Adhesive tape
The adhesive tape with filler particles and triblock copolymer structure addresses the challenge of easy peeling and high adhesive strength, ensuring effective load holding and removability on rough surfaces.
Patent Information
- Application Number
- CN202180008831.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-01-21
- Filing Date
- 2021-01-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-01-14
AI Technical Summary
Adhesive tapes used in electronic devices face challenges in being easily peeled off, especially in narrow spaces, while maintaining high adhesive strength and load holding power, particularly when adhering to rough surfaces over time.
Incorporating filler particles and a specific triblock copolymer structure in the adhesive layer, with a D50/T ratio of 0.05 to 1.0, to enhance peelability and maintain high adhesive strength.
The adhesive tape achieves excellent high-load holding power, high peeling strength, and removability, even on rough surfaces, allowing easy peeling in a 90° direction without significant adhesion increase over time.
Smart Images

Figure CN114945642B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an adhesive tape. Background Art
[0002] The adhesive tape has excellent operability and high bonding reliability. Therefore, the adhesive tape is widely used as a bonding means to fix the parts of relatively large electronic devices such as thin TVs, home appliances, OA equipment (office automation equipment), or relatively small electronic devices such as portable electronic terminals, cameras, and personal computers. More specifically, in various industrial fields such as OA equipment, IT and home appliances, and automobiles, it is not only used for fixing metal plates constituting large electronic devices to each other or fixing external parts to shells, and fixing rigid parts such as external parts or batteries to small electronic devices, and temporary fixing of the parts, but also for labeling purposes such as displaying product information.
[0003] In recent years, from the perspective of protecting the global environment and for the purpose of saving resources, there is an increasing trend in the above-mentioned industrial fields to disassemble the used products and reuse or re-use the reusable or reusable parts used in the products. At this time, when an adhesive tape is used, it is necessary to peel off the adhesive tape attached to the parts, but the adhesive tape usually has a strong adhesive force and is attached to multiple parts of the product, so the operation of peeling them off is accompanied by considerable labor. Therefore, an adhesive tape that can be relatively easily peeled off and removed when reused or reused is required.
[0004] As a technology related to an adhesive tape that can be easily peeled and removed, for example, Patent Document 1 can be cited. Patent Document 1 discloses an adhesive tape having an adhesive portion and a tab portion, which can be peeled off by clamping the tab portion from adherends on both sides of the adhesive portion and stretching it in a direction substantially parallel to the adhesive surface. However, in a small electronic device, since the space between components in the electronic device is narrow, there is a problem that it is difficult to stretch and peel the adhesive tape attached to the space in a direction parallel to the adhesive surface.
[0005] As a technology to solve this problem, Patent Document 2 discloses an adhesive tape that can be removed again by stretching it in a direction of 30° relative to the adhesive surface. However, in order to stretch and peel the adhesive tape attached to a narrow space, it is necessary to stretch and peel the adhesive tape at a greater angle relative to the adhesive surface. Therefore, the technology of Patent Document 2 still cannot solve the problem that it is difficult to stretch and peel in a direction parallel to the adhesive surface.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2015-124289
[0009] Patent Document 2: Japanese Patent Application No. 2016-504449 Summary of the invention
[0010] Technical problem to be solved by the invention
[0011] As described above, the pressure-sensitive adhesive tape is used to fix components of various devices ranging from small to large, and therefore it is required to be able to firmly fix each component even when a high load is applied.
[0012] On the other hand, in order to reuse or re-use the components of various devices, the adhesive tape is required to have the property of being relatively easy to peel off and remove. Here, in addition to being required to firmly fix the components by the adhesive tape, in order to pull the adhesive tape and peel it off during reuse or re-use, it is also required to have high adhesive strength and excellent re-peelability even if the adherend is a rough surface whose adhesion is easily increased over time.
[0013] Therefore, the problem of the present invention is to solve the above-mentioned problems of the prior art and provide an adhesive tape having excellent high load holding power, high adhesive strength and excellent re-peelability. In addition, the problem of the present invention is to provide an adhesive tape that can be re-peeled in the 90° direction even if the adherend whose adhesion is likely to increase over time is a rough surface.
[0014] Means for solving technical problems
[0015] The present inventors conducted intensive studies to solve the above-mentioned problems and found that the above-mentioned problems can be solved by using filler particles and a triblock copolymer of a specific structure in the adhesive layer of the adhesive tape and further setting the ratio of the average particle size of the filler particles to the average thickness of the adhesive layer to a specific range, thereby completing the present invention.
[0016] The main configuration of the present invention for solving the above-mentioned problems is as follows.
[0017] [1] The adhesive tape of the present invention comprises an adhesive layer, wherein:
[0018] The adhesive layer comprises filler particles and a triblock copolymer having repeating units represented by the following general formula (1):
[0019] [Chemical formula 1]
[0020]
[0021] (In the above general formula (1), A, B and C each independently represent a repeating unit,
[0022] A and C each independently represent an alkyl methacrylate monomer unit,
[0023] B represents an alkyl acrylate monomer unit,
[0024] p, q and r each independently represent the degree of polymerization of each monomer unit,
[0025] A and C may be the same, or may be alkyl methacrylate monomer units having different chemical structures. In the above general formula (1), * represents the bonding position with other atoms.
[0026] D50 / T, which is the relationship between the average particle size D50 of the filler particles and the average thickness T of the adhesive layer, is in the range of 0.05 to 1.0.
[0027] [2] The pressure-sensitive adhesive tape of the present invention preferably further includes a base layer in contact with one surface of the pressure-sensitive adhesive layer.
[0028] [3] The pressure-sensitive adhesive tape of the present invention preferably has a peel strength of 5 N / 20 mm or more.
[0029] [4] The adhesive tape of the present invention preferably has a cleavage adhesive strength of 10 to 200 N / cm 2 .
[0030] [5] In the pressure-sensitive adhesive tape of the present invention, it is preferred that the pressure-sensitive adhesive layer further contains a tackifier resin.
[0031] [6] Here, the adhesive layer preferably contains 10 to 150 parts by mass of the tackifier resin based on 100 parts by mass of the triblock copolymer.
[0032] [7] In addition, the substrate layer preferably has a breaking stress of 1 to 100 MPa, a breaking elongation of 400 to 3000%, and a 50% modulus of 0.1 to 5 MPa.
[0033] Effects of the Invention
[0034] According to the present invention, an adhesive tape having excellent high load holding power, high peeling adhesive strength and cleavage adhesive strength, and excellent removability can be provided. The adhesive tape is particularly difficult to increase in adhesion over time even if the adherend is a rough surface, and can be re-peeled in a 90° direction. DETAILED DESCRIPTION
[0035] Hereinafter, an embodiment of the present invention (hereinafter referred to as “the present embodiment”) will be described in detail, but the present invention is not limited to the present embodiment.
[0036] The adhesive tape of the present embodiment has an adhesive layer, and the adhesive layer contains filler particles and a triblock copolymer having a repeating unit represented by the following general formula (1):
[0037] [Chemical formula 2]
[0038]
[0039] (In the above general formula (1), A, B and C each independently represent a repeating unit,
[0040] A and C each independently represent an alkyl methacrylate monomer unit,
[0041] B represents an alkyl acrylate monomer unit,
[0042] p, q and r each independently represent the degree of polymerization of each monomer unit,
[0043] A and C may be the same, or may be alkyl methacrylate monomer units having different chemical structures. In the above general formula (1), * represents the bonding position with other atoms. ).
[0044] In the pressure-sensitive adhesive tape of the present embodiment, D50 / T, which is a relationship between the average particle size D50 of the filler particles and the average thickness T of the pressure-sensitive adhesive layer, is in the range of 0.05 to 1.0.
[0045] Since the adhesive layer of the pressure-sensitive adhesive tape of the present embodiment contains the triblock copolymer having a repeating unit represented by the general formula (1), the pressure-sensitive adhesive tape has high initial adhesive strength and is excellent in high-load holding power.
[0046] Furthermore, the pressure-sensitive adhesive tape of the present embodiment contains filler particles in the pressure-sensitive adhesive layer. When stretched, the filler particles are exposed from the pressure-sensitive adhesive layer, thereby reducing the bonding area between the pressure-sensitive adhesive layer and the adherend. Therefore, the adhesive force during stretching is low.
[0047] In addition, the adhesive tape of this embodiment makes D50 / T, which is the relationship between the average particle size D50 of the filler particles in the adhesive layer and the average thickness T of the above-mentioned adhesive layer, greater than 0.05, so that the filler particles are easily exposed from the adhesive layer during extension, thereby further reducing the bonding area between the adhesive layer and the adherend, and thus further reducing the bonding force during extension.
[0048] In addition, the adhesive tape of this embodiment suppresses the filler particles from being exposed from the adhesive layer when the adhesive tape is not stretched (i.e., the initial state) by making D50 / T, which is the relationship between the average particle size D50 of the filler particles in the adhesive layer and the average thickness T of the above-mentioned adhesive layer, less than 1.0, thereby improving the initial bonding force and the high load holding force.
[0049] Therefore, the pressure-sensitive adhesive tape of the present embodiment is excellent in high-load holding power, and although the initial adhesive force is high, the adhesive force during elongation is low, so that the pressure-sensitive adhesive tape can be simply and easily peeled off by elongating the pressure-sensitive adhesive tape.
[0050] "Adhesive layer"
[0051] The adhesive layer of the adhesive tape of the present embodiment contains filler particles and a triblock copolymer having a repeating unit represented by the general formula (1) described below, and preferably further contains a tackifier resin, and may further contain other components.
[0052] The adhesive layer of the adhesive tape of the present embodiment is formed of an adhesive composition containing filler particles, a triblock copolymer having a repeating unit represented by the general formula (1) described below, and, if necessary, a tackifier resin and / or other components.
[0053] <Filling particles>
[0054] The adhesive layer of the adhesive tape of the present embodiment includes filler particles. In addition, in the present embodiment, the adhesive composition as a precursor of the adhesive layer contains filler particles. By making the adhesive composition as a precursor of the adhesive layer include the filler particles, the filler particles are exposed from the adhesive layer when the adhesive tape is stretched, so that the bonding area between the adhesive layer and the adherend becomes smaller. Therefore, even in the case where the elongation direction of the adhesive tape is a larger angle relative to the attachment surface (hereinafter, sometimes also referred to as "adhesive surface") of the adherend, such as the vertical direction (sometimes also referred to as "90 ° direction"), in addition, even in the case of stretching at a fast speed, the adhesive tape can be peeled off more simply and more quickly.
[0055] The type of filler particles is not particularly limited and can be appropriately selected within a range that does not impair the effects of the present invention, and may be either an inorganic filler or an organic filler. These may be used alone or in combination of two or more.
