A resistive memory and a method for preparing the same
By forming MoS2-xOx compounds in the two-dimensional semiconductor material MoS2 and controlling the migration of oxygen ions using Ti and Au contact electrodes, a resistive memory with high switching ratio and good retention performance is achieved, and the device preparation in the prior art is solved The undefinite issue of stability and resistance change effects improves the performance and application prospects of memory.
Patent Information
- Application Number
- CN202210285359.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-03-23
AI Technical Summary
The existing two-dimensional material resistance memory has instability in the device preparation process, and the resistance effect mechanism is not determined, which affects its high-density, low-energy consumption, and high-speed storage performance in practical applications.
The two-dimensional semiconductor material MoS2 annealed in oxygen to form the MoS2-xOx compound, and the interface resistance effect is formed under specific annealing conditions. Ti and Au are used as contact electrodes to control the migration of oxygen ions through applied voltage to achieve a reversible resistance switching effect. .
It achieves high switching ratio and good retention performance, improves the preparation stability and integration of the device, has broad application prospects, and obtains high-quality two-dimensional materials through mechanical peeling methods.
Smart Images

Figure CN114883484B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of two-dimensional material devices and relates to a device based on the material MoS 2-x O x A resistive random access memory and a preparation method thereof. Background Art
[0002] With the continuous progress of semiconductor memory, devices are getting smaller and smaller, and mainstream flash memory will inevitably have leakage current, floating gate coupling, crosstalk between adjacent cells, etc. As a new type of non-volatile storage technology, resistive random access memory is expected to become the next generation of high-density, low-energy, and high-speed storage devices. Resistive random access memory is essentially an electrical switch. The principle is that some thin film materials will show a difference in high and low resistance under the action of electrical stimulation, and the change of high and low resistance values replaces the "0" and "1" in binary to store data.
[0003] Since the first two-dimensional material graphene was exfoliated in 2004, two-dimensional materials have made great progress. Two-dimensional materials have the characteristics of strong in-plane chemical bonds and weak coupling between layers. It is precisely because of this characteristic that two-dimensional materials can be easily separated into a few atomic layers. Its thickness is usually only a single layer or a few atomic layers thick, which means that it has an ultra-high surface area ratio. This characteristic makes their band structure very sensitive to external perturbations, which is in sharp contrast to the properties of bulk materials.
[0004] Even though many two-dimensional materials have been used in resistive memory, the mechanism of the resistive effect has not yet been determined and the device preparation process is unstable, so resistive devices are still a long way from practical application. Summary of the invention
[0005] Purpose: In order to overcome the deficiencies in the prior art, the present invention provides a material based on MoS 2-x O x A resistive random access memory and a preparation method thereof.
[0006] In the present invention, the two-dimensional semiconductor material MoS2 is selected. After annealing in oxygen, the MoS2 thin layer can be further formed into a MoS with excellent resistance switching characteristics. 2-x O x compounds, which is due to the lower barrier energy of oxygen ions in MoS 2-x O x The present invention found that under certain annealing conditions, MoS 2-x O x As the resistive switching layer becomes thicker, an interface resistive switching effect will appear, and it will exhibit high switching ratio, high retention and durability performance.
