A kind of hydrogen separation palladium membrane pipe fitting and preparation method thereof

By applying microcrystalline glass layer, active metal layer and loaded palladium alloy film on porous ceramic loaded palladium membrane tube and using metal connectors, the problem of poor airtightness of traditional porous ceramic loaded palladium membrane tube is solved, achieving higher The airtightness and reliability improve the application performance of hydrogen-separated palladium membrane tubes.

CN114906810BActive Publication Date: 2024-11-19GRIMAT ENG INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110174241.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-09
Publication Date
2024-11-19
Estimated Expiration
2041-02-09

AI Technical Summary

Technical Problem

Traditional porous ceramic loaded palladium membrane tubes have problems such as poor airtightness and low sealing connection reliability, which limits their application performance in the hydrogen separation and purification process.

Method used

The structure of a porous ceramic pipe fitting is adopted, wherein the outer surface of the open end of the porous ceramic pipe is coated with a microcrystalline glass layer and an active metal layer, and a loaded palladium alloy film is arranged on the part of the uncoated microcrystalline glass layer, combined with the metal connection, through Heat treatment improves airtightness and connection reliability.

Benefits of technology

It significantly improves the air tightness of porous ceramic loaded palladium membrane tube and the reliability during thermal cycling, and improves the application performance of hydrogen-separated palladium membrane tube.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114906810B_ABST
    Figure CN114906810B_ABST
Patent Text Reader

Abstract

The present invention relates to a hydrogen separation palladium membrane pipe fitting and a preparation method thereof, and belongs to the field of hydrogen separation and purification. The pipe fitting comprises a porous ceramic tube and a metal connector. The outer surface of the open end of the porous ceramic tube is provided with a microcrystalline glass coating and an active metal coating from the inside to the outside. The length of the active metal coating is less than the length of the microcrystalline glass coating. The outer surface of the porous ceramic tube without the microcrystalline glass coating and the outer surface of the part of the microcrystalline glass coating adjacent thereto are provided with a loaded palladium alloy membrane. It is prepared by applying a microcrystalline glass coating, performing a primary heat treatment, preparing a loaded palladium alloy membrane, applying an active metal coating, assembling, and performing a secondary heat treatment. The hydrogen separation palladium membrane pipe fitting of the present invention can effectively solve the problem of air tightness of the end of the porous ceramic loaded palladium membrane tube, ensure the reliability of the thermal cycle process of the membrane tube, and significantly improve the application performance of the hydrogen separation palladium membrane tube.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a hydrogen separation palladium membrane pipe fitting and a preparation method thereof. The hydrogen separation palladium membrane pipe fitting can effectively solve the problems of poor air tightness and poor reliability in the sealing connection of a traditional porous ceramic-loaded palladium membrane pipe, is conducive to realizing reliable connection of the pipe fitting, and belongs to the field of hydrogen separation and purification. Background Art

[0002] The separation and purification of hydrogen is an important part of the hydrogen preparation and application process. Palladium membranes have excellent selective permeability to hydrogen and can be used in hydrogen separation processes in electronics, hydrogen isotope processing, fusion reactors, petrochemicals and other fields. Traditional palladium membrane tubes are mainly cold-rolled or drawn palladium tubes. The palladium membrane is thick, costly and has low hydrogen permeability, which greatly limits the application of palladium membranes. Due to process limitations, it is difficult to further reduce the thickness of traditional palladium membrane tubes. In recent years, the research and development of porous carrier-loaded palladium membranes has made significant progress. The palladium membrane is supported by a porous carrier, and the thickness of the membrane layer can be greatly reduced, thereby significantly improving the hydrogen permeation efficiency and reducing costs.