[0056] Specific examples of the inorganic filler include aluminum hydroxide, magnesium hydroxide, aluminum oxide, silicon oxide, magnesium oxide, zinc oxide, titanium oxide, zirconium oxide, iron oxide, silicon carbide, boron nitride, aluminum nitride, titanium nitride, silicon nitride, titanium boride, carbon, nickel, copper, aluminum, titanium, gold, silver, zirconium hydroxide, basic magnesium carbonate, dolomite, hydrotalcite, calcium hydroxide, barium hydroxide, tin oxide, hydrate of tin oxide, borax, zinc borate, zinc metaborate, barium metaborate, zinc carbonate, magnesium-calcium carbonate, calcium carbonate, barium carbonate, molybdenum oxide , antimony oxide, red phosphorus, mica, clay, kaolin, talc, zeolite, wollastonite, montmorillonite, silicon dioxide (quartz, fumed silica, precipitated silica, anhydrous silicic acid, fused silica, crystalline silica, ultrafine amorphous silica, etc.), potassium titanate, magnesium sulfate, sepiolite, xonotlite, aluminum borate, barium sulfate, barium titanate, zirconium oxide, cerium, tin, indium, carbon, sulfur, cobalt, molybdenum, strontium, chromium, barium, lead, indium oxide, diamond, magnesium, platinum, zinc, manganese, stainless steel, etc. Among them, aluminum hydroxide, nickel, etc. are preferred.
[0057] In order to improve the dispersibility in the binder resin, the inorganic filler may be subjected to a surface treatment such as a silane coupling treatment or a stearic acid treatment.
[0058] Specific examples of organic fillers include polystyrene fillers, benzoguanamine fillers, polyethylene fillers, polypropylene fillers, silicone fillers, urea-formalin fillers, styrene / methacrylic acid copolymers, fluorine fillers, acrylic fillers, polycarbonate fillers, polyurethane fillers, polyamide fillers, epoxy resin fillers, and thermosetting resin hollow fillers.
[0059] It should be noted that, among the organic fillers, as silicone fillers, specifically, silicone rubber particles obtained by three-dimensionally crosslinking straight-chain organopolysiloxane (refer to Japanese Patent Laid-Open No. 63-77942, Japanese Patent Laid-Open No. 3-93834, Japanese Patent Laid-Open No. 04-198324), powdered silicone rubber (refer to U.S. Patent No. 3843601, Japanese Patent Laid-Open No. 62-270660, Japanese Patent Laid-Open No. 59-96122), etc. can be used. In addition, silicone composite particles having a structure in which the surface of the silicone rubber particles obtained by the above method is coated with a silicone resin which is a cured polyorganosilsesquioxane (refer to Japanese Patent Laid-Open No. 7-196815), wherein the cured polyorganosilsesquioxane is (R′SiO 3 / 2 ) n (R' represents a substituted or unsubstituted monovalent hydrocarbon group) indicates that it has a structure cross-linked into a three-dimensional network.
[0060] As the silicone particles, TREFIL E-500, TREFIL E-600, TREFIL E-601, TREFILE-850 and the like commercially available from Toray Dow Corning Silicones Co., Ltd. under the above-mentioned trade names can be used. In addition, KMP-600, KMP-601, KMP-602, KMP-605 and the like commercially available from Shin-Etsu Chemical Co., Ltd. can be used.
[0061] In addition, as other silicone fillers, acrylic modified silicone particles can be used. Examples of acrylic modified silicone particles include emulsified graft polymers of polyorganosiloxane represented by the following general formula (C), acrylic ester monomers and / or methacrylic ester monomers, and monomers containing functional groups copolymerizable therewith.
[0062] [Chemical formula 3]
[0063]
[0064] (In the above general formula (C), R 5 and R 6 Each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and X 1 , X 2 , X 3 , X 4 , X 5 , and X 6 each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a hydroxyl group, and Y 1 and Y 2 Each independently represents X 1 or -[O-Si(X 7 )(X 8 )] c -X 9 The group shown, X 7 , X 8 and X 9 Each independently represents a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or a hydroxyl group, and X 1 , X 2 , X 3 , X 4 , X 5 , X 6 , X 7 , X 8 , and X 9 and Y 1 and Y 2 At least two of the groups are hydroxyl groups, and a, b and c are each independently an integer satisfying 0≤a≤1000, an integer satisfying 100≤b≤10000, and an integer satisfying 1≤c≤1000. )
[0065] In the general formula (C), R 5 or R 6 The alkyl group having 1 to 20 carbon atoms shown may be straight-chain or branched, or may be cyclic. Specifically, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, cyclopentyl, cyclohexyl, cycloheptyl, etc. may be mentioned. These alkyl groups may be substituted with halogen atoms, acryloyloxy, methacryloyloxy, carboxyl, alkoxy, alkenyloxy, amino, and amino groups substituted with alkyl / alkoxy / (meth)acryloyloxy.
[0066] As R 5 or R 6 Examples of the aryl group having 6 to 20 carbon atoms include phenyl, tolyl, naphthyl and the like.
[0067] As R 5 or R 6 , preferably methyl.
[0068] In the general formula (C), X 1 ~X 9 The alkyl group having 1 to 20 carbon atoms and the aryl group having 6 to 20 carbon atoms represented by 5 or R 6 The alkyl group and aryl group exemplified are the same groups.
[0069] As X 1 ~X 9 Examples of the alkoxy group having 1 to 20 carbon atoms include methoxy, ethoxy, propoxy, butoxy, hexyloxy, heptyloxy, octyloxy, decyloxy and tetradecyloxy.
[0070] In the general formula (C), a, b and c are integers of 0≤a≤1000, 100≤b≤10000, and 1≤c≤1000, and a is preferably an integer of 0 to 200. If a is greater than 1000, the strength of the obtained film becomes insufficient. b is preferably an integer of 1000 to 5000. If b is less than 100, the softness of the film is insufficient, and if it is greater than 10000, it is difficult to form a solid such as particles. c is preferably an integer of 1 to 200.
[0071] In addition, from the viewpoint of crosslinking properties, the polyorganosiloxane represented by the general formula (C) has at least 2, preferably 2 to 4, hydroxyl groups in one molecule, and preferably has the hydroxyl groups at both ends of the molecular chain.
[0072] Examples of the acrylic acid ester monomer or methacrylic acid ester monomer include methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, and cyclohexyl methacrylate.
[0073] Examples of the monomer containing a functional group copolymerizable with the acrylic acid ester monomer and / or the methacrylic acid ester monomer include monomers having an unsaturated bond such as a carboxyl group, an amide group, a hydroxyl group, a vinyl group, and an allyl group.
[0074] The acrylic modified silicone particles are preferably obtained by mixing 100 parts by mass of the polyorganosiloxane represented by the general formula (C), 10 to 100 parts by mass of an acrylic ester monomer and / or a methacrylic ester monomer, and 0.01 to 20 parts by mass of a monomer containing a functional group copolymerizable therewith, and performing emulsion graft polymerization. The conditions in the emulsion graft polymerization are not particularly limited, and as the initiator used in the polymerization, a known free radical initiator commonly used for acrylic polymers can be used. In addition, the emulsifier can also use a known anionic surfactant or nonionic surfactant.
[0075] The acrylic modified silicone particles can be granulated and powdered by the following methods. That is, spray drying, airflow drying, etc. are mentioned, but spray drying is preferred in view of productivity. Powdering is preferably performed by heat drying, preferably at 80 to 150°C.
[0076] As the acrylic-modified silicone particles, for example, commercially available products such as CHALINE R-170S and CHALINE R-200 (both manufactured by Nissin Chemical Industry Co., Ltd.) may be used.
[0077] As the shape of the filler particles of the present embodiment, there is no particular restriction, can be suitably selected according to the purpose, can be a regular shape, can also be an irregular shape. As the specific example of the shape of the filler particles, polygonal, cubic, elliptical, spherical, needle-shaped, flat, flaky, etc. can be enumerated. The filler particles of these shapes can be used alone 1 kind, and can also be used in combination with more than 2 kinds. In addition, it can also be the particles that the filler particles of these shapes are agglomerated. Wherein, as the shape of the filler particles, preferably elliptical, spherical, polygonal. When the shape of the filler particles is elliptical, spherical, polygonal, etc., when the adhesive tape is extended, the sliding of the adhesive layer relative to the adherend becomes good, and the adhesive tape can be peeled off more simply and more quickly.
[0078] The particle size distribution (D90 / D10) of the filler particles of the present embodiment is not particularly limited and can be appropriately selected according to the purpose, preferably 2.5 to 20, more preferably 2.5 to 15, and further preferably 2.5 to 5 from the perspective of impact resistance. When the particle size distribution (D90 / D10) of the filler is 2.5 or more, the elongation peeling property of the adhesive tape is improved, and the adhesive tape can be peeled off more easily and more quickly, and it is not easy to break even when the adhesive tape does not have a substrate layer, or when the adhesive tape has a substrate layer and the thickness of the substrate layer is thin. In addition, when the particle size distribution (D90 / D10) of the filler is 20 or less, the bonding performance such as high load holding power, initial bonding strength, impact resistance, shear bonding strength, and cleavage bonding strength is improved.
[0079] The particle size distribution (D90 / D10) of the filler in the present embodiment can be obtained by, for example, measuring the average particle size of the filler using a measuring device (Microtrac) using a laser diffraction scattering method and converting it into a particle size distribution.
[0080] The average particle size D50 of the filler particles of this embodiment is preferably 0.1 to 40 μm, more preferably 5 to 40 μm, further preferably 10 to 35 μm, further preferably 10 to 30 μm, and particularly preferably 10 to 25 μm. When the average particle size D50 of the filler particles is 0.1 μm or more, the elongation peeling property of the adhesive tape is improved, and the adhesive tape can be peeled off more easily and quickly, and it is not easy to break even when the adhesive tape does not have a substrate layer, or when the adhesive tape has a substrate layer and the thickness of the substrate layer is thin. In addition, when the average particle size D50 of the filler particles is 40 μm or less, the bonding properties such as high load holding force, initial bonding force, impact resistance, shear bonding force, and cleavage bonding force are improved.
[0081] In addition, the average particle diameter D50 of the filler particles in the present embodiment refers to a volume average particle diameter, and can be measured by using a measuring machine (Microtrac) using a laser diffraction scattering method, for example.
[0082] It should be noted that, when the silicone rubber particles or silicone composite particles are used as filler particles of the present embodiment, the average particle size D50 of the silicone rubber particles or silicone composite particles is preferably 0.1 to 40 μm, and more preferably 5 to 40 μm. When the average particle size D50 is 0.1 μm or more, the effect of reducing the bonding area caused by the filler particles when the adhesive tape is extended becomes greater, and when it is 40 μm or less, the adhesive force of the adhesive tape can be maintained at a high level.
[0083] In addition, when the above-mentioned acrylic modified silicone particles are used as filler particles of the present embodiment, the average particle diameter D50 of the acrylic modified silicone particles is preferably 0.1 to 40 μm, more preferably 5 to 40 μm, further preferably 5 to 30 μm, and further preferably 10 to 25 μm. When the average particle diameter D50 is 0.1 μm or more, the effect of reducing the bonding area caused by the filler particles when the adhesive tape is extended becomes greater, and when it is 40 μm or less, the adhesive force of the adhesive tape can be maintained at a high level.