[0007] Technical solution: To solve the above technical problems, the preferred technical solution adopted by the present invention is:
[0008] In a first aspect, a method for preparing a resistive random access memory is provided, comprising:
[0009] Step S1: preparing the bottom electrode
[0010] SiO2 / Si silicon wafer is used as substrate, and the SiO2 / Si silicon wafer is adsorbed on a coating machine, methyl methacrylate MMA EL6 glue is spin-coated and dried, and then polymethyl methacrylate PMMA A5 electron beam photoresist is spin-coated and dried;
[0011] A bottom electrode pattern and a mark for positioning the top electrode are drawn on the silicon wafer after the glue coating, and exposure, development, fixing, electron beam evaporation and stripping are performed in sequence to obtain a silicon wafer with a bottom electrode, wherein the electron beam evaporation comprises: in an electron beam cavity of an electron beam evaporation system, the cavity is evacuated to a vacuum of 10 -4 Below the Pa level, first evaporate titanium Ti as an adhesion layer, and then evaporate gold Au;
[0012] Step S2: Preparation of MoS 2-x O x Layer, where x is greater than 0 and less than 2;
[0013] Prepare a two-dimensional material MoS2 layer, and transfer the MoS2 layer to the bottom electrode prepared in step S1 using a transfer platform to obtain a silicon wafer with a bottom electrode and MoS2;
[0014] The silicon wafer with the bottom electrode and MoS2 is placed in a tube furnace for oxidation annealing to obtain a silicon wafer with the bottom electrode and MoS2. 2-x O x Silicon wafers;
[0015] Step S3: preparing the top electrode
[0016] The bottom electrode and MoS 2-x O x The silicon wafer is adsorbed on a coating machine, methyl methacrylate MMA EL6 glue is spin-coated and dried, and then polymethyl methacrylate PMMA A5 electron beam photoresist is spin-coated and dried;
[0017] According to the label and MoS 2-x O x The top electrode pattern is drawn on the silicon wafer after the glue coating, and exposure, development and fixing, electron beam evaporation and stripping are performed in sequence, wherein the electron beam evaporation comprises: in the electron beam cavity of the electron beam evaporation system, and the cavity is vacuumed to 10 -4 Below the Pa level, metal titanium Ti is first evaporated as an adhesion layer, and then gold Au is evaporated.
[0018] In some embodiments, in step S1 / S3, spin coating methyl methacrylate MMA EL6 glue includes: dropping methyl methacrylate MMA EL6 glue on the silicon wafer substrate, setting 4500 rad / min to rotate on a glue spreader for 45 seconds, and baking on a heating table after completion.
[0019] In some embodiments, in step S1 / S3, spin coating polymethyl methacrylate PMMA A5 electron beam photoresist includes: dripping polymethyl methacrylate PMMA A5 electron beam photoresist, setting two speeds for uniform coating, first setting 4500 rad / min to rotate for 30 seconds, then setting 7000 rad / min to rotate for 8 seconds, and then baking on a heating table.
[0020] Furthermore, baking on a heating table includes: the temperature of the heating table is 120° C., and baking for 2 minutes.
[0021] In some embodiments, in step S1, the thickness of the evaporated titanium Ti is 2 nm, and the thickness of the evaporated gold Au is 15 nm. In step S3, the thickness of the evaporated titanium Ti is 5 nm, and the thickness of the evaporated gold Au is 30 nm.
[0022] In some embodiments, in step S1 / S3, the rate of evaporating Ti is The rate of Au evaporation is
[0023] In some embodiments, in step S1 / S3, developing and fixing includes: the developing solution is MIBK (methyl isobutyl ketone): IPA (isopropyl alcohol) in a volume ratio of 1:3, the sample is gently clamped with tweezers and completely immersed in the developing solution and shaken;
[0024] Preferably, the developing time is 40 seconds, and after the developing is completed, the film is placed in isopropyl alcohol for fixing for 20 seconds.
[0025] The auxiliary peeling tool is polydimethylsiloxane (PDMS).
[0026] In some embodiments, the total thickness of the SiO2 / Si silicon wafer is 500±15 μm, and the thickness of the SiO2 oxide layer is 285 nm;
[0027] In some embodiments, MoS 2-x O x The thickness of the layer was 6.5 nm.
[0028] In some embodiments, in step S2, the oxidation annealing conditions are in an oxygen environment, with a pressure of about 1 kPa, a temperature of 200° C., and maintaining for 90 minutes.
[0029] The structural formula of the polymer polymethyl methacrylate (PMMA) is:
[0030]
[0031] The structural formula of polymer methyl methacrylate (MMA) is:
[0032]
[0033] Wherein, the above n is a positive integer.
