Cs2(18C6)3-[Cu2I4] crystal is as follows:

[0082] (1) Solvent evaporation method: Cesium iodide, cuprous iodide, and 18-crown-6 were dissolved in N,N'-dimethylformamide at a molar ratio of 3:2:6 and a mass fraction of 40%, and stirred for one day to form a clear solution. The solution was filtered with a 0.22 μm filter head and placed in a natural environment to evaporate the solvent. Block crystals were precipitated after one day, and the resulting crystals were rinsed with ether several times and finally vacuum dried at 40°C for 6 hours.

[0083] (2) Anti-solvent assisted method 1: Cesium iodide, cuprous iodide, and 18-crown ether-6 are dissolved in N,N'-dimethylformamide at a molar ratio of 3:2:6 and a mass fraction of 40% to prepare a 1 mL solution. Stir for one day to form a clear solution. Filter the solution with a 0.22 μm filter and place it in a 1.5 mL vial. Then take 2 mL of ether and place it in a 20 mL large bottle, and place the 1.5 mL vial containing the precursor solution in a 20 mL large bottle. Tighten the lid and place it in a cool and dry place. After standing for 2 days, block crystals will precipitate. Finally, rinse the resulting crystals with ether several times and vacuum dry them at 40°C for 6 hours.

[0084] (3) Anti-solvent assisted method 2: Cesium iodide, cuprous iodide, and 18-crown ether-6 are dissolved in N,N'-dimethylformamide at a molar ratio of 3:2:6 and a mass fraction of 40% to prepare a 3 mL precursor solution. Stir for one day to form a clear solution. Filter the solution with a 0.22 μm filter and place it in a 4 mL vial. Then take 10 mL of ether / ethyl acetate and place it in a conical flask and stir it continuously with a magnetic bar. Take the precursor solution with a rubber-tipped dropper and slowly drop it into the conical flask stirred with a magnetic bar to precipitate small crystals and fully disperse them in the solvent. Then take the precipitated small crystals in a test tube and centrifuge them, pour off the supernatant, and leave the precipitate. Finally, the precipitate is vacuum dried at 70°C for 1 hour to obtain dry solid small crystals.

[0085] 2. Conventional characterization of Cs2(18C6)3-[Cu2I4] crystals

[0086] like Figure 1 This is a crystal diagram of Cs2(18C6)3-[Cu2I4].

[0087] like Figure 2 This is a schematic diagram of the crystal structure of Cs2(18C6)3-[Cu2I4]. It can be seen that the internal structure of the crystal is arranged periodically and the crystal structure is stable.

[0088] like Figure 3 This is the photoluminescence spectrum (PL) of Cs2(18C6)3-[Cu2I4] crystal, with an obvious emission peak at 488nm.

[0089] like Figure 4 The photoexcitation spectra (PLE) of Cs2(18C6)3-[Cu2I4] crystals at different wavelengths show that light of different emission wavelengths all come from the same exciton absorption and have a large Stokes shift, indicating that its possible luminescence mechanism is derived from the self-trapped state.

[0090] like Figure 5 The thermogravimetric analysis and differential scanning calorimetry analysis curves of Cs2(18C6)3-[Cu2I4] crystals show that the melting point of Cs2(18C6)3-[Cu2I4] crystals is 185°C, which is relatively low, indicating that the material can be melted into film.

[0091] like Figure 6 This is the X-ray diffraction pattern of Cs2(18C6)3-[Cu2I4] crystal. It can be seen that the X-ray diffraction peak signal of Cs2(18C6)3-[Cu2I4] crystal is obvious and corresponds well to the simulated XRD signal, indicating that the crystal purity is high.

[0092] like Figure 7This is the light intensity-dependent fluorescence emission spectrum of Cs2(18C6)3-[Cu2I4] crystal. It can be seen that the fluorescence intensity of Cs2(18C6)3-[Cu2I4] crystal increases with the increase of excitation light intensity, indicating that its luminescence is not permanent defect luminescence.

[0093] like Figure 8 This is the transient fluorescence spectrum of Cs2(18C6)3-[Cu2I4] crystal. It can be seen that the lifetime of Cs2(18C6)3-[Cu2I4] crystal is 1.82μs.