[0084] In the present embodiment, D50 / T, which is the relationship between the average particle size D50 of the filler particles and the average thickness T of the adhesive layer, is in the range of 0.05 to 1.0. In addition, D50 / T is preferably in the range of 0.05 to 0.95, more preferably in the range of 0.10 to 0.75, and particularly preferably in the range of 0.20 to 0.60. When D50 / T is above 0.05, the adhesive force of the adhesive tape during elongation becomes lower, and the adhesive tape can be peeled off more easily and quickly, and it is not easy to break even when the adhesive tape does not have a substrate layer, or when the adhesive tape has a substrate layer and the thickness of the substrate layer is thin. In addition, when D50 / T is below 1.0, it is advantageous in that the adhesive properties such as high load holding power, initial adhesion, impact resistance, shear adhesion, and cleavage adhesion are also more excellent.
[0085] Relative to 100 parts by mass of the triblock copolymer with repeating units shown in the general formula (1) described later, the content of the filler particles in the adhesive layer of the present embodiment is preferably in the range of 5 to 200 parts by mass, more preferably in the range of 10 to 100 parts by mass, and more preferably in the range of 20 to 50 parts by mass. When the content of the filler particles is 5 parts by mass or more relative to 100 parts by mass of the triblock copolymer with repeating units shown in the general formula (1), the adhesive tape can be peeled off more simply and more quickly. In addition, when the content of the filler particles is 200 parts by mass or less relative to 100 parts by mass of the triblock copolymer with repeating units shown in the general formula (1), it is possible to prevent the adhesive composition from remaining on the adherend, prevent the impact resistance from deteriorating, and prevent the shear adhesion and cleavage adhesion from weakening.
[0086] The content of the filler particles in the adhesive layer of the present embodiment can be appropriately adjusted when preparing the adhesive composition as a precursor of the adhesive layer.
[0087] When the silicone rubber particles or silicone composite particles are used as filler particles, the content of the silicone rubber particles or silicone composite particles is preferably in the range of 10 to 100 parts by mass based on 100 parts by mass of the triblock copolymer having repeating units represented by the general formula (1).
[0088] When the acrylic modified silicone particles are used as filler particles, the content of the acrylic modified silicone particles is preferably in the range of 10 to 50 parts by mass based on 100 parts by mass of the triblock copolymer having a repeating unit represented by the general formula (1).
[0089] The volume ratio of the filler particles relative to the volume of the entire adhesive layer is preferably 4 to 40%, more preferably 5 to 30%, further preferably 5 to 20%, and most preferably 5 to 15%. By making the volume ratio of the filler particles 4% or more, the adhesive tape can be peeled off more simply and more quickly. In addition, by making the volume ratio of the filler particles 40% or less, it is possible to prevent the adhesive layer from remaining on the adherend, prevent the impact resistance from deteriorating, and prevent the shear bonding strength and cleavage bonding strength from weakening.
[0090] The volume ratio of the filler particles to the adhesive layer can be calculated from the following formulas (1) to (3).
[0091] Binder resin *1 Mass A(g) / binder resin *1 Density A(g / cm 3 )=Binder resin *1 Volume A(cm 3 )···Mathematical formula (1)
[0092] The mass of filler particles B (g) / the density of filler particles B (g / cm 3 ) = volume of filler B (cm 3 )···Mathematical formula (2)
[0093] The volume of filler particles B (cm 3 ) / (Binder resin *1 Volume A(cm 3 ) + volume of filler particles B (cm 3 ))×100=volume ratio of filler particles (%)···Mathematical formula (3)
[0094] It should be noted that in the above mathematical formulas (1) and (3), *1 The binder resin shown may contain other components described below.
[0095] In addition, the density is a value measured in accordance with JIS Z 8804.
[0096] <Triblock copolymer>
[0097] The adhesive layer of the adhesive tape of the present embodiment contains a triblock copolymer having a repeating unit represented by the following general formula (1).
[0098] [Chemical formula 4]
[0099]
[0100] (In the above general formula (1), A, B and C each independently represent a repeating unit, A and C each independently represent an alkyl methacrylate monomer unit, B represents an alkyl acrylate monomer unit, p, q and r each independently represent the degree of polymerization of each monomer unit, A and C may be the same, or may be an alkyl methacrylate monomer unit with a different chemical structure. In the above general formula (1), * represents a connecting bond to other atoms.)
[0101] In the above general formula (1), A and C represent repeating units different from B, and represent alkyl methacrylate monomer units. In addition, A and C are each independent and may be the same alkyl methacrylate monomer units, or may be alkyl methacrylate monomer units having different chemical structures. The "alkyl methacrylate monomer unit" in this specification refers to a structural unit derived from an alkyl methacrylate monomer when an alkyl methacrylate monomer is (co)polymerized or graft-polymerized, that is, a repeating unit derived from a methacrylate monomer. The alkyl methacrylate monomer unit in the present invention is preferably represented by the following general formula (2).
[0102] [Chemical formula 5]
[0103]
[0104] (In the above general formula (2), R 1 represents an alkyl group having 1 to 12 carbon atoms, in which one or more hydrogen atoms may be substituted by R 2 Substitution, the substituent R 2 represents a halogen atom, an amino group, or a cyano group. ).
[0105] In the above general formula (2), from the viewpoint of removability and high load holding power, R 1 More preferably, it is an alkyl group having 1 to 12 carbon atoms, and still more preferably, it is an alkyl group having 1 to 4 carbon atoms. 1The alkyl group having 1 to 12 carbon atoms may be straight-chain, branched or cyclic. From the viewpoint of adhesive strength, it is preferably straight-chain or branched, and more preferably straight-chain. Examples of the alkyl group having 1 to 12 carbon atoms include straight-chain or branched alkyl groups such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, hexyl, octyl, nonyl, decyl, undecyl, dodecyl, and cyclic alkyl groups such as cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, and dicyclopentyl. In addition, examples of the alkyl group having 1 to 4 carbon atoms include straight-chain or branched alkyl groups such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, and tert-butyl, and cyclic alkyl groups such as cyclobutyl. As the alkyl group having 1 to 4 carbon atoms, from the viewpoint of removability and high load holding power, a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, and a tert-butyl group are preferred, and a methyl group is more preferred.
[0106] In the above general formula (2), preferably R 1 is any alkyl group selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl or cyclobutyl, and one or more hydrogen atoms in the alkyl group may be substituted with a substituent R 2 (halogen atom, amino group, cyano group) substitution.
[0107] In the present embodiment, for example, the methacrylate alkyl ester monomer is not particularly limited, and examples thereof include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, pentadecyl methacrylate, cyclohexyl methacrylate, lauryl methacrylate, tridecyl methacrylate, 2-hexyldecyl methacrylate, etc. Among them, methyl methacrylate is preferred from the viewpoint of high load holding power and disassembly properties.
[0108] In the above general formula (1), B represents a repeating unit different from A and C, and represents an alkyl acrylate monomer unit. The "alkyl acrylate monomer unit" in this specification refers to a structural unit derived from an alkyl acrylate monomer when an alkyl acrylate monomer is (co)polymerized or graft-polymerized, that is, a repeating unit derived from an acrylate monomer. The alkyl acrylate monomer unit in the present invention is preferably represented by the following general formula (3).
[0109] [Chemical formula 6]
[0110]
[0111] (In the above general formula (3), R 3represents an alkyl group having 1 to 12 carbon atoms, in which one or more hydrogen atoms may be substituted by R 4 Substitution, the substituent R 4 represents a halogen atom, an amino group, or a cyano group. ).
[0112] In the above general formula (3), from the viewpoint of adhesiveness, R 3 An alkyl group having 1 to 12 carbon atoms is more preferred, and an alkyl group having 4 to 8 carbon atoms is further preferred. The alkyl group may be linear, branched, or cyclic, and is preferably linear or branched from the viewpoint of adhesiveness.
[0113] In the above general formula (3), examples of the alkyl group having 1 to 12 carbon atoms are the same as the examples of the alkyl group having 1 to 12 carbon atoms in the above general formula (2).
[0114] In the above general formula (3), preferably R 3 It is any alkyl group selected from the group consisting of n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, hexyl, octyl, cyclohexyl, cycloheptyl and cyclooctyl, and one or more hydrogen atoms in the alkyl group may be substituted by a substituent R4 (halogen atom, amino group, cyano group).
[0115] In the present embodiment, examples of the acrylic acid alkyl ester monomer include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, amyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, lauryl acrylate, etc. Among them, n-butyl acrylate, 2-ethylhexyl acrylate, and copolymers thereof are preferred from the viewpoint of achieving both adhesive strength and removability.
[0116] In the above general formula (1), p, q and r each independently represent the degree of polymerization of each monomer unit. The respective values of p, q and r are related to the molecular weight, etc. p / (p+q+r) is preferably 0.02 to 0.40, and more preferably 0.05 to 0.37. q / (p+q+r) is preferably 0.20 to 0.95, and more preferably 0.25 to 0.90. r / (p+q+r) is preferably 0.02 to 0.40, and more preferably 0.05 to 0.37.
[0117] In the present embodiment, the triblock copolymer preferably has a repeating unit represented by the following general formula (4).
[0118] [Chemical formula 7]
[0119]
[0120] (In the above general formula (4), R 1 and R 5Each independently represents an alkyl group having 1 to 4 carbon atoms, and one or more hydrogen atoms in the alkyl group may be substituted by R 2 Substitution, the substituent R 2 represents a halogen atom, an amino group, or a cyano group,
[0121] R 3 represents an alkyl group having 4 to 8 carbon atoms, in which one or more hydrogen atoms may be substituted by R 4 Substitution, the substituent R 4 represents a halogen atom, an amino group, or a cyano group, and p, q, and r each independently represent the degree of polymerization of each monomer unit. ).
[0122] In the above general formula (4), R 1 It can be applied to R in the above general formula (2) 1 In the above general formula (4), R 3 The same as R in the above general formula (3) can be applied 3 In the above general formula (4), R 5 It can be applied to R in the above general formula (2) 1 In the above general formula (4), p, q and r can be applied in the same form as p, q and r in the above general formula (1). In the above general formula (4), R 1 and R 5 It can be the same or different.
[0123] In this embodiment, when the triblock copolymer is represented by the above general formula (4), R 1 It is preferably selected from the group consisting of a linear or branched alkyl group such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and a cyclobutyl group, 3 Preferably, R is selected from the group consisting of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, hexyl, octyl, nonyl, decyl or undecyl. 5 It is preferably selected from the group consisting of linear or branched alkyl groups such as methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and cyclobutyl, and preferably p / (p+q+r) is 0.02 to 0.40, q / (p+q+r) is 0.20 to 0.95, and r / (p+q+r) is 0.02 to 0.40.
[0124] In the triblock copolymer of the present invention, it is preferred that A and C in the general formula (1) are the same. Specifically, when the triblock copolymer has a repeating unit represented by the general formula (4), it is preferred that R 1 With R 5For the same group, p / (p+q+r) is 0.02-0.40, q / (p+q+r) is 0.20-0.95, and r / (p+q+r) is 0.02-0.40.
[0125] In the triblock copolymer having repeating units represented by the general formula (1), when A and C are the same (ABA type triblock copolymer), a higher elastic modulus can be secured, and therefore, it is easier to secure an adhesive force with high load holding power, excellent removability over time, and excellent storage stability.