[0034] The structure of the two-dimensional material 2H-MoS2 is:
[0035]
[0036] In a second aspect, a resistive random access memory is provided, wherein the resistive random access memory is prepared by the preparation method, and comprises a SiO2 / Si silicon wafer, a Ti / Au bottom electrode layer, a MoS 2-x O x layer, Ti / Au top electrode layer.
[0037] Beneficial effects:
[0038] (1) The present invention uses Ti as the top contact electrode and metal Au as the bottom contact electrode. Au / Ti / MoS is produced using micro-nano processing technology. 2-x O x / Au device. By applying an external voltage, an oxygen-rich layer is formed between Ti and the resistive switching layer, and the device changes from a low-resistance state to a high-resistance state. When a reverse voltage is applied, the oxygen in the oxygen-rich layer returns to its initial state, and the device changes from a high-resistance state to a low-resistance state. This reversible oxidation process can achieve a more practical and effective resistance switching effect by controlling the content of the metal / oxide interface, and has broad application prospects in resistance switching memory devices.
[0039] (2) The device structure and preparation process are relatively simple, which greatly improves the fault tolerance in the device preparation process and is conducive to device integration.
[0040] (3) In the process flow of the present invention, a mechanical exfoliation method is used to obtain the two-dimensional material, and the overall quality of the material obtained directly from the two-dimensional material crystal is relatively high.
[0041] (4) MoS, the core sample of the device 2-x O x Has good chemical stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1is a schematic diagram of a device structure according to an embodiment of the present invention;
[0043] Figure 2 A schematic diagram of the device preparation process for the embodiment;
[0044] Figure 3 It is a top view of the device and a test schematic diagram;
[0045] Figure 4 The following is a picture of the device of the embodiment under an optical microscope;
[0046] Figure 5 The resistive switching characteristic IV curve of the device of the embodiment shows the cycles from the 1st to the 150th cycle. DETAILED DESCRIPTION
[0047] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0048] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0049] For the purpose of this specification and the appended claims, unless otherwise stated, all numbers expressing amounts, percentages or ratios and other numerical values used in this specification and the appended claims are understood to be modified in all cases by the term "about". In addition, all ranges disclosed herein are inclusive and independently combinable.
[0050] Example 1
[0051] like Figure 1 , Figure 2 As shown, a material based on MoS 2-x O x The resistive random access memory of the present invention comprises the following steps:
[0052] Phase One: Preliminary preparations.
[0053] Step 1: Prepare clean SiO2 / Si (silicon wafer), the total thickness of SiO2 / Si silicon wafer is 500±15μm, and the thickness of SiO2 oxide layer is 285nm. Place the cut SiO2 / Si (silicon wafer) substrate in acetone, ethanol, and deionized water in turn, and clean it in an ultrasonic cleaner for 2 minutes, with an ultrasonic power of 90W, and blow dry with a nitrogen gun. (Acetone is used to wash away pollutants such as grease debris on the silicon wafer, ethanol is used to remove residual acetone, and deionized water is used to remove residual ethanol.)
[0054] Step 2: Prepare MoS2 blocks and tools such as tweezers and glass slides.
[0055] Stage 2: Preparation of bottom electrode and marking
[0056] The third step: adsorb the clean silicon wafer on the glue machine for glue throwing operation. The present invention adopts a double-layer glue process, which is as follows: first, use a disposable dropper to drop methyl methacrylate (MMA EL6) glue on the silicon wafer, set 4500rad / min to rotate on the glue machine for 45s, and then bake on the heating table for 2min. Then drip polymethyl methacrylate (PMMA A5) electron beam photoresist, and set two speeds for this glue throwing. First, set 4500rad / min to rotate for 30s, and then set 7000rad / min to rotate for 8s. After that, bake on the heating table. The temperature of the heating table is 120℃ and baked for 2min. The low speed is to completely cover the surface of the substrate with the photoresist first, and the high speed is to get rid of the excess photoresist on the substrate surface. The solvent in the photoresist evaporates during centrifugation, and a uniform film is formed under the action of surface tension. Use DrawBeam software to draw the bottom electrode design pattern and at least three "+" shaped marks, and then use electron-beam lithography (EBL) system's electron beam chamber to reduce the vacuum in the chamber to 10 -6 Below the Pa level; after exposure, development and fixing are performed.