[0094] like Fig. 9 This is the fluorescence quantum efficiency diagram of Cs2(18C6)3-[Cu2I4] crystal. It can be seen that the PLQY of Cs2(18C6)3-[Cu2I4] crystal is 96.81%.

[0095] like Fig.10 This is the fluorescence emission spectrum (RL) of Cs2(18C6)3-[Cu2I4] crystal under X-ray irradiation. It can be seen that the highest point of RL intensity of Cs2(18C6)3-[Cu2I4] crystal is at 492nm, and its RL is almost consistent with PL spectrum.

[0096] like Fig.11 This is the absorption spectrum of Cs2(18C6)3-[Cu2I4] crystal within the photon energy range. It can be seen that Cs2(18C6)3-[Cu2I4] crystal has strong absorption under X-ray.

[0097] like Fig.12 This is the X-ray photoelectron spectrum of Cs2(18C6)3-[Cu2I4] crystal. It shows that the light emission peak is mainly caused by I 3d, Cs 3d and Cu 2p.

[0098] like Fig.13 The dose rate diagram of Cs2(18C6)3-[Cu2I4] crystal excited by X-rays. The radiation luminescence curve measured at different dose rates is shown. When the signal-to-noise ratio is 3, the slope of the fitting line gives a minimum detection limit of 28.3nGy s -1 .

[0099] like Fig.14 This is the photostability spectrum of Cs2(18C6)3-[Cu2I4] crystal under X-ray excitation. After 120 consecutive cycles, it was found that its intensity hardly decreased, indicating its good stability under X-ray.

[0100] Example 2

[0101] 1. The preparation process of Cs2(15C5)4-[Cu2I4] crystal is as follows:

[0102] 1) Solvent evaporation method: Cesium iodide, cuprous iodide, and 15-crown ether-5 were dissolved in N,N'-dimethylformamide at a molar ratio of 3:2:6 and a mass fraction of 40%, and stirred for one day to form a clear solution. The solution was filtered with a 0.22 μm filter head and placed in a natural environment to evaporate the solvent. Block crystals were precipitated after one day, and the obtained crystals were washed with ether several times and finally vacuum dried at 40°C for 6 hours.

[0103] (2) Anti-solvent assisted method 1: Cesium iodide, cuprous iodide, and 15-crown ether-5 are dissolved in N,N'-dimethylformamide at a molar ratio of 3:2:6 and a mass fraction of 40% to prepare a 1 mL solution. Stir for one day to form a clear solution. Filter the solution with a 0.22 μm filter and place it in a 1.5 mL vial. Then take 2 mL of ether and place it in a 20 mL large bottle, and place the 1.5 mL vial containing the precursor solution in a 20 mL large bottle. Tighten the lid and place it in a cool and dry place. After standing for 2 days, block crystals will precipitate. Finally, rinse the resulting crystals with ether several times and vacuum dry them at 40°C for 6 hours.

[0104] (3) Anti-solvent assisted method 2: Cesium iodide, cuprous iodide, and 15-crown ether-5 are dissolved in N,N'-dimethylformamide at a molar ratio of 3:2:6 and a mass fraction of 40% to prepare a 3mL precursor solution. Stir for one day to form a clear solution. Filter the solution with a 0.22μm filter and place it in a 4mL vial. Then take 10mL of ether / ethyl acetate and place it in a conical flask and stir it continuously with a magnetic bar. Use a rubber-tipped dropper to take the precursor solution and slowly add it dropwise into the conical flask stirred with a magnetic bar to precipitate small crystals and fully disperse them in the solvent. Then use a test tube to take the precipitated small crystals and centrifuge them. Pour out the supernatant and leave the precipitate. Finally, place the precipitate under vacuum and dry it at 70°C for 1 hour to obtain dry solid small crystals.

[0105] 2. Conventional characterization of Cs2(15C5)4-[Cu2I4]

[0106] like Fig.15 This is a schematic diagram of the crystal structure of Cs2(15C5)4-[Cu2I4]. It can be seen that the internal structure of the crystal is arranged periodically and the crystal structure is stable.

[0107] like Fig.16 Schematic diagram of the crystal structure of Cs2(15C5)4-[Cu2I4].