[0126] --Molecular weight--
[0127] The weight average molecular weight Mw of the triblock copolymer is preferably 50,000 to 300,000, and the number average molecular weight Mn is preferably 50,000 to 300,000. More preferably, the weight average molecular weight Mw of the triblock copolymer is 100,000 to 250,000, and the number average molecular weight Mn is 100,000 to 250,000, and further preferably, the weight average molecular weight Mw of the triblock copolymer is 130,000 to 230,000, and the number average molecular weight Mn is 130,000 to 230,000.
[0128] When the weight average molecular weight Mw of the triblock copolymer is within the above range, it is preferred from the viewpoint of adhesion, removability and high load holding power, and when the number average molecular weight Mn of the triblock copolymer is within the above range, it is preferred from the viewpoint of adhesion, removability and high load holding power.
[0129] Here, the weight average molecular weight Mw and number average molecular weight Mn of the triblock polymer measured by the GPC method are standard polystyrene conversion values measured using a GPC apparatus (HLC-8329GPC, manufactured by Tosoh Corporation), and the measurement conditions are as follows.
[0130] -Measurement conditions-
[0131] Sample concentration: 0.5 mass% (tetrahydrofuran (THF) solution)
[0132] Sample injection volume: 100μL
[0133] ·Eluent: THF
[0134] Flow rate: 1.0mL / min
[0135] ·Measurement temperature: 40℃
[0136] ·Main column (Honkara): TSKgel GMHHR-H (20) 2 pieces
[0137] Guard column: TSKgel HXL-H
[0138] Detector: Differential refractometer
[0139] · Standard polystyrene molecular weight: 10,000 to 20,000,000 (manufactured by Tosoh Corporation)
[0140] -- Stereoregularity --
[0141] The triblock copolymer and / or a partial structure (e.g., block) of the triblock copolymer preferably has stereoregularity (stereoregularity). Specifically, the triblock copolymer and / or a partial structure (e.g., block) of the triblock copolymer may have any stereoregularity of isotactic, syndiotactic, and atactic, or may have a plurality of blocks having any of these stereoregularities.
[0142] As a preferred embodiment of the above triblock copolymer, it is preferred that "-(A)" in the general formula (1) p The syndiotactic stereoregularity of the polymer block of the -" portion shows a ratio of rr triads of 65% or more, and more preferably a ratio of rr triads of 75 to 95%.
[0143] As a preferred embodiment of the above triblock copolymer, it is preferred that "-(C) r The syndiotactic stereoregularity of the polymer block of the -" portion shows a ratio of rr triads of 65% or more, and more preferably a ratio of rr triads of 75 to 95%.
[0144] As a preferred embodiment of the above triblock copolymer, "-(B)" in the general formula (1) q The polymer block of the "-" portion preferably exhibits atactic structure.
[0145] In the above triblock copolymer, the ratio of rr triads is 65% or more, "-(A) p In the case of a polymer block having a "-" portion, the removability and the retention force at high temperature are excellent.
[0146] Generally, the syndiotacticity of a polymer is expressed by the ratio of chains (triads) composed of three monomer units to rr. In this specification, it is calculated by NMR measurement of the polymer. Specifically, 13 The signal peaks representing the triad sequence in C-NMR vary depending on the type of polymer, measurement solvent, measurement temperature and other conditions, so the signals need to be identified and quantified according to the respective measurement conditions. It should be noted that in this specification, the sample dissolved in deuterated chloroform was measured at 50°C.
[0147] Preferred embodiments of the triblock copolymer include polymethyl methacrylate block-polyn-butyl acrylate block-polymethyl methacrylate, polyethyl methacrylate block-polyn-butyl acrylate block-polyethyl methacrylate, polypropyl methacrylate block-polyn-butyl acrylate block-polypropyl methacrylate, polymethyl methacrylate block-polyt-butyl acrylate block-polymethyl methacrylate, polymethyl methacrylate block-polypropyl acrylate block-polymethyl methacrylate, and the like.
[0148] The molecular weight distribution of the triblock copolymer as a whole is preferably in the range of 1.0 to 2.3, more preferably in the range of 1.00 to 1.50, in terms of the ratio of weight average molecular weight to number average molecular weight.
[0149] In this embodiment, when A and C in the general formula (1) are different repeating units, from the viewpoint of adhesive properties, the "-(A)" contained in the molecule of the triblock copolymer is p -" (the total weight of the polymer block p The total weight of the polymer block in the "-" part is called a.) and "-(B) q -" (the total weight of the polymer block of the "- (B) q The total weight of the polymer block of the -" portion is referred to as b.) The ratio a / b mass ratio is preferably in the range of 2 / 98 to 67 / 33, more preferably in the range of 5 / 95 to 60 / 40.
[0150] In this embodiment, when A and C in the general formula (1) are different repeating units, from the viewpoint of adhesive properties, the "-(C)" contained in the molecule of the triblock copolymer is r -" (the total weight of the polymer block of the "- (C) r The total weight of the polymer block of the "-" part is called C.) and "-(B) q The ratio of the total weight of the polymer block of the -" portion is preferably in the range of 2 / 98 to 67 / 33, and more preferably in the range of 5 / 95 to 60 / 40, in terms of c / b mass ratio.
[0151] In this embodiment, when A and C in the general formula (1) are the same repeating units, the "-(A)" contained in the molecule of the triblock copolymer is p -" polymer block and "-(C) r -" (replace "-(A) p -" polymer block and "-(C) r The total weight of the polymer block of the "-" part is called d.) and "-(B) qThe ratio of the total weight of the polymer block of the -" portion (referred to as b) is preferably within the range of 5 / 95 to 80 / 20, and more preferably within the range of 10 / 90 to 75 / 25, as a d / b mass ratio.
[0152] The triblock copolymer may be modified with a functional group such as a hydroxyl group, a carboxyl group, an acid anhydride group, an amino group, a trimethoxysilyl group, etc. in the molecular side chain or at the molecular main chain terminal as required within a range not impairing the effects of the present invention.
[0153] --Method for producing triblock copolymer--
[0154] The method for producing the triblock copolymer is not particularly limited and can be appropriately selected from conventionally known production methods, such as a method in which block copolymers are sequentially polymerized by anionic living polymerization or cationic living polymerization. In addition, when the triblock copolymer has stereoregularity (e.g., syndiotactic stereoregularity), a known method using an organic metal complex can be used.
[0155] As an example of a method for producing the above-mentioned triblock copolymer, the triblock copolymer can be produced by the following method, which comprises: using a polymerization initiator in an inert polymerization solvent, sequentially polymerizing an alkyl methacrylate monomer as a main component and polymerizing an alkyl acrylate monomer as a main component and / or a monomer having the alkyl methacrylate monomer as a main component in a manner to obtain a desired block bonding order.
[0156] As a more specific method for producing the triblock copolymer, a method is as follows: first, an alkyl methacrylate monomer is polymerized in a polymerization solvent using a polymerization initiator to form a polyalkyl methacrylate block having an active terminal (corresponding to "-(A)" in the general formula (1)). p -" part). Second, an alkyl acrylate monomer is polymerized from the active end of the polyalkyl methacrylate to obtain an alkyl methacrylate-alkyl acrylate binary block copolymer having an active end (corresponding to "-(A)" in the general formula (1) p -(B) q -" part). Third, a part of the alkyl methacrylate-alkyl acrylate binary block copolymer having an active terminal is reacted with a coupling agent to form a coupled alkyl methacrylate-alkyl acrylate-alkyl methacrylate triblock copolymer (corresponding to "-(A)" of the general formula (1) p -(B) q -(C) r -" part). At this time, the polymerization is terminated by reacting with a polymerization terminator such as alcohol, if necessary.
[0157] Examples of the polymerization initiator include organic metal compounds such as organic lithium compounds and organic metal complexes.
[0158] Examples of the above-mentioned organolithium compounds include alkyl lithiums such as tert-butyl lithium, compounds obtained by reacting alkyl lithiums with 1,1-diphenylethylene, diphenylmethane, etc. In addition, these organolithium compounds may be used in combination with inorganic salts such as lithium chloride, lithium salts of alkoxides such as 2-(2-methoxyethoxy)lithium ethoxide, and organoaluminum compounds such as diisobutyl(2,6-di-tert-butyl-4-methylphenoxy)aluminum.
[0159] As the above-mentioned organic metal complex, there can be mentioned rare earth metal complexes having pentamethylcyclopentadienyl as a ligand, such as bis(pentamethylcyclopentadienyl) methyltetrahydrofuran samarium, bis(pentamethylcyclopentadienyl) methyltetrahydrofuran yttrium, etc. In addition, these organic metal complexes can also be used in combination with alkyl aluminums such as trimethylaluminum.
[0160] As the polymerization solvent, there can be used hydrocarbon solvents such as benzene, toluene, and xylene; halogenated hydrocarbon solvents such as chloroform, dichloromethane, and carbon tetrachloride; and ether solvents such as tetrahydrofuran and diethyl ether.
[0161] <Other binder resins>
[0162] The adhesive layer of the adhesive tape of this embodiment contains the triblock copolymer having repeating units represented by the general formula (1) as a binder resin, but may further contain a diblock copolymer, an acrylic binder resin, a rubber-based binder resin, etc. as a binder resin other than the triblock copolymer.
[0163] In the adhesive layer of the adhesive tape of the present embodiment, the triblock copolymer preferably accounts for 50 to 100% by mass, and more preferably accounts for 70 to 100% by mass, based on the entire binder resin.
[0164] When the content of the triblock copolymer in the binder resin used in the adhesive layer is within the above range, it is easy to achieve both adhesiveness, disassembly properties, and high load holding power.
[0165] --Diblock copolymers--
[0166] The diblock copolymer may include a diblock copolymer having a repeating unit represented by the following general formula (5).
[0167] [Chemical formula 8]
[0168]
[0169] (In the above general formula (5), D and E each independently represent a repeating unit, D represents an alkyl methacrylate monomer unit, E represents an alkyl acrylate monomer unit, and s and t each independently represent the degree of polymerization of each monomer unit. In the above general formula (5), * represents a connecting bond to other atoms.)
[0170] In this embodiment, when a triblock copolymer and a diblock copolymer are used in combination as an adhesive resin, it is easy to ensure high elastic modulus and initial adhesion, and therefore, it is easier to ensure high load holding power, time-dependent removability, and initial adhesion. In particular, when the adhesive tape is stretched, the filler particles in the adhesive layer can be kept exposed on the surface for a long time, so that the effect of the filler particles complements each other and exerts an excellent synergistic effect.
[0171] The alkyl methacrylate monomer units and alkyl acrylate monomer units in the general formula (5) can be in the same form as the alkyl methacrylate monomer units and alkyl acrylate monomer units in the general formula (1).