[0003] The supporting materials of the palladium membrane loaded on a porous carrier mainly include porous glass, porous ceramics and porous metals. Porous glass has a large pore size and poor high-temperature stability, and is rarely used as a palladium membrane carrier. Porous metal has the advantage of reliable sealing connection as a palladium membrane carrier, but its main problem is that the porous metal and the palladium membrane are prone to elemental interdiffusion, resulting in poor high-temperature stability of the palladium membrane. Porous ceramic materials have the characteristics of high-temperature stability, corrosion resistance, and small pore size, and are the most widely used palladium membrane carrier materials. Porous ceramic-loaded palladium membrane tubes generally use graphite sealing rings or rubber sealing rings to achieve sealed connections. The sealing material has poor temperature resistance and air leakage caused by poor matching, which greatly limits the application of porous ceramic-loaded palladium membrane tubes. Summary of the invention

[0004] The purpose of the present invention is to provide a palladium membrane pipe fitting that can achieve reliable connection, so as to solve the problems of poor air tightness and low sealing connection reliability of porous ceramic-loaded palladium membrane tubes, thereby improving the performance and reliability of the palladium membrane pipe fitting during actual use.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A hydrogen separation palladium membrane pipe fitting comprises a porous ceramic tube and a metal connector, etc. The outer surface of the open end of the porous ceramic tube is provided with a microcrystalline glass coating and an active metal coating from the inside to the outside, the length of the active metal coating is shorter than the length of the microcrystalline glass coating, and the outer surface of the porous ceramic tube not provided with the microcrystalline glass coating and the outer surface of the part of the microcrystalline glass coating adjacent to the porous ceramic tube are provided with a loaded palladium alloy membrane.

[0007] The structure of the porous ceramic tube is a one-end sealed and the other end through tube (open) structure or a two-end through tube (open) structure, preferably a one-end sealed and the other end through tube structure; the material of the porous ceramic tube is alumina or zirconia.

[0008] The outer diameter of the porous ceramic tube is 8-50 mm, and the length is 100-1500 mm.

[0009] The outer surface of the open end of the porous ceramic tube is coated with a glass-ceramic coating with a thickness of 20-200 microns. The glass-ceramic coating material is silicon oxide-aluminum oxide-based glass-ceramic, and the coating heat treatment temperature is 900-1400°C.

[0010] An active metal coating (or active alloy coating) is coated on the microcrystalline glass coating at the open end of the porous ceramic tube, the effective length covered by the active metal coating is smaller than the microcrystalline glass coating, and the active metal coating is not coated on a portion of the microcrystalline glass coating away from the open end of the porous ceramic tube. The thickness of the active metal coating is 20-200 microns.

[0011] The material of the active metal coating is a titanium-silver-copper alloy, including but not limited to AgCuTi4.5, AgCuTi2, AgCuTi6, etc.

[0012] The components of the supported palladium alloy film include but are not limited to Pd-Ag, Pd-Y, Pd-Au, Pd-Cu, Pd-Pt, Pd-Ru, Pd-Ag-Cu, Pd-Ni-Au, etc. The thickness of the supported palladium alloy film is 0.5-20 μm.

[0013] The effective length of the loaded palladium alloy membrane should ensure that it covers a portion of the microcrystalline glass coating and has no contact with the active metal coating.

[0014] The metal connector is installed at the open end of the porous ceramic tube, and the material of the metal connector is iron-cobalt-nickel Kovar alloy.

[0015] Another object of the present invention is to provide a method for preparing a palladium membrane tube that can achieve reliable connection. The method has simple process steps and a high yield rate, and can obtain a porous ceramic-loaded palladium membrane tube with good performance and reliability.

[0016] A method for preparing a hydrogen separation palladium membrane pipe comprises the following steps:

[0017] (1) Applying a glass-ceramic coating: applying a glass-ceramic coating on the outer surface of the end (including all ends) of the open end of the porous ceramic tube by a dipping and pulling method;

[0018] (2) performing a heat treatment: performing a heat treatment on the porous ceramic tube coated with the microcrystalline glass coating to form a dense microcrystalline glass coating at the end of the open end of the porous ceramic tube;

[0019] (3) preparing a loaded palladium alloy membrane: using a chemical plating process, plating a loaded palladium alloy membrane on the outer surface of the porous ceramic tube that is not coated with the microcrystalline glass coating and on the outer surface of a portion of the microcrystalline glass coating adjacent thereto;

[0020] (4) applying an active metal coating: applying an active metal coating on the glass-ceramic coating at the end of the open end of the porous ceramic tube by an immersion pulling method, wherein the active metal coating has no contact with the loaded palladium alloy membrane;

[0021] (5) Assembling and performing secondary heat treatment: Assembling a metal connector at the end of the open end of the porous ceramic tube, performing secondary heat treatment, and obtaining a porous hydrogen separation palladium membrane tube with good airtightness.