[0057] Step 3: Place the silicon wafer prepared in the previous step in the electron beam chamber of the electron beam evaporation (EBE) system and evacuate the chamber to 10 -4 Below the Pa level. First, titanium (Ti) was evaporated with EBE as an adhesion layer with a thickness of 2nm, and then gold (Au) was evaporated with a thickness of 15nm. Here, the bottom electrode that is as thin as possible while ensuring the passage of current is conducive to a smoother two-dimensional material, so the top electrode has better contact. Finally, the sample with a metal electrode was obtained by soaking in acetone for stripping.
[0058] Stage 3: Preparation of thin layers of two-dimensional materials.
[0059] Step 4: Use tape to mechanically peel off to obtain MoS2 flakes on SiO2 / Si (silicon wafer).
[0060] Step 5: Transfer the obtained MoS2 to the prepared bottom electrode using a transfer platform, paying attention to alignment.
[0061] Stage 4: Preparation of MoS 2-x O x
[0062] Step 6: Place the silicon wafer with the bottom electrode and MoS2 into a tube furnace for oxidation annealing to obtain MoS 2- x O x The oxidation annealing conditions are in an oxygen environment, with a pressure of about 1 kPa, a temperature of 200 °C, and a holding time of 90 min. 2-x O x The thickness of the layer was 6.5 nm.
[0063] Stage 5: Preparation of top electrode.
[0064] Step 7: Place the MoS 2-x O x The silicon wafer is adsorbed on the coating machine, and the double-layer coating process is also used. The specific steps are the same as the second step above. The design of the top electrode requires a 20x image under a light microscope. The sample and the mark are displayed in the same image. The top electrode is designed according to the light microscope image. It should be noted that the pixel size in the instrument matches the actual size. Finally, the exposure is completed and the image is fixed.
[0065] Step 8: Place the silicon wafer prepared in the previous step in the electron beam chamber of the electron beam evaporation (EBE) system and evacuate the chamber to 10 -4 Below Pa level. First, metal titanium (Ti) is evaporated with EBE as an adhesion layer with a thickness of 5nm, and then gold (Au) is evaporated with a thickness of 30nm. At this time, the metal Ti is used as a contact electrode in the device. Finally, it is immersed in acetone for stripping to obtain a sample with a metal electrode, which is our target device.
[0066] Stage 6: Conduct electrical transport measurements on the finished device to determine device performance.
[0067] Figure 1 , Figure 3 The device adopts a "sandwich" structure, with the upper contact electrode being metal Ti and the lower electrode being metal Au. The test adopts a two-terminal method, that is, disconnecting the top electrode and connecting the other end to the bottom electrode. Figure 4 Shown, scale bar is 10 μm. Figure 5 The device has been tested for more than 300 cycles, fully demonstrating its cyclability. The device has a durability in which the ratio of high resistance to low resistance remains at 10 within the 300 cycles tested. 3 The device's practicality is greatly enhanced. The retention characteristics of the device prepared by the method of the present invention can be determined by the length of time the device can maintain a high resistance or low resistance state for a long time.