[0172] The above diblock copolymer preferably has a repeating unit represented by the following general formula (6):
[0173] [Chemical formula 9]
[0174]
[0175] (In the above general formula (6), R 6 represents an alkyl group having 1 to 12 carbon atoms, in which one or more hydrogen atoms may be substituted by R 8 Substitution, the substituent R 8 represents a halogen atom, an amino group, or a cyano group, R 7 represents an alkyl group having 1 to 12 carbon atoms, in which one or more hydrogen atoms may be substituted by R 9 Substitution, the substituent R 9 represents a halogen atom, an amino group, or a cyano group, and s and t each independently represent the degree of polymerization of each monomer unit. ).
[0176] In the above general formula (6), R 6 It can be applied to R in the above general formula (2) 1 In the above general formula (6), R 7 The same as R in the above general formula (3) can be applied 3 In the above general formula (6), s and t can be in the same form as p and q in the above general formula (1).
[0177] In this embodiment, the diblock copolymer preferably has a weight average molecular weight Mw of 50,000 to 300,000 and a number average molecular weight Mn of 50,000 to 300,000. The weight average molecular weight can be measured by the method for measuring the weight average molecular weight of the triblock copolymer in the present invention.
[0178] In the above general formula (6), s and t each independently represent the degree of polymerization of each monomer unit. The values of s and t are related to the molecular weight, etc. s / (s+t) is preferably 0.01 to 0.99, more preferably 0.1 to 0.9. t / (s+t) is preferably 0.01 to 0.99, more preferably 0.1 to 0.9.
[0179] In the present embodiment, as the content of the above-mentioned diblock copolymer, there is no particular limitation and can be appropriately selected according to the purpose. In the present embodiment, relative to 100 parts by mass of the triblock copolymer, it is preferred to contain 0 to 100 parts by mass of the diblock copolymer, more preferably 1 to 50 parts by mass, and further preferably 10 to 50 parts by mass. When the range of the content of the tackifying resin in the adhesive layer is the above range, it is easy to ensure the adhesion with the adherend.
[0180] --Acrylic Binder Resin--
[0181] The acrylic binder resin is not particularly limited and may be appropriately selected depending on the intended purpose. Examples thereof include resins containing an acrylic polymer and, if necessary, additives such as a tackifier resin and a crosslinking agent.
[0182] The acrylic polymer has a chemical structure other than the triblock copolymer having repeating units represented by the general formula (1), and can be produced, for example, by polymerizing a (meth)acrylic acid ester monomer.
[0183] As the (meth)acrylate monomer, for example, an alkyl (meth)acrylate having an alkyl group having 1 to 12 carbon atoms, etc. can be used.
[0184] Specific examples of the alkyl (meth)acrylate having an alkyl group with 1 to 12 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0185] As the alkyl (meth)acrylate having an alkyl group having 1 to 12 carbon atoms, an alkyl (meth)acrylate having an alkyl group having 4 to 12 carbon atoms is preferably used, and an alkyl (meth)acrylate having an alkyl group having 4 to 8 carbon atoms is more preferably used. From the perspective of ensuring excellent adhesion to an adherend, n-butyl acrylate is particularly preferably used.
[0186] The (meth)acrylic acid alkyl ester having an alkyl group having 1 to 12 carbon atoms is preferably used in an amount within a range of 0 to 50% by mass, more preferably 0 to 30% by mass, based on the total amount of monomers used in the production of the acrylic polymer.
[0187] As the monomers that can be used for producing the acrylic polymer, in addition to the above-mentioned monomers, a highly polar vinyl monomer may be used as necessary.
[0188] Examples of the highly polar vinyl monomer include a vinyl monomer having a hydroxyl group, a vinyl monomer having a carboxyl group, a vinyl monomer having an amide group, etc. These may be used alone or in combination of two or more.
[0189] Specific examples of the vinyl monomer having a hydroxyl group include (meth)acrylic acid monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 6-hydroxyhexyl (meth)acrylate.
[0190] Specific examples of the vinyl monomer having a carboxyl group include (meth)acrylic acid monomers such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, (meth)acrylic acid dimer, crotonic acid, and ethylene oxide-modified succinic acid acrylate. Among them, acrylic acid is preferred.
[0191] Specific examples of the vinyl monomer having an amide group include (meth)acrylic acid monomers such as N-vinyl pyrrolidone, N-vinyl caprolactam, acryloyl morpholine, acrylamide, and N,N-dimethylacrylamide.
[0192] The high polarity vinyl monomer is preferably used in an amount of 1.5 to 20% by mass, more preferably 1.5 to 10% by mass, relative to the total amount of monomers used in the production of the acrylic polymer. When used in an amount of 2 to 8% by mass, an adhesive layer having a balance in cohesive force, holding power and adhesiveness can be formed, which is further preferred.
[0193] The method for producing the acrylic polymer is not particularly limited and can be appropriately selected from known methods according to the purpose, and examples thereof include methods of polymerizing monomers by polymerization methods such as solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization. Among them, the acrylic polymer is preferably produced by solution polymerization or bulk polymerization.
[0194] During the polymerization, as necessary, peroxide-based thermal polymerization initiators such as benzoyl peroxide and lauroyl peroxide, azo thermal polymerization initiators such as azobisisobutyronitrile, acetophenone-based photopolymerization initiators, benzoin ether-based photopolymerization initiators, benzyl ketal-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzophenone-based photopolymerization initiators, etc. can be used.
[0195] Regarding the weight average molecular weight of the acrylic polymer obtained by the above method, it is preferred to use an acrylic polymer having a weight average molecular weight of 300,000 to 3,000,000 measured in terms of standard polystyrene using gel permeation chromatography (GPC) in the same method and conditions as for the above triblock copolymer, and it is more preferred to use an acrylic polymer having a weight average molecular weight of 500,000 to 2,500,000.
[0196] In the adhesive layer, the acrylic adhesive resin preferably accounts for 0 to 50% by mass, and more preferably accounts for 0 to 30% by mass, relative to the entire adhesive resin. When the content of the acrylic adhesive resin in the adhesive resin used in the adhesive layer is within the above range, it is easy to achieve both adhesion, removability over time, and high load holding power.
[0197] --Rubber-based adhesive resin--
[0198] The rubber-based binder resin is not particularly limited, and examples thereof include resins containing a rubber material generally used as a binder resin, such as a synthetic rubber-based binder resin and a natural rubber-based binder resin, and, if necessary, an additive such as a tackifier resin.
[0199] As rubber material, for example, block copolymers of aromatic vinyl compounds and conjugated diene compounds can be enumerated, specifically, styrene resins such as styrene-isoprene copolymer, styrene-isoprene-styrene copolymer, styrene-isoprene-butadiene-styrene copolymer, styrene-butadiene-styrene copolymer, styrene-ethylene-butylene copolymer, styrene-ethylene-propylene copolymer and their hydrides can be enumerated. They can be used alone or in combination with more than two kinds. Wherein, the combination of more than two kinds of styrene resins can give excellent adhesive properties and holding power to the adhesive tape, so it is more preferred, and particularly preferably, styrene-isoprene copolymer and styrene-isoprene-styrene copolymer are used in combination.
[0200] The above-mentioned styrene resin can be, for example, a styrene resin of a single structure of a linear structure, a branched structure or a multi-branched structure, or a styrene resin of a mixed structure of different structures. When a styrene resin rich in a linear structure is used for an adhesive layer, excellent bonding properties can be imparted to the adhesive tape. On the other hand, although it is a branched structure or a multi-branched structure, a structure having a styrene block at the molecular end can obtain a pseudo cross-linked structure, which can impart excellent cohesive force, and therefore can impart high holding power. Therefore, the styrene resin is preferably used in combination according to the characteristics required.
[0201] As the above-mentioned styrene resin, relative to the total mass of the styrene resin, it is preferred to use a styrene resin having a structural unit shown in the following chemical formula (B) in a range of 10 to 80% by mass, more preferably a styrene resin having a structural unit shown in the following chemical formula (B) in a range of 12 to 60% by mass, further preferably a styrene resin having a structural unit shown in the following chemical formula (B) in a range of 15 to 40% by mass, and particularly preferably a styrene resin having a structural unit shown in the following chemical formula (B) in a range of 17 to 35% by mass. Thus, excellent adhesion and heat resistance can be obtained. It should be noted that the * in the following chemical formula (B) represents the bond position with other atoms.
[0202] [Chemical formula 10]
[0203]
[0204] The method for producing the styrene-based resin is not particularly limited, and a method may be appropriately selected from conventionally known production methods. A block copolymer may be obtained by an anionic living polymerization method, and a coupling agent may be added as needed to react the resultant block copolymer to obtain a styrene-based resin.
[0205] In the adhesive layer, the rubber-based adhesive resin preferably accounts for 0 to 50% by mass, and more preferably accounts for 0 to 30% by mass, relative to the entire adhesive resin. When the content of the rubber-based adhesive resin in the adhesive resin used in the adhesive layer is within the above range, it is easy to achieve both adhesion, disassembly properties, and high load holding power.
[0206] <Tackifying resin>
[0207] The adhesive layer of the adhesive tape of the present embodiment preferably further contains a tackifier resin. The tackifier resin is preferably used to improve the adhesion to the adherend and the surface adhesive strength.
[0208] The softening point of the tackifier resin is preferably 95° C. or higher, more preferably 95° C. to 180° C., and even more preferably 95° C. to 140° C. When the softening point is within this range, an adhesive layer having high adhesive performance can be formed.
[0209] As the above-mentioned tackifying resin, a tackifying resin having a softening point (softening temperature) of 95°C or more can be preferably used. By using an adhesive layer containing a tackifying resin having a softening point above the above lower limit, an adhesive tape with better adhesion can be achieved. Among the above-mentioned exemplified tackifying resins, terpene-based tackifying resins (such as terpene-modified phenolic resins), rosin-based tackifying resins (such as esters of polymerized rosin), etc. having the above-mentioned softening point can be preferably used. There is no particular restriction on the upper limit of the softening point of the tackifying resin, for example, it can be set to about 200°C or less. It should be noted that the softening point of the tackifying resin mentioned here is defined as the value measured by the softening point test method (ring and ball method) specified in either JIS K 5902 and JIS K 2207.
[0210] As the specific example of the above-mentioned tackifying resin, rosin-based tackifying resin (polymerized rosin-based tackifying resin, polymerized rosin ester-based tackifying resin, rosin phenolic tackifying resin, stabilized rosin ester-based tackifying resin, disproportionated rosin ester-based tackifying resin, hydrogenated rosin ester-based tackifying resin, etc.), terpene-based tackifying resin (terpene phenolic tackifying resin, etc.), hydrocarbon-based tackifying resin (petroleum resin-based tackifying resin, etc.), (methyl) acrylate-based tackifying resin, etc., can be enumerated. One kind can be used alone, or two or more kinds can be used in combination. Among them, as tackifying resin, preferably polymerized rosin ester-based tackifying resin, rosin phenolic tackifying resin, disproportionated rosin ester-based tackifying resin, hydrogenated rosin ester-based tackifying resin, terpene phenolic tackifying resin, (methyl) acrylate-based tackifying resin.