[0022] In step (1), the structure of the porous ceramic tube is a one-end sealed and one-end open tube structure or a two-end open tube structure, preferably a one-end sealed and one-end open tube structure; the material of the porous ceramic tube is alumina or zirconia. The microcrystalline glass coating material is silicon oxide-alumina based microcrystalline glass.

[0023] The outer diameter of the porous ceramic tube is 8-50 mm, and the length is 100-1500 mm. The length of the microcrystalline glass coating at the end of the porous ceramic tube is 5-50 mm, and the thickness of the coating is 20-200 microns.

[0024] In step (2), the coating is heat treated at a temperature of 900-1400° C. for a time of 0.5-10 hours.

[0025] In step (3), the material of the loaded palladium alloy film includes Pd-Ag, Pd-Y, Pd-Au, Pd-Cu, Pd-Pt, Pd-Ru, Pd-Ag-Cu and Pd-Ni-Au, etc. The thickness of the loaded palladium alloy film is 0.5-20 μm.

[0026] The effective length of the loaded palladium alloy membrane should ensure that it covers part of the microcrystalline glass coating and has no contact with the active metal coating. The overlap length of the loaded palladium alloy membrane and the microcrystalline glass coating is 1-50 mm.

[0027] In step (4), the length of the active metal coating is less than the length of the microcrystalline glass coating and has no contact with the supported palladium alloy membrane. The length of the active metal coating at the end of the porous ceramic tube is 1-50 mm.

[0028] The material of the active metal coating is a titanium-silver-copper alloy, including but not limited to AgCuTi4.5, AgCuTi2, AgCuTi6, etc.

[0029] The length of the active metal coating at the end of the porous ceramic tube is 1-50 mm, and the thickness of the active metal coating is 20-200 microns.

[0030] In step (5), the metal connector is made of iron-cobalt-nickel Kovar alloy and is installed and connected to the end of the porous ceramic tube; the metal connector is assembled in the area where the active metal coating is applied on the outer surface of the porous ceramic tube.

[0031] The secondary heat treatment is carried out in a vacuum or inert protective atmosphere, the heat treatment temperature is 800-1200° C., and the heat treatment time is 3-30 minutes.

[0032] Beneficial effects of the present invention: The present invention adopts a new type of hydrogen separation palladium membrane pipe structure, and the adopted microcrystalline glass layer ensures the air tightness of the end of the porous ceramic supported palladium membrane tube. In addition, since the thermal expansion coefficient of the Kovar alloy pipe and the porous ceramic carrier matches, the air tightness of the Kovar alloy pipe and the end of the porous ceramic supported palladium membrane tube and the connection reliability during the thermal cycle process can be achieved through the active alloy layer.

[0033] The hydrogen separation palladium membrane tube of the present invention can effectively solve the problem of air tightness at the end of the porous ceramic-loaded palladium membrane tube, ensure the reliability of the membrane tube thermal cycle process, and significantly improve the application performance of the hydrogen separation palladium membrane tube. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The present invention is a schematic structural diagram of a hydrogen separation palladium membrane tube.

[0035] Figure 2 It is a schematic structural diagram of another hydrogen separation palladium membrane tube of the present invention.

[0036] Description of main reference numerals:

[0037] 1Porous ceramic tube 2Loaded palladium alloy membrane

[0038] 3 Glass-ceramic coating 4 Active metal coating

[0039] 5Metal connectors DETAILED DESCRIPTION

[0040] The hydrogen separation palladium membrane pipe fitting of the present invention is composed of a porous ceramic tube, a loaded palladium alloy membrane, a metal connector, etc., wherein the porous ceramic tube adopts a one-end sealed and one-end open tube structure or a two-end open tube structure.