[0108] like Fig.17 This is the photoluminescence spectrum (PL) of Cs2(15C5)4-[Cu2I4] crystal, with an obvious emission peak at 702nm.

[0109] like Fig.18 The photoexcitation spectra (PLE) of Cs2(15C5)4-[Cu2I4] crystals at different wavelengths show that light of different emission wavelengths all come from the same exciton absorption and have a large Stokes shift, indicating that its possible luminescence mechanism is derived from the self-trapped state.

[0110] like Fig.19 The thermogravimetric analysis and differential scanning calorimetry analysis curves of Cs2(15C5)4-[Cu2I4] crystals show that the melting point of Cs2(15C5)4-[Cu2I4] crystals is 153°C.

[0111] like Figure 6 The lower part is the X-ray diffraction spectrum of Cs2(15C5)4-[Cu2I4] crystal. It can be seen that the X-ray diffraction peak signal of Cs2(15C5)4-[Cu2I4] crystal is obvious and has a good correspondence with the simulated XRD signal, indicating that the crystal purity is high. Fig. 20 This is the light intensity-dependent fluorescence emission spectrum of Cs2(15C5)4-[Cu2I4] crystal. It can be seen that the fluorescence intensity of Cs2(15C5)4-[Cu2I4] crystal increases with the increase of excitation light intensity, indicating that its luminescence is not permanent defect luminescence.

[0112] like Fig.21 This is the transient fluorescence spectrum of Cs2(15C5)4-[Cu2I4] crystal. It can be seen that the lifetime of Cs2(15C5)4-[Cu2I4] crystal is 7.69μs.

[0113] like Fig. 22 This is the fluorescence emission spectrum of Cs2(15C5)4-[Cu2I4] crystal under X-ray irradiation.

[0114] Example 3

[0115] 1. The preparation process of Cs2(18C6)2-[MnBr4] crystal is as follows:

[0116] Antisolvent-assisted method: Cesium bromide, manganese bromide, and 18-crown ether-6 are dissolved in N,N'-dimethylformamide at a molar ratio of 2:1:2 and a mass fraction of 40% to form a 1mL solution. Stir for one day to form a clear solution. Filter the solution with a 0.22μm filter and place it in a 1.5mL vial. Then take 2mL of ether and place it in a 20mL large bottle, and place the 1.5mL vial containing the precursor solution in a 20mL large bottle, tighten the lid and place it in a cool and dry place. After standing for 1 day, block crystals will precipitate. Finally, rinse the resulting crystals with ether several times and vacuum dry them at 40°C for 6 hours.

[0117] 2. Conventional characterization of Cs2(18C6)2-[MnBr4]

[0118] like Fig.23 This is a crystal diagram of Cs2(18C6)2-[MnBr4].

[0119] like Fig.24 This is a schematic diagram of the crystal structure of Cs2(18C6)2-[MnBr4]. It can be seen that the internal structure of the crystal is arranged periodically and the crystal structure is stable.

[0120] like Fig.25 This is the photoemission spectrum (PL) of Cs2(18C6)2-[MnBr4] crystal, with an obvious emission peak at 510nm.

[0121] like Fig.26 The photoexcitation spectra (PLE) of Cs2(18C6)2-[MnBr4] crystals at different wavelengths.

[0122] like Fig. 27 This is the X-ray diffraction pattern of Cs2(18C6)2-[MnBr4] crystal. It can be seen that the X-ray diffraction peak signal of Cs2(18C6)2-[MnBr4] crystal is obvious and corresponds well with the simulated XRD signal, indicating that the crystal purity is high.

[0123] like Fig.28 This is the fluorescence emission spectrum of Cs2(18C6)2-[MnBr4] under X-ray irradiation.

[0124] like Fig.29 The photostability of Cs2(18C6)2-[MnBr4] under X-ray excitation at 50 kV with repeated cycles at 5 s intervals. The intensity hardly decreased after 120 cycles, indicating its good stability under X-rays.