[0211] Specific examples of the above-mentioned rosin-based tackifying resins include unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin; modified rosins obtained by modifying these unmodified rosins by hydrogenation, disproportionation, polymerization, etc. (hydrogenated rosin, disproportionated rosin, polymerized rosin, other chemically modified rosins, etc., the same below); and various other rosin derivatives. Examples of the rosin derivatives include rosin esters such as those obtained by esterifying unmodified rosin with alcohols (i.e., esters of rosin) and those obtained by esterifying modified rosin with alcohols (i.e., esters of modified rosin); unsaturated fatty acid-modified rosins obtained by modifying unmodified rosin or modified rosin with unsaturated fatty acids; unsaturated fatty acid-modified rosin esters obtained by modifying rosin esters with unsaturated fatty acids; rosin alcohols obtained by reducing the carboxyl groups in unmodified rosin, modified rosin, unsaturated fatty acid-modified rosin or unsaturated fatty acid-modified rosin esters; metal salts of rosins (particularly rosin esters) such as unmodified rosin, modified rosin, and various rosin derivatives; rosin phenolic resins obtained by adding phenol to rosins (unmodified rosin, modified rosin, various rosin derivatives, etc.) using an acid catalyst and thermally polymerizing the rosins; and the like. From the viewpoint of improving adhesive properties such as adhesive strength, it is more preferred to use two or more rosin-based tackifier resins that are different in type and properties (eg, softening point) in combination.
[0212] Examples of the above-mentioned terpene-based tackifying resins include terpene resins such as α-pinene polymers, β-pinene polymers, and dipentene polymers; modified terpene resins obtained by modifying these terpene resins (phenol modification, aromatic modification, hydrogenation modification, hydrocarbon modification, etc.). Examples of the above-mentioned modified terpene resins include terpene-modified phenolic resins, styrene-modified terpene resins, aromatic-modified terpene resins, and hydrogenated terpene resins. From the viewpoint of improving adhesive properties such as adhesion, it is preferred to use one or more of the above-mentioned terpene-based tackifying resins (such as terpene-modified phenolic resins) in combination with different types and properties (such as softening points).
[0213] Examples of the above-mentioned hydrocarbon-based tackifying resins include various hydrocarbon-based resins such as aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aliphatic / aromatic petroleum resins (styrene-olefin copolymers, etc.), aliphatic / alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone resins, and coumarone indene resins.
[0214] The amount of the tackifier resin used is not particularly limited and can be appropriately selected according to the purpose. It is preferably in the range of 10 to 150 parts by mass, more preferably in the range of 10 to 65 parts by mass, relative to 100 parts by mass of the triblock copolymer. When used in the range of 10 to 55 parts by mass, it is easy to ensure adhesion to the adherend, and therefore it is more preferred.
[0215] <Cross-linking agent>
[0216] The adhesive layer preferably contains a crosslinking agent. When the adhesive layer contains a crosslinking agent, the cohesive force of the adhesive layer can be further increased.
[0217] As the above-mentioned cross-linking agent, there is no particular limitation and it can be appropriately selected according to the purpose, for example, isocyanate cross-linking agents, epoxy cross-linking agents, metal chelate cross-linking agents, aziridine cross-linking agents, etc. can be mentioned. Among them, isocyanate cross-linking agents are preferred. They can be used alone or in combination of two or more.
[0218] As the above-mentioned isocyanate crosslinking agent, for example, toluene diisocyanate, triphenylmethane isocyanate, naphthalene-1,5-diisocyanate, hexamethylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, trimethylolpropane-modified toluene diisocyanate, etc. can be mentioned. These can be used alone or in combination of two or more. Among them, toluene diisocyanate, which is a trifunctional polyisocyanate compound, and its trimethylolpropane adducts and triphenylmethane isocyanate are particularly preferred.
[0219] As an index of the degree of crosslinking, the value of the gel fraction of the insoluble components after the adhesive layer is immersed in toluene for 24 hours is used. The gel fraction of the adhesive layer is not particularly limited and can be appropriately selected according to the purpose, preferably 0 to 50% by mass, more preferably 0 to 20% by mass, and further preferably 0 to 10% by mass from the perspective of obtaining an adhesive layer with good cohesiveness and adhesion.
[0220] It should be noted that the gel fraction refers to a value measured by the following method. The adhesive composition is applied to a release sheet in such a manner that the thickness after drying becomes 50 μm, dried at 100°C for 3 minutes, aged at 40°C for 2 days, and the resultant is cut into 50 mm squares to serve as a sample. Next, the mass (G1) of the sample before toluene immersion is measured in advance, and the toluene insoluble components of the sample after immersion in a toluene solution at 23°C for 24 hours are separated by filtering with a 300-mesh metal wire mesh, and the mass (G2) of the residue after drying at 110°C for 1 hour is measured, and the gel fraction is calculated according to the following formula (4). It should be noted that the mass (G3) of the filler particles in the sample is calculated from the mass (G1) of the sample and the composition of the adhesive composition.
[0221] Gel fraction (mass %) = (G2-G3) / (G1-G3)×100 Formula (4)
[0222] <Other ingredients>
[0223] As other components in the above-mentioned adhesive layer, there is no particular restriction, and they can be appropriately selected within the range that does not damage the characteristics of the adhesive tape, and for example, polymer components other than the adhesive resin, anti-aging agents, ultraviolet absorbers, fillers, polymerization inhibitors, surface regulators, antistatic agents, defoamers, viscosity modifiers, light stabilizers, weather stabilizers, heat stabilizers, antioxidants, leveling agents, organic pigments, inorganic pigments, pigment dispersants, plasticizers, softeners, flame retardants, metal deactivators and other additives can be cited. They can be used alone or in combination of two or more.
[0224] The content of other components in the adhesive layer can be appropriately selected within a range that does not impair the properties of the adhesive tape.
[0225] <Physical properties of adhesive layer>
[0226] The stress at 25% elongation of the above-mentioned adhesive layer is preferably 0.04 to 0.4 MPa, and more preferably 0.05 to 0.1 MPa. When the stress at 25% elongation of the adhesive layer is within the preferred range, a bonding strength suitable for the adhesive tape can be obtained, and it can be relatively easily peeled off even when the adhesive tape is peeled off by elongation. In addition, when the stress at 25% elongation of the adhesive layer is above 0.04 MPa, the adhesive tape is not easy to peel off even when a load in the shear direction of the raw adhesive tape is generated while fixing hard adherends to each other. When it is below 0.4 MPa, when peeling the adhesive tape, the force required to stretch the adhesive tape will not become too large.
[0227] The stress at 25% elongation of the above-mentioned adhesive layer refers to the stress value measured when the adhesive layer is punched into a dumbbell shape with a marking line length of 20 mm and a width of 10 mm, and stretched in the longitudinal direction at a stretching speed of 300 mm / min under the conditions of a measuring atmosphere of 23°C and 50% RH using a Tensilon tensile testing machine (model: RTF1210, manufactured by A&D Co., Ltd.) and elongated by 25%.
[0228] The fracture strength of the adhesive layer is preferably 0.5 to 2.1 MPa, more preferably 1.0 to 2.1 MPa. When the fracture strength of the adhesive layer is within the above preferred range, even when the adhesive tape is stretched and peeled off, the adhesive tape can be prevented from rupturing, and the load used to extend the adhesive tape will not be excessively excessive, so the re-peeling operation using peeling becomes easy. In addition, when the fracture strength of the adhesive layer is more than 0.5 MPa, when the adhesive tape is stretched and peeled off, it is not easy to produce residual glue caused by the cohesive failure of the adhesive layer, and when it is less than 2.1 MPa, sufficient adhesion can be obtained.
[0229] The breaking strength of the adhesive layer is the stress value measured when the adhesive layer is punched into a dumbbell shape with a marking length of 20 mm and a width of 10 mm, and stretched in the longitudinal direction at a stretching speed of 300 mm / min using a Tensilon tensile testing machine (model: RTF1210, manufactured by A&D Co., Ltd.) under the conditions of a measuring atmosphere of 23°C and 50% RH.
[0230] The elongation at break of the adhesive layer is preferably 450 to 1300%, more preferably 500 to 1200%, and further preferably 600 to 1100%. By setting the elongation at break of the adhesive layer within the above preferred range, both appropriate adhesiveness and removability (ease of peeling) can be achieved.
[0231] The elongation at break of the adhesive layer is the tensile elongation measured when the adhesive layer is punched into a dumbbell shape with a marking length of 20 mm and a width of 10 mm, and stretched in the longitudinal direction at a stretching speed of 300 mm / min using a Tensilon tensile tester (model: RTF1210, manufactured by A&D Co., Ltd.) under the conditions of a measuring atmosphere of 23°C and 50% RH.
[0232] The average thickness of the adhesive layer is preferably 5 μm to 150 μm, more preferably 20 μm to 120 μm, further preferably 40 μm to 110 μm, and particularly preferably 50 μm to 100 μm. It should be noted that, in the case where the adhesive tape has adhesive layers on both sides, the "average thickness of the adhesive layer" refers to the average thickness of the adhesive layer on one side of the adhesive tape. In the case where the adhesive tape has adhesive layers on both sides, the average thickness of the adhesive layer on one side may be the same as or different from the average thickness of the adhesive layer on the other side, and preferably the same average thickness.
[0233] It should be noted that the average thickness of the above-mentioned adhesive layer can be measured by the following method. That is, after immersing the adhesive tape in liquid nitrogen for 1 minute, use tweezers to bend and cut the adhesive tape in liquid nitrogen with the width direction of the adhesive tape as a fold, and make a slice for observing the cut surface in the thickness direction of the adhesive tape. After the above-mentioned slice is restored to room temperature in a dryer, the above-mentioned slice is fixed to the sample table in a manner that the electron beam is incident vertically with respect to the above-mentioned cut surface, and the above-mentioned cut surface is observed using an electron microscope. Based on the scale of the electron microscope, the thickness of the adhesive layer in the above-mentioned adhesive tape at 10 locations is measured, and the arithmetic mean thereof is taken as the average thickness of the adhesive layer. It should be noted that the thickness of the adhesive layer is the length measured from the surface on one side to the surface on the other side along the stacking direction.
[0234] "Substrate layer"
[0235] As described above, the pressure-sensitive adhesive tape according to the present embodiment is a pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer, and preferably further has a base layer that contacts one surface of the pressure-sensitive adhesive layer.
[0236] The pressure-sensitive adhesive tape of the present embodiment may include two pressure-sensitive adhesive layers in contact with the base layer on both sides of the base layer. In this case, the two pressure-sensitive adhesive layers may be the same or different.
[0237] The substrate layer can be appropriately selected from known materials that can be used for pressure-sensitive adhesive tapes, and preferably contains the following substrate layer materials, and may further contain other components as necessary.
[0238] Furthermore, the base layer may have a single-layer structure, or may have a two-layer, three-layer, or more-layer structure.
[0239] <Characteristics of base material layer>
[0240] The fracture stress of the substrate layer is preferably 1 to 100 MPa, more preferably 10 to 90 MPa, further preferably 15 to 90 MPa, further preferably 30 to 90 MPa, and particularly preferably 50 to 90 MPa. By making the fracture stress of the substrate layer 1 MPa or more, when the adhesive tape is peeled off from the adherend, even if the operator stretches it, the adhesive tape can be peeled off from the adherend without breaking. In addition, by making the fracture stress of the substrate layer 100 MPa or less, it is possible to avoid the stress when the operator stretches the adhesive tape becoming too large.