[0041] like Figure 1As shown, the hydrogen separation palladium membrane pipe is composed of a porous ceramic tube 1, a loaded palladium alloy membrane 2 and a metal connector 5. The structure of the porous ceramic tube 1 is a through-tube structure at both ends, and the material of the porous ceramic tube 1 is alumina or zirconia. The outer surfaces of both ends of the porous ceramic tube 1 are provided with a microcrystalline glass coating 3 and an active metal coating 4 from the inside to the outside. The length of the active metal coating 4 is less than the length of the microcrystalline glass coating 3. The active metal coating 4 is not coated on a part of the microcrystalline glass coating 3 away from the end of the porous ceramic tube 1. The outer surface of the porous ceramic tube 1 without the microcrystalline glass coating 3 and the outer surface of the part of the microcrystalline glass coating 3 adjacent to it are provided with a loaded palladium alloy membrane 2. The effective length of the loaded palladium alloy membrane 2 should ensure that it covers part of the microcrystalline glass coating 3 and has no contact with the active metal coating 4. The outer diameter of the porous ceramic tube 1 is 8-50mm and the length is 100-1500mm. The outer surface of the end of the porous ceramic tube 1 is coated with a microcrystalline glass coating 3, the coating thickness is 20-200 microns, and the length of the microcrystalline glass coating 3 at the end of the porous ceramic tube 1 is 5-50 mm. The material of the microcrystalline glass coating 3 is silicon oxide-alumina-based microcrystalline glass, and the coating heat treatment temperature is 900-1400°C. The thickness of the active metal coating 4 is 20-200 microns, and the length of the active metal coating 4 at the end of the porous ceramic tube 1 is 1-50 mm. The material of the active metal coating 4 is a titanium-silver-copper alloy, such as AgCuTi4.5, AgCuTi2, AgCuTi6, etc. The components of the loaded palladium alloy membrane 2 include Pd-Ag, Pd-Y, Pd-Au, Pd-Cu, Pd-Pt, Pd-Ru, Pd-Ag-Cu, Pd-Ni-Au, etc. The thickness of the loaded palladium alloy membrane 2 is 0.5-20 μm, and the length of the overlap between the loaded palladium alloy membrane 2 and the microcrystalline glass coating 3 is 1-50 mm. The metal connector 5 is made of iron-cobalt-nickel Kovar alloy and is installed and connected to the two ends of the porous ceramic tube 1 .

[0042] like Figure 2As shown, the hydrogen separation palladium membrane pipe is composed of a porous ceramic tube 1, a loaded palladium alloy membrane 2 and a metal connector 5. The structure of the porous ceramic tube 1 is a closed-end and open-end tube structure. The material of the porous ceramic tube 1 is alumina or zirconium oxide. The outer surface of the open end of the porous ceramic tube 1 is provided with a microcrystalline glass coating 3 and an active metal coating 4 from the inside to the outside. The length of the active metal coating 4 is less than the length of the microcrystalline glass coating 3. The active metal coating 4 is not coated on a part of the microcrystalline glass coating 3 away from the open end of the porous ceramic tube 1. The outer surface of the porous ceramic tube 1 (including the closed end) without the microcrystalline glass coating 3 and the outer surface of the part of the microcrystalline glass coating 3 adjacent to it are provided with a loaded palladium alloy membrane 2. The effective length of the loaded palladium alloy membrane 2 should ensure that it covers part of the microcrystalline glass coating 3 and has no contact with the active metal coating 4. The outer diameter of the porous ceramic tube 1 is 8-50mm and the length is 100-1500mm. The outer surface of the open end of the porous ceramic tube 1 is coated with a microcrystalline glass coating 3, the coating thickness is 20-100 microns, and the length of the microcrystalline glass coating 3 at the open end of the porous ceramic tube 1 is 5-50 mm. The material of the microcrystalline glass coating 3 is silicon oxide-alumina-based microcrystalline glass, and the coating heat treatment temperature is 900-1400°C. The thickness of the active metal coating 4 is 20-200 microns, and the length of the active metal coating 4 at the open end of the porous ceramic tube 1 is 1-50 mm. The material of the active metal coating 4 is a titanium-silver-copper alloy, such as AgCuTi4.5, AgCuTi2, AgCuTi6, etc. The components of the loaded palladium alloy film 2 include Pd-Ag, Pd-Y, Pd-Au, Pd-Cu, Pd-Pt, Pd-Ru, Pd-Ag-Cu, Pd-Ni-Au, etc. The thickness of the loaded palladium alloy film 2 is 0.5-20 μm, and the overlap length of the loaded palladium alloy film 2 and the microcrystalline glass coating 3 is 1-50 mm. The metal connector 5 is made of iron-cobalt-nickel Kovar alloy and is installed and connected to the open end of the porous ceramic tube 1.