[0125] Example 4

[0126] 1. Crystals prepared with a ratio exceeding the optimal range

[0127] Solvent evaporation method: Cesium iodide, cuprous iodide, and 15-crown ether-5 are dissolved in N, N'-dimethylformamide at a molar ratio of 1:2:2 and a mass fraction of 40%, stirred for one day to form a clear solution, filtered with a 0.22μm filter head, and placed in a natural environment to evaporate the solvent. Block crystals precipitated after 1 day, and the resulting crystals were rinsed with ether several times, and finally vacuum dried at 40°C for 6 hours. The obtained crystals were taken to test PL and found that the maximum PL peak was at 573nm, which was consistent with the luminescence of pure CsCu2I3, indicating that pure inorganic crystals were obtained, rather than what we call hybrid non-metallic halides.

[0128] 2. Conventional Characterization of the Crystals of This Example

[0129] Fig.30 This is the PL spectrum of the crystal prepared in this example.

[0130] Example 5

[0131] Solvent evaporation method: Cesium iodide, cuprous iodide, and 18-crown ether-6 are dissolved in water at a molar ratio of 3:2:6 and a mass fraction of 40%. There are a lot of solids in the solution, which are filtered. When the ultraviolet lamp is used at 302nm, there is obvious yellow light. The obtained powder is taken to test PL and it is found that its PL peak maximum is at 572nm, which is consistent with the luminescence of pure CsCu2I3, indicating that pure inorganic crystals are obtained, rather than the hybrid non-metallic halide we mentioned.

[0132] Conventional Characterization of Crystals in This Example Fig.31 This is the PL spectrum of the crystals prepared when the solvent exceeds the optimal range.

[0133] Example 6

[0134] 1. Preparation of scintillator flexible thin film (taking Cs2(18C6)3-[Cu2I4] as an example)

[0135] Cesium iodide, cuprous iodide, and 18-crown ether-6 were dissolved in N,N'-dimethylformamide in a molar ratio of 3:2:6 and a mass fraction of 40%, stirred for one day to form a clear solution, and single crystals were grown by the solvent evaporation method in Example 1. Cs2(18C6)3-[Cu2I4] crystals were placed in an ethyl acetate solution and stirred until all the crystals turned into powder, and then the powder was dried. The dried powder was stirred and mixed with a toluene solution of polymethyl methacrylate (crystal powder: PMMA=1:1) to form a colloid, and then the uniformly mixed solid particle solution was placed in a film mold and slowly evaporated for 8 hours at room temperature to solidify it into a flexible film.

[0136] 2. Conventional characterization of Cs2(18C6)3-[Cu2I4] flexible films

[0137] Fig.32 This is a schematic diagram of the Cs2(18C6)3-[Cu2I4] flexible film under a 302nm ultraviolet lamp. It can be seen that the film is uniform and flat, emits light evenly and can be flexibly bent.

[0138] Fig.33 This is the imaging result of the prepared Cs2(18C6)3-[Cu2I4] flexible film under X-ray.

[0139] Fig.34The resolution of the prepared Cs2(18C6)3-[Cu2I4] flexible film under X-ray was calculated and the resolution was about 16lp mm -1 .

[0140] Example 7

[0141] 1. Preparation of scintillator melt film (taking Cs2(18C6)3-[Cu2I4] as an example)

[0142] Cesium iodide, cuprous iodide, and 18-crown-6 were dissolved in N,N'-dimethylformamide at a molar ratio of 3:2:6 and a mass fraction of 40%, and stirred for one day to form a clear solution, and a single crystal was grown by the solvent evaporation method in Example 1. Cs2(18C6)3-[Cu2I4] crystals were ground into powder, 200 mg of the powder was evenly spread on a glass sheet, and placed on a 185°C hot table to melt the crystal powder instantly, and the molten crystals were quickly transferred to a cold iron block to be rapidly cooled to a solidified state, and finally a molten film of Cs2(18C6)3-[Cu2I4] was obtained.

[0143] 2. Conventional characterization of Cs2(18C6)3-[Cu2I4] molten films

[0144] like Fig.35 Schematic diagram of Cs2(18C6)3-[Cu2I4] molten film under 302nm UV lamp.

[0145] like Fig.36 This is the imaging result of Cs2(18C6)3-[Cu2I4] molten film under X-ray.