[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a resistive random access memory, characterized in that: include: Step S1: preparing the bottom electrode SiO2 / Si silicon wafer is used as substrate, the SiO2 / Si silicon wafer is adsorbed on a coating machine, methyl methacrylate MMAEL6 glue is spin-coated and dried, and then polymethyl methacrylate PMMA A5 electron beam photoresist is spin-coated and dried; The bottom electrode pattern and the mark for positioning the top electrode are drawn on the silicon wafer after the glue coating, and exposure, development and fixing, electron beam evaporation and stripping are performed in sequence to obtain the silicon wafer with the bottom electrode, wherein the electron beam evaporation includes: in the electron beam cavity of the electron beam evaporation system, the cavity is vacuumed to 10 -4 Below the Pa level, first evaporate titanium Ti as an adhesion layer, and then evaporate gold Au; Step S2: Preparation of MoS 2-x O x Layer, where x Greater than 0 and less than 2; Prepare a two-dimensional material MoS2 layer, and transfer the MoS2 layer to the bottom electrode prepared in step S1 using a transfer platform to obtain a silicon wafer with a bottom electrode and MoS2; The silicon wafer with the bottom electrode and MoS2 is placed in a tube furnace for oxidation annealing to obtain a silicon wafer with the bottom electrode and MoS2. 2- x O x Silicon wafers; Step S3: preparing the top electrode The bottom electrode and MoS 2-x O x The silicon wafer is adsorbed on a coating machine, methyl methacrylate MMAEL6 glue is spin-coated and dried, and then polymethyl methacrylate PMMA A5 electron beam photoresist is spin-coated and dried; According to the label and MoS 2-x O x The top electrode pattern is drawn on the silicon wafer after the glue coating, and exposure, development and fixing, electron beam evaporation and stripping are performed in sequence, wherein the electron beam evaporation includes: in the electron beam cavity of the electron beam evaporation system, and the cavity is vacuumed to 10 -4 Below the Pa level, first evaporate titanium Ti as an adhesion layer, and then evaporate gold Au; In step S1 / S3, spin coating methyl methacrylate MMA EL6 glue includes: dropping methyl methacrylate MMA EL6 glue on the silicon wafer substrate, rotating on a glue spreader at 4500 rad / min for 45 seconds, and baking on a heating table after completion; In step S1 / S3, spin coating PMMA A5 electron beam photoresist includes: dripping PMMA A5 electron beam photoresist, setting two speeds for coating, first setting 4500 rad / min for 30 seconds, then setting 7000 rad / min for 8 seconds, and baking on a heating table after completion.
2. The preparation method according to claim 1, characterized in that: Baking on the heating table includes: the heating table temperature is 120° C., and baking is 2 minutes.
3. The preparation method according to claim 1, characterized in that: In step S1, the vapor deposition thickness of the metal titanium Ti is 2 nm, and the vapor deposition thickness of the gold Au is 15 nm.
4. The preparation method according to claim 1, characterized in that: In step S3, the vapor deposition thickness of the metal titanium Ti is 5 nm, and the vapor deposition thickness of the gold Au is 30 nm.
5. The preparation method according to claim 1, characterized in that: In step S1 / S3, the rate of evaporation of Ti is 0.2Å / s, and the rate of evaporation of Au is 0.4Å / s.
6. The preparation method according to claim 1, characterized in that: In step S1 / S3, the developing and fixing process includes: the developing solution is methyl isobutyl ketone:isopropyl alcohol in a volume ratio of 1:3, the sample is gently clamped with tweezers and completely immersed in the developing solution and shaken; The developing time was 40 s, and after development, the film was placed in isopropanol for fixing for 20 s.
7. The preparation method according to claim 1, characterized in that: The total thickness of SiO2 / Si wafer is 500±15μm, and the thickness of SiO2 oxide layer is 285nm; and / or, MoS 2-x O x The thickness of the layer was 6.5 nm.
8. The preparation method according to claim 1, characterized in that: In step S2, the oxidation annealing conditions are in an oxygen environment, with a gas pressure of 1 kPa, a temperature of 200° C., and maintaining for 90 minutes.
9. A resistive random access memory, characterized in that: The resistive random access memory is manufactured by the manufacturing method according to any one of claims 1 to 8.