[0043] In the present invention, the outer surface of one end of the through pipe is coated with a silicon oxide-aluminum oxide-based microcrystalline glass coating 3, and the heat treatment temperature of the microcrystalline glass coating 3 is 900-1400°C. The outer surface of the microcrystalline glass coating 3 is an active metal coating 4, and the active metal material is a titanium-silver-copper alloy, and the effective length covered by the active metal coating 4 is less than the microcrystalline glass coating 3. The effective length of the palladium alloy membrane 2 loaded on the porous ceramic tube 1 should ensure that the high-temperature microcrystalline glass coating 3 is covered and has no contact with the active metal coating 4.

[0044] Embodiment 1

[0045] like Figure 1As shown, the hydrogen separation palladium membrane pipe fittings use a porous alumina tube with a through-tube structure at both ends. The outer diameter of the porous alumina tube is 14 mm and the length is 500 mm. The CaO-Al2O3-SiO2 microcrystalline glass coating 3 is coated on both ends of the porous alumina tube by the immersion pulling method. The length of the end microcrystalline glass coating 3 is 20 mm and the thickness is 50 microns. The porous alumina tube coated with the microcrystalline glass coating 3 is placed in a high-temperature muffle furnace and sintered at 1200°C for 1 hour in an air atmosphere to form a dense microcrystalline glass coating 3 on both ends of the porous alumina. A Pd-27Ag alloy membrane is prepared on the porous alumina tube by chemical plating. The length of the Pd-27Ag alloy membrane is 470 mm. The Pd-27Ag alloy membrane covers the area not coated with the microcrystalline glass coating 3 and the area coated with the microcrystalline glass coating 3 away from the end of the pipe fitting. The distance from the Pd-27Ag alloy membrane to the two ends is the same. AgCuTi4.5 was coated on both ends of the porous alumina by the immersion and pulling method. The length of the metal coating on the end was 5 mm and the thickness was 100 microns. Kovar alloy pipe fittings were assembled on both ends of the porous alumina and placed in a tubular atmosphere furnace. They were sintered at 900°C for 30 minutes in an argon atmosphere to obtain porous alumina loaded Pd-27Ag alloy membrane pipe fittings with good airtightness. The helium leakage rate was better than 10 -12 Pa·m 3 / s.

[0046] Embodiment 2

[0047] like Figure 1 As shown, the hydrogen separation palladium membrane pipe fittings use a porous zirconia tube with a through-tube structure at both ends. The outer diameter of the porous zirconia tube is 12 mm and the length is 300 mm. The CaO-Al2O3-SiO2 microcrystalline glass coating 3 is coated on both ends of the porous zirconia tube by the immersion pulling method. The length of the end microcrystalline glass coating 3 is 20 mm and the thickness is 50 microns. The porous zirconia tube coated with the microcrystalline glass coating 3 is placed in a high-temperature muffle furnace and sintered at 1200°C for 1 hour in an air atmosphere to form a dense microcrystalline glass coating 3 at both ends of the porous zirconia. A Pd-5Ru alloy membrane is prepared on the porous zirconia tube by chemical plating. The length of the Pd-5Ru alloy membrane is 270 mm. The Pd-5Ru alloy membrane covers the area not coated with the microcrystalline glass coating 3 and the area coated with the microcrystalline glass coating 3 away from the end of the pipe fitting. The distance from the Pd-5Ru alloy membrane to the two ends is the same. AgCuTi2 metal coating was applied on both ends of porous zirconia by immersion pulling method. The length of the metal coating on the end was 5mm and the thickness was 80 microns. Kovar alloy pipe fittings were assembled on both ends of porous zirconia and placed in a tubular atmosphere furnace. They were sintered at 850℃ for 0.5 hours in nitrogen atmosphere to obtain porous zirconia loaded Pd-5Ru alloy membrane pipe fittings with good airtightness. The helium leakage rate was better than 10 -12 Pa·m 3 / s.

