Burn-resistant composite material and preparation method thereof, lithium battery and vehicle

By using glass fiber or carbon fiber load-bearing layer and ceramic fiber flame retardant layer in lithium battery packs and adding caloriresistant composite materials with phenolic foam insulation layer, the problem that existing materials cannot prevent flame spread at high temperatures is solved, and the problem of existing materials cannot prevent flame spread at high temperatures is achieved. The lightweight and high-temperature flame retardant performance of lithium battery packs ensure the safety and performance of new energy vehicles.

CN114937845BActive Publication Date: 2024-12-03SHANGHAI PENGSHENG MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210604270.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-05-19
Publication Date
2024-12-03
Estimated Expiration
2042-05-19

AI Technical Summary

Technical Problem

The existing high-temperature resistant composite materials cannot effectively prevent the flame from spreading at 1500℃, and cannot meet the ablation requirements of lithium battery packs at high temperatures. The battery packs prepared by traditional metal stamping process are bulky and cannot meet the lightweight needs of new energy vehicles. .

Method used

A burn-resistant composite material consisting of glass fiber or carbon fiber load-bearing layer and ceramic fiber flame retardant layer is used, and a phenolic foam heat insulation layer is added to it. Through structural flame retardant, it meets the flame retardant requirements of UL94V0 and achieves ablation at 1500℃. The effect of not burning through for 30 minutes.

Benefits of technology

The flame retardant performance without burning through at 1500℃ for 30 minutes and the thermal temperature control below 210℃ are achieved, which improves the safety and lightweight characteristics of the lithium battery pack and meets the safety and performance needs of new energy vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114937845B_ABST
    Figure CN114937845B_ABST
Patent Text Reader

Abstract

This patent discloses a burn-resistant composite material and its preparation, lithium battery and transportation vehicle, which relates to the field of layered products and is used to solve the problem that lightweight composite materials are not resistant to strong burns. When a lithium battery pack catches fire abnormally, the shell needs to suppress combustion in a short period of time, and can prevent the spread of flames for a long time, fully protecting human life and property safety. The present invention meets the UL94V0 flame retardant requirements on the premise of ensuring the mechanical properties and lightweight of the material through structural flame retardancy, and achieves ablation at 1500°C for 30 minutes without burning through. In one embodiment, a phenolic foam sandwich layer is added to achieve the effect of a back heat temperature below 210°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of layered products, and in particular to a burn-resistant composite material and preparation thereof, a lithium battery and a vehicle. Background Art

[0002] At present, lightweight research is hot in the field of new energy vehicles. As the focus of new energy vehicles, the endurance is the key to all parts of the vehicle. All parts of the vehicle are being replaced with lightweight within a safe and controllable range. As for lithium battery packs, which are the core components of new energy vehicles, the battery pack shells prepared by traditional metal stamping processes are bulky and no longer meet the current needs of new energy vehicles. In order to solve the problem of lightweight replacement of lithium battery packs, the existing technology uses high-temperature resistant inorganic ceramic material composites. As the protective substrate of the battery pack, the composite lithium battery pack shell needs to ensure that the lithium battery pack can play an excellent protective role in unexpected situations, such as accidental fire of the lithium battery pack. This requires the lithium battery pack shell material to have certain fire retardant functions. When the lithium battery pack catches fire abnormally, the shell needs to suppress combustion in a short time, and can prevent the spread of flames for a long time to fully protect human life and property safety. Therefore, the requirements for flame retardancy are more stringent. However, when the existing composite materials are used as battery pack shells, their temperature resistance is about 450℃~1000℃, which cannot meet the requirements of long-term ablation at 1500℃. Summary of the invention

[0003] The present invention provides a burn-resistant composite material and a preparation method thereof, which are used to solve the problem that lightweight composite materials are not resistant to strong burns. The present application also provides a lithium battery using the above-mentioned burn-resistant composite material as a battery pack shell and a vehicle using the lithium battery, which are used to improve the safety of lithium batteries and related vehicles. The present invention prepares high-temperature ablation-resistant ceramic fiber layers into prepregs of different thicknesses, and uses glass fiber and carbon fiber composite materials as skin support materials. Through structural flame retardancy, while ensuring the mechanical properties and lightweight of the material, it meets the UL94V0 flame retardant requirements and achieves ablation at 1500°C for 30 minutes without burning through. In one embodiment, a phenolic foam sandwich layer is added to achieve the beneficial effect of the back heat temperature being lower than 210°C.