[0241] The breaking stress of the substrate layer is the stress value measured when the substrate layer is punched into a dumbbell shape with a marking length of 20 mm and a width of 5 mm, and stretched in the longitudinal direction at a stretching speed of 500 mm / min using a Tensilon tensile testing machine (model: RTF-1210, manufactured by A&D Co., Ltd.) under the conditions of a measuring atmosphere of 23°C and 50% RH.
[0242] The breaking stress can be adjusted by appropriately selecting the material and applying stretching or the like during the production process of the base material layer.
[0243] As the above-mentioned base material layer, the elongation at break is preferably 400 to 3000%, more preferably 500 to 2500%, further preferably 530 to 1700%, further preferably 560 to 1300%, and particularly preferably 600 to 1200%. By making the elongation at break of the base material layer 400% or more, the stress when peeling the adhesive tape will not become too large even if the adhesive tape is firmly adhered to the adherend. In addition, by making the elongation at break of the base material layer 3000% or less, the stretching distance will not become too long when peeling the adhesive tape, and the operation can be performed in a small space.
[0244] The elongation at break of the above-mentioned substrate layer refers to the tensile elongation measured when the substrate layer is punched into a dumbbell shape with a marking line length of 20 mm and a width of 5 mm, and stretched in the longitudinal direction at a stretching speed of 500 mm / min using a Tensilon tensile testing machine (model: RTF-1210, manufactured by A&D Co., Ltd.) under the conditions of a measuring atmosphere of 23°C and 50% RH.
[0245] The elongation at break can be adjusted by selecting an appropriate material and applying stretching or the like in the production process of the base material layer.
[0246] The 50% modulus of the substrate layer is preferably 0.1 to 5 MPa, more preferably 0.5 to 4.5 MPa, and further preferably 1 to 4 MPa. By making the 50% modulus of the substrate layer 0.1 MPa or more, when a load is applied to the adhesive tape or adherend, it is possible to suppress the undesirable conditions associated with shape deformation such as deviation. In addition, by making the 50% modulus of the substrate layer 5 MPa or less, the operator can stretch the adhesive tape with a relatively light force in the initial stage of peeling the adhesive tape from the adherend.
[0247] The 50% modulus of the above-mentioned substrate layer refers to the stress value measured when the substrate layer is punched into a dumbbell shape with a marking line length of 20 mm and a width of 5 mm, and stretched in the longitudinal direction at a stretching speed of 500 mm / min using a Tensilon tensile testing machine (model: RTF-1210, manufactured by A&D Co., Ltd.) under the conditions of a measuring atmosphere of 23°C and 50% RH, and the elongation is 50%.
[0248] The 50% modulus can be adjusted by selecting an appropriate material and applying stretching or the like during the production process of the base material layer.
[0249] The rubber hardness of the substrate layer is preferably 20 to 90A, more preferably 30 to 85A, and further preferably 40 to 80A. By making the rubber hardness of the substrate layer 20A or more, the adhesive tape can be prevented from being broken when the adhesive tape is stretched and peeled off. In addition, by making the rubber hardness of the substrate layer 90A or less, the substrate layer becomes soft, for example, when the adherend to which the adhesive tape is attached is dropped, the adhesive tape can easily absorb the impact, and can protect the adherend from the impact (the impact resistance of the adhesive tape can be improved).
[0250] The rubber hardness of the substrate layer is Shore A hardness, which is a value measured in accordance with JIS K 6253 using a durometer (spring type rubber durometer) (model: GS-719G, manufactured by TECLOCK CO., LTD.).
[0251] The rubber hardness can be adjusted by, for example, changing the molecular weight of the resin, or, when a styrene monomer unit is contained, changing the content of the monomer unit, or selecting an appropriate material.
[0252] The average thickness of the substrate layer is preferably 10 to 500 μm, more preferably 30 to 250 μm, and even more preferably 50 to 200 μm. By setting the average thickness of the substrate layer to be 10 μm or more, the strength of the adhesive tape can be increased. In addition, by setting the average thickness of the substrate layer to be 500 μm or less, it is possible to avoid the adhesive tape being too thick and difficult to stretch.
[0253] It should be noted that the above-mentioned "average thickness of the substrate layer" refers to the substrate layer being cut into 5 places in the width direction at intervals of 100 mm in the length direction, and the thickness of 5 places in each cut surface being measured at intervals of 100 mm in the width direction using a TH-104 paper / film thickness measuring machine (manufactured by TESTER SANGYO Co., Ltd.), and the average value of these measured values.
[0254] As the ratio of the thickness of the above-mentioned adhesive layer to the above-mentioned substrate layer, there is no particular restriction, and it can be appropriately selected according to the purpose. The ratio of the average thickness of the adhesive layer relative to the average thickness of the substrate layer, represented by [average thickness of the adhesive layer / average thickness of the substrate layer], is preferably 1 / 5 to 5 / 1, more preferably 1 / 3 to 3 / 1, and further preferably 1 / 2 to 2 / 1. When the ratio of the average thickness of the adhesive layer relative to the average thickness of the substrate layer is within a preferred range, the excellent adhesion and re-peelability (peeling ease) of the adhesive tape can be obtained. In addition, when the above-mentioned ratio is less than 5 / 1, it is possible to prevent only the adhesive layer from remaining on the adherend in the re-peeling process of the adhesive tape. In addition, when the above-mentioned ratio is more than 1 / 5, even when the surface of the adherend is a concave-convex shape, the adhesive layer can follow and can maintain sufficient bonding strength.
[0255] <Material of base material layer>
[0256] As the material of the above-mentioned substrate layer, for example, styrene resins such as polystyrene, styrene-isoprene copolymer, styrene-isoprene-styrene copolymer, styrene-isoprene-butadiene-styrene copolymer, styrene-butadiene-styrene copolymer, styrene-ethylene-butylene copolymer, and styrene-ethylene-propylene copolymer; polyurethane resins such as ester polyurethane and ether polyurethane; polyolefin resins such as polyethylene and polypropylene; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polycarbonate; polymethylpentene; polysulfone; polyetheretherketone; polyethersulfone; polyetherimide; polyimide; fluororesin; polyamide; acrylic resin, etc. These can be used alone or in combination of two or more, preferably in combination of two or more.
[0257] Among them, styrene resins and polyurethane resins are preferred because they can easily provide suitable breaking strength and breaking elongation. Styrene resins are more preferred, and it is particularly preferred to use a styrene-isoprene copolymer and a styrene-isoprene-styrene copolymer in combination.
[0258] --Styrene resin--
[0259] The above-mentioned styrene resin is a resin showing thermoplasticity, so it is excellent in moldability such as extrusion molding and injection molding, and it is easy to mold the base layer. In addition, the styrene resin is easy to obtain an elongation at break that is particularly excellent even in the resin group generally called thermoplastic resins, and can be suitably used as the base layer of the adhesive tape.
[0260] Therefore, in the material of the substrate layer, the proportion of the styrene resin relative to the total resin components is preferably 50 to 100 mass %, more preferably 60 to 100 mass %, further preferably 65 to 100 mass %, and particularly preferably 70 to 100 mass %. By making the proportion of the styrene resin within the above-mentioned preferred range, a substrate layer having excellent elongation at break and breaking strength can be obtained.
[0261] The above-mentioned styrene resin can use a single structure styrene resin of a linear structure, a branched structure or a multi-branched structure, or can be mixed with styrene resins of different structures. The styrene resin rich in linear structure can give excellent elongation at break to the substrate layer. On the other hand, although it is a branched structure or a multi-branched structure, a structure with a styrene block at the molecular end can obtain a pseudo cross-linked structure, which can give excellent cohesive force. Therefore, the styrene resin is preferably mixed and used according to the mechanical properties required.
[0262] As the above-mentioned styrene resin, it is preferred to use a styrene resin having a structural unit shown in the following chemical formula (A) in a range of 13 to 60% by mass relative to the total mass of the styrene resin, more preferably a styrene resin having a structural unit shown in the following chemical formula (A) in a range of 15 to 50% by mass, further preferably a styrene resin having a structural unit shown in the following chemical formula (A) in a range of 15 to 45% by mass, and particularly preferably a styrene resin having a structural unit shown in the following chemical formula (A) in a range of 15 to 35% by mass. By making the ratio of the structural unit shown in the following chemical formula (A) relative to the total mass of the styrene resin within the above-mentioned preferred range, it is easy to obtain a suitable range of elongation at break and breaking strength. It should be noted that the * in the following chemical formula (A) represents the bond position with other atoms.
[0263] [Chemical formula 11]
[0264]
[0265] When a styrene-based resin is used in combination with a styrene-isoprene copolymer and a styrene-isoprene-styrene copolymer, the content of the styrene-isoprene copolymer is preferably 0 to 80% by mass, more preferably 0 to 70% by mass, further preferably 0 to 50% by mass, and particularly preferably 0 to 30% by mass, relative to the total mass of the styrene-isoprene copolymer and the styrene-isoprene-styrene copolymer. When the content of the styrene-isoprene copolymer is within the above-mentioned preferred range, thermal durability can be achieved while maintaining excellent elongation at break and breaking strength.
[0266] In addition, as the styrene-isoprene copolymer, it is preferred to use a styrene-isoprene copolymer having a weight average molecular weight of 10,000 to 800,000 as measured by gel permeation chromatography (GPC) in terms of standard polystyrene, more preferably 30,000 to 500,000, and further preferably 50,000 to 300,000. The weight average molecular weight of the styrene-isoprene copolymer is within the above preferred range, because the heat flowability and compatibility during solvent dilution can be ensured, so the workability in the manufacturing process is good, and a substrate layer having heat durability can be obtained, so it is preferred.
[0267] Here, the weight average molecular weight of the styrene-isoprene copolymer measured by the GPC method is a standard polystyrene conversion value measured using a GPC apparatus (SC-8020, manufactured by Tosoh Corporation), and the measurement conditions are as follows.
[0268] -Measurement conditions-
[0269] Sample concentration: 0.5 mass% (tetrahydrofuran solution)
[0270] Sample injection volume: 100μL
[0271] ·Eluent: Tetrahydrofuran
[0272] Flow rate: 1.0mL / min
[0273] ·Measurement temperature: 40℃
[0274] Main column: TSKgel (registered trademark) GMHHR-H (20) 2 pieces
[0275] Guard column: TSKgel HXL-H
[0276] Detector: Differential refractometer
[0277] · Standard polystyrene molecular weight: 10,000 to 20,000,000 (manufactured by Tosoh Corporation)
[0278] There are no particular restrictions on the production method of styrene-isoprene copolymers, styrene-isoprene-styrene copolymers, and mixtures of styrene-isoprene copolymers and styrene-isoprene-styrene copolymers, and they can be appropriately selected from conventionally known production methods. Block copolymers can be obtained by anionic living polymerization, and a coupling agent can be added as needed to react them.