[0146] Example 8

[0147] 1. Preparation of scintillator pressed film (taking Cs2(18C6)3-[Cu2I4] as an example)

[0148] Cesium iodide, cuprous iodide, and 18-crown-6 were dissolved in N,N'-dimethylformamide at a molar ratio of 3:2:6 and a mass fraction of 40%, stirred for one day to form a clear solution, and a single crystal was grown by the room temperature reagent volatilization method in Example 1. Cs2(18C6)3-[Cu2I4] crystals were ground into powder, and the powder was placed on a sieve with an aperture of 0.1 mm for screening to obtain crystal powders with a size of less than 0.1 mm. 100 mg of the evenly ground powder was placed in a tableting mold, and pressed for 15 minutes under a pressure of 15 MPa to finally obtain a scintillator circular sheet with a diameter of 3 cm and a thickness of 100 μm.

[0149] 2. Conventional characterization of Cs2(18C6)3-[Cu2I4] thin films

[0150] Fig.37 This is a schematic diagram of Cs2(18C6)3-[Cu2I4] thin film under 302nm ultraviolet lamp. It can be seen that the film is uniform and flat, and the light emission is uniform.

[0151] Example 9

[0152] 1. Preparation of scintillator spin-coated thin films (taking Cs2(18C6)3-[Cu2I4] as an example)

[0153] Cesium iodide, cuprous iodide, and 18-crown ether-6 were dissolved in N,N'-dimethylformamide at a molar ratio of 2:2:3 and a mass fraction of 14% to prepare a 1 mL precursor solution, and stirred at room temperature for one day to form a clear solution. The cleaned glass / quartz sheet was placed on a coater, and 30 μL of the solution was dropped on the glass / quartz sheet using a pipette. The coater speed was set to 4000 rpm / s, and the rotation time was 30 s. In-situ spin coating was performed to finally obtain a uniform film.

[0154] 2. Conventional characterization of Cs2(18C6)3-[Cu2I4] spin-coated films

[0155] Fig.38 This is a schematic diagram of the Cs2(18C6)3-[Cu2I4] spin-coated film under a 302nm UV lamp. It can be seen that the film is uniform and flat.

Claims

1. A hybrid metal halide luminescent material for high-energy ray detection and imaging, characterized in that: The general structural formula of the hybrid metal halide material is A a B b C c X d ; Wherein, A is one or more of formic acid, acetic acid, ethyl acetate, ethyl butyrate, 15-crown-5, 18-crown-6, dimethyl sulfoxide, N,N-dimethylformamide, and methacrylate; B is Li + 、Na + , K + , Rb + , Cs + One or more of; C is Cu + , Cu 2+ Sn 2+ Sn 4+ , Mn 2+ 、In 3+ 、Zn 2+ One or more of; X is 1 - Br - , Cl - 、F - One or more of; the hybrid metal halide material is Cs2(18C6)3-[Cu2I4], Cs2(15C5)4-[Cu2I4] or Cs2(18C6)2-[MnBr4] luminescent crystal; The crystal preparation method comprises the following steps: 1) Raw materials A and B x X y and C x X y The precursor solution is obtained by dissolving in a good solvent in a molar ratio of 2-6:2-4:1-2; wherein A and B x X y and C x X y The sum of the masses of the precursor solution accounts for 10-50% of the total mass of the precursor solution; the good solvent is formamide, N,N'-dimethylformamide, dimethyl sulfoxide, tetramethylene sulfoxide, 1,3-dimethylpropylene urea, γ-butyrolactone, N-alkyl pyrrolidone, acetonitrile, dichloromethane, methanol, ethanol, isopropanol, butanol or any mixture thereof in any proportion; 2) Obtaining metal halide crystals by solvent volatilization method or anti-solvent assisted method; wherein the anti-solvent assisted method refers to slowly diffusing the anti-solvent into the precursor solution or dropping the precursor solution into the anti-solvent; the anti-solvent is one of ether, toluene, chlorobenzene, methanol, chloroform, formates, acetates, propionates, butyrates, valerates, acrylates, methacrylates, dichloromethane or any mixture thereof in any proportion.