[0004] Specifically, the present invention provides a burn-resistant composite material, which comprises: a glass fiber bearing layer and a ceramic fiber flame-retardant layer.

[0005] Preferably, the glass fiber bearing layer is arranged on the outside.

[0006] Preferably, the glass fiber bearing layer is composed of at least one layer of glass fiber prepreg.

[0007] Preferably, a phenolic foam insulation layer is also included.

[0008] Preferably, the phenolic foam insulation layer is located between the glass fiber load-bearing layer and the ceramic fiber flame-retardant layer.

[0009] Preferably, glass fiber prepreg is included between the ceramic fiber flame retardant layer and the phenolic foam insulation layer.

[0010] Preferably, the ceramic fiber flame retardant layer is composed of alumina prepreg.

[0011] Preferably, the single layer thickness of the glass fiber prepreg is 0.2 mm-0.45 mm.

[0012] Preferably, the glass fiber bearing layer is replaced by a carbon fiber bearing layer.

[0013] The present invention also provides a method for preparing the burn-resistant composite material, the method comprising:

[0014] The glass fiber prepreg and the ceramic fiber prepreg are prepared; the glass fiber prepreg and the ceramic fiber prepreg are laid in a specific order; and the prepreg is cured and formed.

[0015] The present invention provides a lithium battery using a burn-resistant composite material, wherein the lithium battery uses a shell made of the burn-resistant composite material;

[0016] The invention provides a vehicle using a burn-resistant composite material lithium battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0018] Figure 1 It is a structural diagram of Example 1 and Example 2 of the burn-resistant composite material of the present invention, wherein 100 is a glass fiber (or carbon fiber) load-bearing layer, 300 is a ceramic fiber flame-retardant layer, and 200 is a phenolic foam heat-insulating layer;

[0019] Figure 2 It is a structural diagram of Example 3 and Example 4 of the burn-resistant composite material of the present invention, wherein 100 is a glass fiber (or carbon fiber) bearing layer, and 300 is a ceramic fiber flame retardant layer;

[0020] Figure 3 Schematic diagram of the fixing method of thermocouples in the burn resistance test of the present invention, wherein the thermocouples are arranged in a cross shape, with 7 in both the horizontal and vertical directions;

[0021] Figure 4The horizontal temperature curve of the non-fired surface of the composite material prepared in Example 1 of the present invention is shown in FIG. 1 . The horizontal axis is time in seconds. The numbers marked on the right side of the curve are the numbers of the thermocouples, which respectively represent the attached Figure 3 Thermocouples in the horizontal direction shown in the figure;

[0022] Figure 5 The temperature curve of the composite material prepared in Example 1 of the present invention in the vertical direction of the back-fired surface is shown in Figure 1. The horizontal axis is time in seconds. The numbers marked on the right side of the curve are the numbers of the thermocouples, which represent the attached Figure 3 The vertical thermocouples shown in FIG.

[0023] Figure 6 The horizontal temperature curve of the non-fired surface of the composite material prepared in Example 2 of the present invention is shown in FIG. 1 . The horizontal axis is time in seconds. The numbers marked on the right side of the curve are the numbers of the thermocouples, which represent the attached Figure 3 Thermocouples in the horizontal direction shown in the figure;

[0024] Figure 7 The temperature curve in the vertical direction of the back-fired surface of the composite material prepared in Example 2 of the present invention is shown in FIG. 1 . The horizontal axis is time in seconds. The numbers marked on the right side of the curve are the numbers of the thermocouples, which respectively represent the attached Figure 3 The vertical thermocouples shown in FIG. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Specifically, the present invention provides a burn-resistant composite material, which includes: a glass fiber bearing layer and a ceramic fiber flame-retardant layer. In a certain embodiment, it also includes a phenolic foam insulation layer. The bearing layer is used to maintain the mechanical properties of the composite material, and can also be made of better carbon fiber. The insulation layer is used to reduce the thermal conductivity temperature and is made of phenolic foam. The ceramic fiber flame-retardant layer can withstand high-temperature burning without burning through, and in a preferred embodiment, it is made of alumina fiber with better flame-retardant effect.