[0048] Embodiment 3

[0049] like Figure 2 As shown, the hydrogen separation palladium membrane pipe fittings use a porous alumina tube with a closed end and a through-tube structure at the other end. The outer diameter of the porous alumina tube is 14 mm and the length is 400 mm. The CaO-Al2O3-SiO2 microcrystalline glass coating 3 is coated on both ends of the porous alumina tube by the immersion pulling method. The length of the end microcrystalline glass coating 3 is 20 mm and the thickness is 50 microns. The porous alumina tube coated with the microcrystalline glass coating 3 is placed in a high-temperature muffle furnace and sintered at 1200°C for 1 hour in an air atmosphere to form a dense microcrystalline glass coating 3 on both ends of the porous alumina. A Pd-27Ag alloy membrane is prepared on the porous alumina tube by chemical plating process. The length of the Pd-27Ag alloy membrane is 370 mm. The Pd-27Ag alloy membrane covers the area not coated with the microcrystalline glass coating 3 (including the closed end of the pipe fitting) and the area coated with the microcrystalline glass coating 3 away from the open end of the pipe fitting. AgCuTi4.5 metal coating is applied to both ends of porous alumina by immersion and pulling method. The length of the metal coating at the end is 5mm and the thickness is 80 microns. Kovar alloy pipe fittings are assembled at the open end of porous alumina, placed in a tubular atmosphere furnace, and sintered at 900℃ for 30 minutes under vacuum to obtain porous alumina loaded Pd-27Ag alloy membrane pipe fittings with good airtightness, and the helium leakage rate is better than 10 -12 Pa·m 3 / s.

[0050] Embodiment 4

[0051] like Figure 2As shown, the hydrogen separation palladium membrane pipe fittings use a porous alumina tube with a closed end and a through-tube structure at the other end. The outer diameter of the porous alumina tube is 14 mm and the length is 400 mm. The CaO-Al2O3-SiO2 microcrystalline glass coating 3 is coated on both ends of the porous alumina tube by the immersion pulling method. The length of the end microcrystalline glass coating 3 is 20 mm and the thickness is 50 microns. The porous alumina tube coated with the microcrystalline glass coating 3 is placed in a high-temperature muffle furnace and sintered at 1200°C for 1 hour in an air atmosphere to form a dense microcrystalline glass coating 3 on both ends of the porous alumina. A Pd-40Cu alloy membrane is prepared on the porous alumina tube by chemical plating process. The length of the Pd-40Cu alloy membrane is 370 mm. The Pd-40Cu alloy membrane covers the area not coated with the microcrystalline glass coating 3 (including the closed end of the pipe fitting) and the area coated with the microcrystalline glass coating 3 away from the open end of the pipe fitting. AgCuTi4.5 metal coating is applied to both ends of porous alumina by immersion and pulling method. The length of the metal coating at the end is 5mm and the thickness is 50 microns. Kovar alloy pipe fittings are assembled at the open end of porous alumina and placed in a tubular atmosphere furnace. Sintered at 900℃ for 30 minutes under vacuum, porous alumina loaded Pd-40Cu alloy membrane pipe fittings with good airtightness can be obtained, and the helium leakage rate is better than 10 -12 Pa·m 3 / s.

[0052] The hydrogen separation palladium membrane tube of the present invention can effectively solve the problem of air tightness at the end of the porous ceramic-loaded palladium membrane tube, ensure the reliability of the membrane tube thermal cycle process, and significantly improve the application performance of the hydrogen separation palladium membrane tube.