2. A method for preparing a hybrid metal halide luminescent film using the metal halide crystal according to claim 1, characterized in that: The hybrid metal halide crystal is ground into powder, then mixed with polymer additives and solvent, and finally the mixture is scraped onto a rigid or flexible substrate to obtain a luminescent film; the hybrid metal halide crystal is prepared by the following method: 1) raw materials A and B x X y and C x X y The precursor solution is obtained by dissolving in a good solvent according to a molar ratio of 2-6:2-4:1-2; 2) obtaining metal halide crystals by solvent volatilization method or anti-solvent assisted method; wherein the anti-solvent assisted method refers to slowly diffusing the anti-solvent into the precursor solution or dropping the precursor solution into the anti-solvent.

3. The method for preparing a hybrid metal halide thin film from a metal halide crystal according to claim 2, characterized in that: The polymer additives include polyvinylidene fluoride, polydimethylsiloxane, polyvinyl pyrrolidone, polymethyl methacrylate, polyethylene glycol, and polystyrene; the solvents include formamide, N,N'-dimethylformamide, dimethyl sulfoxide, tetramethylene sulfoxide, 1,3-dimethylpropyleneurea, γ-butyrolactone, N-alkylpyrrolidone, acetonitrile, dichloromethane, methanol, ethanol, isopropanol, butanol, or any mixture thereof in any proportion; the mass ratio of the crystal powder to the polymer additive is 5%-80%; the distance between the scraper and the substrate during scraping is 0.01-10mm, and the size of the prepared film is 0.5-100cm.

4. A method for preparing a hybrid metal halide luminescent film using the metal halide crystal according to claim 1, characterized in that: The hybrid metal halide crystals are ground into powder, and the powder is pressed into a sheet-like film by a tablet press; or the hybrid metal halide crystals are ground into powder, and the powder is pressed into a sheet-like film by a tablet press under the condition of a polymer additive; the hybrid metal halide crystals are prepared by the following method: 1) raw materials A and B x X y and C x X y The precursor solution is obtained by dissolving in a good solvent according to a molar ratio of 2-6:2-4:1-2; 2) obtaining a metal halide crystal by a solvent volatilization method or an anti-solvent assisted method; wherein the anti-solvent assisted method refers to slowly diffusing the anti-solvent into the precursor solution or dripping the precursor solution into the anti-solvent; the metal halide crystal is ground into powder with a particle size of 10nm-50μm; the pressure applied by the tablet press is 5-35MPa for 1-30min; the sheet film has a size of 1-15cm and a thickness of 100-1000μm; the polymer additive includes polyvinylidene fluoride, polydimethylsiloxane, polyvinyl pyrrolidone, polymethyl methacrylate, polyethylene glycol, and polystyrene.

5. A method for preparing a hybrid metal halide luminescent film using the metal halide crystal according to claim 1, characterized in that: The hybrid metal halide crystal is ground into powder, and a light-emitting film is obtained on a rigid substrate by a melting method; the hybrid metal halide crystal is prepared by the following method: 1) raw materials A and B x X y and C x X y The precursor solution is obtained by dissolving it in a good solvent in a molar ratio of 2-6:2-4:1-2; 2) obtaining a metal halide crystal by a solvent volatilization method or an anti-solvent assisted method; wherein the anti-solvent assisted method refers to slowly diffusing the anti-solvent into the precursor solution or dripping the precursor solution into the anti-solvent; wherein the melting temperature is 100-200°C, the melting time is 0.5-10min; the cooling rate is 5-50°C / min; the rigid substrate includes ordinary glass, quartz glass, conductive glass, silicon wafer, and metal; the flexible substrate includes polyethylene terephthalate, polyvinyl chloride, polyvinyl alcohol, polyimide, polyethylene naphthalate, paper, and textile materials.

6. Use of the hybrid metal halide luminescent single crystal according to claim 1 in high-energy ray detection and imaging.

7. The use according to claim 6, wherein the high-energy rays are X-rays, α, β, or γ rays.

Citation Information

Patent Citations

  • Metal halide perovskite materials, preparation method thereof as well as solar cell device and preparation method of solar cell device

    CN109912458A

  • Germanium-based perovskite photoelectric material, application, preparation method, device and device preparation method

    CN112993198A

  • Lead-free metal halide luminescent material, and preparation method and device thereof

    CN113388385A