[0027] Embodiment 1:

[0028] The ceramic fiber flame retardant layer is composed of a single layer of alumina short fiber prepreg felt with a thickness of about 0.54 mm, and the alumina short fiber prepreg felt is made of alumina short fiber felt (produced by Shandong Dongheng Guoxian New Materials Co., Ltd., with a gram weight of about 400g / m2) impregnated with flame retardant resin, wherein the resin weight accounts for about 40%. The ceramic fiber flame retardant layer directly contacts the flame when exerting its burning resistance.

[0029] The ceramic fiber flame retardant layer is adjacent to a single layer of glass fiber prepreg A with a thickness of 0.21 mm, and the glass fiber prepreg A is made of glass fiber cloth impregnated with flame retardant resin (weight is about 200 g / ㎡), wherein the resin weight accounts for about 40%. The glass fiber prepreg A is used to bond the ceramic fiber flame retardant layer to the phenolic foam insulation layer.

[0030] The phenolic foam insulation layer is filled with 10 mm phenolic foam, and the other side of the phenolic foam insulation layer is a glass fiber bearing layer.

[0031] The glass fiber bearing layer as the surface layer is composed of three layers of glass fiber prepreg B with a single layer thickness of 0.42 mm. The glass fiber prepreg B is made of glass fiber cloth impregnated with flame retardant resin (weight is about 400g / ㎡), of which the resin weight accounts for about 40%.

[0032] The flame retardant resin component comprises: 35 parts of bisphenol A epoxy resin, 30 parts of phenolic epoxy resin, 12 parts of dicyandiamide curing agent, 1.5 parts of accelerator, 22 parts of phosphorus flame retardant, 8 parts of aluminum hydroxide, and 1.5 parts of viscosity reducing agent.

[0033] Embodiment 2:

[0034] The specifications of the glass fiber bearing layer and the ceramic fiber flame retardant layer on the surface of Example 2 are the same as those of Example 1, except that the phenolic foam insulation layer is filled with 5 mm phenolic foam.

[0035] Embodiment 3:

[0036] The ceramic fiber flame retardant layer is composed of a single layer of alumina short fiber prepreg felt with a thickness of about 0.54 mm. The alumina short fiber prepreg felt is made of alumina chopped fiber felt impregnated with flame retardant resin (produced by Shandong Dongheng Guoxian New Materials Co., Ltd., with a gram weight of about 400g / m2), of which the resin weight accounts for about 40%.

[0037] The glass fiber bearing layer as the surface layer is composed of two layers of glass fiber prepreg B with a single layer thickness of 0.42 mm and one layer of glass fiber prepreg A with a single layer thickness of 0.21 mm. The composition and specifications of the glass fiber prepregs A and B are the same as those in Example 1.

[0038] Embodiment 4:

[0039] The ceramic fiber flame retardant layer is composed of a single layer of alumina short fiber prepreg felt with a thickness of about 0.54 mm. The alumina short fiber prepreg felt is made of alumina chopped fiber felt impregnated with flame retardant resin (produced by Shandong Dongheng Guoxian New Materials Co., Ltd., with a gram weight of about 400g / m2), of which the resin weight accounts for about 40%.

[0040] The carbon fiber bearing layer as the surface layer is composed of two layers of carbon fiber prepreg with a single layer thickness of 0.4 mm. The carbon fiber prepreg is made of carbon fiber cloth impregnated with flame retardant resin (weight is about 400g / ㎡), of which the resin weight accounts for about 40%.

[0041] The flame retardant resin component is the same as that in Example 1.

[0042] The present invention also provides a method for preparing a burn-resistant composite material, the method comprising: preparing glass fiber prepreg and ceramic fiber prepreg; laying the glass fiber prepreg and ceramic fiber prepreg in a specific order; and curing and molding.

[0043] Embodiment 1:

[0044] S10, preparing glass fiber prepreg and ceramic fiber prepreg;

[0045] S11, preparing a resin system that meets the flame retardant requirements of UL94V0, and coating the resin evenly on the release paper through a coating device to form upper and lower resin films, with the mass content of the resin film being 35% to 45%.

[0046] The flame retardant resin system specifically includes: 35 parts of bisphenol A epoxy resin, 30 parts of phenolic epoxy resin, 12 parts of dicyandiamide curing agent, 1.5 parts of accelerator, 22 parts of phosphorus flame retardant, 8 parts of aluminum hydroxide, and 1.5 parts of viscosity reducing agent.