Claims

1. A hydrogen separation palladium membrane pipe, characterized in that: The pipe fitting includes a porous ceramic tube and a metal connector. The outer surface of the open end of the porous ceramic tube is provided with a microcrystalline glass coating and an active metal coating from the inside to the outside. The length of the active metal coating is shorter than the length of the microcrystalline glass coating. The outer surface of the porous ceramic tube without the microcrystalline glass coating and the outer surface of the part of the microcrystalline glass coating adjacent to it are provided with a loaded palladium alloy membrane.

2. The hydrogen separation palladium membrane tube according to claim 1, characterized in that: The structure of the porous ceramic tube is a tube structure with one end sealed and the other end open, or a tube structure with two ends open. The material of the porous ceramic tube is alumina or zirconia.

3. The hydrogen separation palladium membrane tube according to claim 1, characterized in that: The outer surface of the open end of the porous ceramic tube is coated with a microcrystalline glass coating with a coating thickness of 20-200 microns; the microcrystalline glass coating material is silicon oxide-aluminum oxide-based microcrystalline glass, and the coating heat treatment temperature is 900-1400°C.

4. The hydrogen separation palladium membrane tube according to claim 1, characterized in that: The material of the active metal coating is a titanium-silver-copper alloy; the thickness of the active metal coating is 20-200 microns.

5. The hydrogen separation palladium membrane tube according to claim 1, characterized in that: The loaded palladium alloy film is Pd-Ag, Pd-Y, Pd-Au, Pd-Cu, Pd-Pt, Pd-Ru, Pd-Ag-Cu or Pd-Ni-Au; and the thickness of the loaded palladium alloy film is 0.5-20 μm.

6. The hydrogen separation palladium membrane tube according to claim 1, characterized in that: The effective length of the loaded palladium alloy membrane is to cover a portion of the microcrystalline glass coating and have no contact with the active metal coating.

7. The hydrogen separation palladium membrane tube according to claim 1, characterized in that: The metal connector is installed at the open end of the porous ceramic tube, and the material of the metal connector is iron-cobalt-nickel Kovar alloy.

8. The method for preparing a hydrogen separation palladium membrane tube according to any one of claims 1 to 7, characterized in that: The steps include: (1) Applying a glass-ceramic coating: applying a glass-ceramic coating on the outer surface of the end of the open end of the porous ceramic tube by a dipping and pulling method; (2) performing a heat treatment: performing a heat treatment on the porous ceramic tube coated with the microcrystalline glass coating to form a dense microcrystalline glass coating at the end of the open end of the porous ceramic tube; (3) preparing a loaded palladium alloy membrane: using a chemical plating process, plating a loaded palladium alloy membrane on the outer surface of the porous ceramic tube that is not coated with the microcrystalline glass coating and on the outer surface of a portion of the microcrystalline glass coating adjacent thereto; (4) applying an active metal coating: applying an active metal coating on the glass-ceramic coating at the end of the open end of the porous ceramic tube by an immersion pulling method, wherein the active metal coating has no contact with the loaded palladium alloy membrane; (5) Assembling and performing secondary heat treatment: Assembling a metal connector at the end of the open end of the porous ceramic tube, performing secondary heat treatment, and obtaining a porous hydrogen separation palladium membrane tube with good airtightness.

9. The method for preparing the hydrogen separation palladium membrane tube according to claim 8, characterized in that: The outer diameter of the porous ceramic tube is 8-50mm, and the length is 100-1500mm; the length of the microcrystalline glass coating at the end of the porous ceramic tube is 5-50mm, and the length of the active metal coating at the end of the porous ceramic tube is 1-50mm; the overlapping length of the loaded palladium alloy membrane and the microcrystalline glass coating is 1-50mm.

10. The method for preparing a hydrogen separation palladium membrane tube according to claim 8, characterized in that: The temperature of the primary heat treatment is 900-1400°C, and the heat treatment time is 0.5-10 hours; the secondary heat treatment is carried out in an inert or vacuum atmosphere, and the heat treatment temperature is 900-1200°C, and the heat treatment time is 3-30 minutes.