[0047] S12, effectively impregnating the resin film with the glass fiber (or carbon fiber) fabric through a prepreg device to prepare a glass fiber (or carbon fiber) fabric prepreg; the glass fiber prepreg includes glass fiber prepreg A and glass fiber prepreg B. The specifications of the prepregs refer to the product example 1 above. The specifications of the carbon fiber prepreg refer to the product example 4 above.

[0048] S13, prefabricating the resin film and the ceramic fiber into a prepreg mat by a prepreg device. The ceramic fiber prepreg is an alumina fiber prepreg.

[0049] S20, laying the glass fiber (or carbon fiber) prepreg and the ceramic fiber prepreg in a specific order;

[0050] From the flame contact surface to the outer surface, it is:

[0051] (1) 1 layer of alumina short fiber prepreg felt;

[0052] (2) a layer of glass fiber prepreg A, the above two layers together constitute a ceramic fiber flame retardant layer;

[0053] (3) 10 mm phenolic foam filled phenolic foam insulation layer;

[0054] (4) Lay down 3 layers of glass fiber prepreg B.

[0055] S30, curing and molding;

[0056] Press cure at 150°C for 5-8 minutes;

[0057] Embodiment 2:

[0058] The preparation method of Example 2 is substantially the same as that of Example 1, except that the sandwich layer is filled with 5 mm phenolic foam.

[0059] Embodiment 3:

[0060] The difference between Example 3 and Example 1 is that:

[0061] S20, laying the glass fiber prepreg and the ceramic fiber prepreg in a specific order;

[0062] From the flame contact surface to the outer surface, it is:

[0063] (1) One layer of alumina short fiber prepreg felt as a ceramic fiber flame retardant layer;

[0064] (2) 2 layers of glass fiber prepreg B and 1 layer of glass fiber prepreg A.

[0065] The remaining steps are the same as those in Example 1.

[0066] Embodiment 4:

[0067] The difference between Example 4 and Example 1 is that:

[0068] S20, laying the carbon fiber prepreg and the ceramic fiber prepreg in a specific order;

[0069] From the flame contact surface to the outer surface, it is:

[0070] (1) 1 layer of alumina short fiber prepreg felt;

[0071] (2) 2 layers of carbon fiber prepreg with a single layer thickness of 0.4 mm.

[0072] The remaining steps are the same as those in Example 1.

[0073] Those skilled in the art may also use other curing methods under the guidance of the above embodiments, for example, curing the composite material in an autoclave at 150°C for 5 minutes and a curing pressure of 6 bar to form the burn-resistant composite material, or using an RTM molding process to form the burn-resistant composite material, or using other molding processes not covered herein. On the basis of being able to achieve the same or similar effects, all of them do not exceed the protection scope of this patent.

[0074] The present invention is used for the test method of the flame retardancy and burning resistance of composite materials:

[0075] Step 1: Weigh the test sample, take a photo, and load it on the laboratory bench.

[0076] according to Figure 2 In the arrangement shown, a carbon strip is used to fix the thermocouple on the back of the test sample, and the two ends of the carbon strip and the test sample are clamped with a fixture. The thermocouple position is the center position, with an interval of 40mm upward, downward, left and right;

[0077] Step 2: Complete the calibration of flame temperature 1500±100℃ (flame diameter reference value 30mm), determine and record the distance between the flame and the nozzle;

[0078] Step 3: Clamp the test sample on the tooling to monitor the flame temperature, place the test sample on the position determined in step 2 through the tooling, start timing and take photos for record;

[0079] Step 4: Record the test process with video, observe the front and back phenomena of the test sample (including whether smoke appears, whether the material has burning flames, etc.), and record the temperature curve of the back panel of the test sample.

[0080] The present invention is used to evaluate the flame retardancy and burning resistance of composite materials:

[0081] The test is terminated when any of the following situations occurs. If none of the following situations occurs, the test is terminated when the test time is 30 minutes.

[0082] Case 1: Flame appears on the back of the test sample and continues to burn for 10 seconds;

[0083] Case 2: The temperature of any thermocouple on the back-fired surface reaches above 500°C.

[0084] With the aid of the above test methods and performance standards, the experimental data of each embodiment of the present invention are as follows:

[0085] Example 1 Test flame retardant data, such as Figure 4 , Figure 5 As shown: 1500±100℃ high temperature ablation for 1800s, the fire-exposed surface is not burned through, and the maximum temperature of the non-fired surface detected by the thermocouple is 185.8℃. This shows that the embodiment of the present invention with a heat insulation layer has the beneficial effects of both burn resistance and heat insulation.

[0086] Example 2 Test flame retardant data, such as Figure 6 , Figure 7 As shown: 1500±100℃ high temperature ablation for 1800s, the fire-exposed surface is not burned through, and the maximum temperature of the non-fired surface detected by the thermocouple is 207.7℃. This shows that the embodiment of the present invention with a heat insulation layer has the beneficial effects of both burn resistance and heat insulation.

[0087] Flame retardant data of Example 3: After high temperature ablation at 1500±100°C for 300s, the fire-exposed surface was not burned through. Since Example 3 did not have a phenolic foam insulation layer, no thermocouple test was performed.

[0088] The flame retardant data of Example 4: 1500±100℃ high temperature ablation for 1800s, the fire-exposed surface was not burned through. Since Example 4 does not have a phenolic foam insulation layer, no thermocouple detection was performed. The test results are detailed in the following table:

[0089]

[0090]

[0091] The present invention provides a lithium battery using a burn-resistant composite material, wherein the lithium battery uses a shell made of the burn-resistant composite material; the present invention also provides a vehicle using a lithium battery using the burn-resistant composite material;

[0092] Compared with the traditional composite lithium battery shell, the lithium battery shell made of the ablation-resistant glass fiber-alumina fiber composite material without a heat insulation layer provided by the burn-resistant composite material embodiment 3 of the present invention can be burned at a fixed point at a high temperature of 1500±100°C, and can be continuously ablated for more than 5 minutes without burning through; the lithium battery shell made of the ablation-resistant carbon fiber-alumina fiber composite material without a heat insulation layer provided by the burn-resistant composite material embodiment 4 of the present invention can be burned at a fixed point at a high temperature of 1500±100°C, and can be continuously ablated for more than 30 minutes without burning through;

[0093] Since both carbon fiber and glass fiber have the property of being resistant to burning, the lithium battery pack shell made of the ablation-resistant glass fiber-alumina fiber composite material with a heat insulation layer provided by the inventor in Examples 1 and 2, and the lithium battery pack shell made of the carbon fiber-alumina fiber composite material that can be obtained without creative labor on the basis of Examples 1 and 4 can be burned at a fixed point at a high temperature of 1500±100℃, and can be continuously ablated for more than 30 minutes, and the back temperature does not exceed 210℃. After burning, the composite lithium battery pack shell still maintains the basic load-bearing function, and the safety of the car and the people in the car is guaranteed to the greatest extent. In addition to being used for battery pack shells, this product can also be used in thermal protection scenarios of various medium and large lithium power sources.

[0094] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention.

Claims

1. A burn-resistant composite material, characterized in that: It is composed of glass fiber bearing layer, ceramic fiber flame retardant layer and phenolic foam insulation layer; The phenolic foam insulation layer is located between the glass fiber load-bearing layer and the ceramic fiber flame-retardant layer; The glass fiber bearing layer is arranged on the outside, and the glass fiber bearing layer is composed of at least one layer of glass fiber prepreg; The ceramic fiber flame retardant layer consists of aluminum oxide prepreg and glass fiber prepreg.

2. The burn-resistant composite material according to claim 1, characterized in that: The single layer thickness of the glass fiber prepreg is 0.2 mm-0.45 mm.

3. The method for preparing the burn-resistant composite material according to claim 1 or 2, characterized in that: Preparation of glass fiber prepreg and ceramic fiber prepreg; The glass fiber prepreg and the ceramic fiber prepreg are laid in a specific order, wherein the ceramic fiber prepreg is an alumina fiber prepreg; wherein the specific order is from the flame contact surface to the outer surface: (1) alumina short fiber prepreg felt layer; (2) glass fiber prepreg layer, wherein the above two layers together constitute a ceramic fiber flame retardant layer; (3) a phenolic foam insulation layer filled with phenolic foam; (4) glass fiber prepreg laying; Curing and forming.

4. A lithium battery using the burn-resistant composite material as claimed in claim 1 or 2 as a battery pack shell.

5. A vehicle using the lithium battery as claimed in claim 4.