[0279] Specifically, the method for producing the styrene-isoprene copolymer is not particularly limited and may be appropriately selected from conventionally known production methods. Examples thereof include a method of sequentially polymerizing a styrene block and an isoprene block by an anionic living polymerization method.
[0280] There are no particular restrictions on the method for producing the styrene-isoprene-styrene copolymer, and it can be appropriately selected from conventionally known production methods, for example, a method of sequentially polymerizing a styrene block and an isoprene block by an anionic living polymerization method, a method of producing a block copolymer having an active active terminal and then reacting with a coupling agent to obtain a block copolymer, etc.
[0281] The method for producing the mixture of the styrene-isoprene copolymer and the styrene-isoprene-styrene copolymer is not particularly limited and can be appropriately selected from conventionally known production methods. Examples thereof include a method of mixing the styrene-isoprene copolymer produced by the above method and the styrene-isoprene-styrene copolymer.
[0282] In addition, as a method for producing a mixture of a styrene-isoprene copolymer and a styrene-isoprene-styrene copolymer, they can be simultaneously produced as a mixture in one polymerization step.
[0283] As a more specific embodiment, by anionic living polymerization, first, in a polymerization solvent, styrene monomers are polymerized using anionic polymerization initiators to form polystyrene blocks having active active ends. Second, isoprene is polymerized from the active active ends of the polystyrene blocks to obtain styrene-isoprene diblock copolymers having active active ends. Third, a portion of the styrene-isoprene diblock copolymer having active active ends is reacted with a coupling agent to form a coupled styrene-isoprene-styrene block copolymer. Fourth, for the remaining portion of the styrene-isoprene diblock copolymer having active active ends, a polymerization terminator is used to inactivate the active active ends to form a styrene-isoprene diblock copolymer.
[0284] --Polyurethane resin--
[0285] The polyurethane resin is not particularly limited and can be appropriately selected according to the purpose. A polyurethane resin having a softening point of 40° C. or higher is preferred, and a polyurethane resin having a softening point of 50° C. or higher is more preferred. The upper limit of the softening point is preferably 100° C. or lower. The softening point refers to a value measured according to JIS K 2207 (dry bulb method) (hereinafter, the same applies to the softening point).
[0286] As the polyurethane resin, a reaction product of a polyol (b1-1) and a polyisocyanate (b1-2) can be preferably used.
[0287] As polyol (b1-1), there is no particular limitation and it can be appropriately selected according to the purpose, for example, polyester polyol, polyether polyol, polycarbonate polyol, acrylic polyol etc. can be cited. They can be used alone or in combination of two or more. Among them, as polyol (b1-1), polyester polyol and polyether polyol can obtain mechanical properties suitable as substrate layer, so they are preferred. In the substrate layer, polyester polyol is preferably used when heat resistance is required, and polyether polyol is preferably used when water resistance and biodegradability resistance are required.
[0288] Examples of the polyester polyol include polyesters obtained by esterification reaction of a low molecular weight polyol and a polycarboxylic acid, polyesters obtained by ring-opening polymerization of a cyclic ester compound such as ε-caprolactone, and copolymerized polyesters thereof.
[0289] Examples of low molecular weight polyols that can be used in the production of the polyester polyol include aliphatic alkylene glycols such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, neopentyl glycol, and 1,3-butanediol, and cyclohexanedimethanol having a weight average molecular weight of about 50 to 300.
[0290] Examples of the polycarboxylic acid include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, and dodecanedicarboxylic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and naphthalenedicarboxylic acid; and anhydrides or esters thereof.
[0291] Examples of the polyether polyol include polyether polyols obtained by addition-polymerizing alkylene oxides using one or more compounds having two or more active hydrogen atoms as an initiator.
[0292] As the polycarbonate polyol, for example, a polycarbonate polyol obtained by reacting a carbonate and / or phosgene with a low molecular weight polyol described below can be used.
[0293] Examples of the carbonate ester include methyl carbonate, dimethyl carbonate, ethyl carbonate, diethyl carbonate, cyclic carbonate, and diphenyl carbonate.
[0294] Examples of the low molecular weight polyol that can be used to produce the polycarbonate polyol and can react with carbonate and / or phosgene include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, tripropylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2,3-butylene glycol, 1,5-pentanediol, 1,5-hexanediol, 1,6-hexanediol, 2,5-hexanediol, and 1,7-heptanediol. , 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol, 1,4-cyclohexanedimethanol, hydroquinone, resorcinol, bisphenol A, bisphenol F, 4,4'-biphenol, etc.
[0295] There is no particular limitation on the polyisocyanate (b1-2), and it can be appropriately selected according to the purpose, and examples thereof include alicyclic polyisocyanates, aliphatic polyisocyanates, aromatic polyisocyanates, etc., preferably alicyclic polyisocyanates, etc. These can be used alone or in combination of two or more.
[0296] Examples of the alicyclic polyisocyanate include isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, 4,4'-dicyclohexylmethane diisocyanate, 2,4-methylcyclohexane diisocyanate, 2,6-methylcyclohexane diisocyanate, cyclohexyl diisocyanate, methylcyclohexyl diisocyanate, bis(2-isocyanatoethyl)-4-cyclohexylene-1,2-dicarboxylate, 2,5-norbornane diisocyanate, 2,6-norbornane diisocyanate, dimer acid diisocyanate, and bicycloheptane triisocyanate. These may be used alone or in combination of two or more.
[0297] There are no particular restrictions on the method for producing the polyurethane resin (b1) by reacting a polyol (b1-1) with a polyisocyanate (b1-2), and it can be appropriately selected from conventionally known production methods. For example, there can be mentioned a method in which the polyol (b1-1) introduced into a reaction container is heated under normal pressure or reduced pressure to remove moisture, and then the polyisocyanate (b1-2) is supplied all at once or in batches to react.
[0298] The reaction of the polyol (b1-1) and the polyisocyanate (b1-2) is preferably carried out under conditions where the equivalent ratio of the isocyanate group (NCO) possessed by the polyisocyanate (b1-2) to the hydroxyl group (OH) possessed by the polyol (b1-1) (NCO / OH equivalent ratio) is in the range of 1.0 to 20.0, more preferably in the range of 1.1 to 13.0, further preferably in the range of 1.2 to 5.0, and particularly preferably in the range of 1.5 to 3.0.
[0299] The reaction conditions of the polyol (b1-1) and the polyisocyanate (b1-2) are not particularly limited and can be appropriately selected in consideration of various conditions such as safety, quality, and cost. The reaction temperature is preferably 70° C. to 120° C., and the reaction time is preferably 30 minutes to 5 hours.
[0300] When the polyol (b1-1) and the polyisocyanate (b1-2) are reacted, for example, a tertiary amine catalyst, an organic metal catalyst or the like may be used as a catalyst, if necessary.
[0301] In addition, the above reaction may be carried out in the absence of a solvent or in the presence of an organic solvent.
[0302] The organic solvent is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include ester solvents such as methyl acetate, ethyl acetate, propyl acetate, and butyl acetate; ketone solvents such as acetone, methyl ethyl ketone, methyl butyl ketone, and cyclohexanone; ether ester solvents such as methyl cellosolve acetate and butyl cellosolve acetate; aromatic hydrocarbon solvents such as toluene and xylene; amide solvents such as dimethylformamide and dimethylacetamide, etc. These solvents can be used alone or in combination of two or more.
[0303] The organic solvent can be removed by an appropriate method such as heating under reduced pressure, drying under normal pressure, etc. during the production process of the polyurethane resin or after the production of the polyurethane resin.
[0304] --Other ingredients--
[0305] As other components in the above-mentioned substrate layer, there is no particular limitation, and they can be appropriately selected within the range that does not damage the characteristics of the adhesive tape, for example, tackifying resins; polymer components other than the materials of the substrate layer; crosslinking agents, anti-aging agents, ultraviolet absorbers, fillers, inhibitors, surface regulators, antistatic agents, defoamers, viscosity modifiers, light stabilizers, weather stabilizers, heat stabilizers, antioxidants, leveling agents, organic pigments, inorganic pigments, pigment dispersants, silica beads, organic beads and other additives; inorganic fillers such as silicon oxide, aluminum oxide, titanium oxide, zirconium oxide, antimony pentoxide, etc. They can be used alone or in combination of two or more.
[0306] The content of other components in the base material layer can be appropriately selected within a range that does not impair the properties of the pressure-sensitive adhesive tape.
[0307] The tackifier resin can be used for the purpose of improving the adhesion between the adhesive layer and the base layer of the adhesive tape or improving the heat resistance.
[0308] The tackifying resin is not particularly limited and can be appropriately selected according to the purpose. A tackifying resin having a softening point of 80° C. or higher is preferred, a tackifying resin having a softening point of 90° C. or higher is more preferred, a tackifying resin having a softening point of 100° C. or higher is further preferred, and a tackifying resin having a softening point of 110° C. or higher is particularly preferred.
[0309] As the tackifier resin used for the base material layer, for example, the tackifier resins described in the above-mentioned item of "rubber-based binder resin" can be used, and the preferred aspects and the like are also the same.
[0310] As the above-mentioned antioxidant, there is no particular restriction, and it can be appropriately selected according to the purpose from known antioxidants, for example, phenolic antioxidants, phosphorus antioxidants (sometimes also referred to as "processing stabilizers"), amine antioxidants, imidazole antioxidants, etc. can be cited. They can be used alone or in combination of two or more. Among them, preferably phenolic antioxidants and phosphorus antioxidants, when used in combination, can effectively improve the heat resistance stability of the substrate layer material, as a result, it is possible to obtain an adhesive tape that maintains good initial adhesion and possesses further excellent thermal durability, so it is preferred. It should be noted that phosphorus antioxidants sometimes change color (yellowing) slightly over time under high temperature environment, and therefore, its usage amount is preferably appropriately set in consideration of the balance between initial adhesion, thermal durability and preventing discoloration.
[0311] As the above-mentioned phenolic antioxidant, a phenolic compound having a sterically hindered group can be generally used, and monophenol type, bisphenol type, and polyphenol type are representative. As specific examples, 2,6-di-tert-butyl-4-methylphenol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-thiobis(6-tert-butyl-3-methylphenol), 4,4'-butylenebis(3-methyl-6-tert-butylphenol), tetrakis-[methylene-3-(3'5'-di-tert-butyl-4-hydroxyphenyl]methane, n-octadecyl-3-(4'-hydroxy-3'5'-di-tert-butylphenyl) propionate, etc. can be cited. They can be used alone or in combination of two or more.
[0312] The amount of the phenolic antioxidant used is not particularly limited and can be appropriately selected according to the purpose. It is preferably used in the range of 0.1 to 5 parts by mass relative to 100 parts by mass of the material for the substrate layer. When used in the range of 0.5 to 3 parts by mass, the heat resistance stability of the material for the substrate layer can be effectively improved. As a result, an adhesive tape that maintains good initial adhesion and has further excellent thermal durability can be obtained.
[0313] "Other Layers"
[0314] The pressure-sensitive adhesive tape of the present embodiment may be provided with one or more other layers as appropriate according to the purpose. Examples of such other layers include a primer layer, an antistatic layer, a non-combustible layer, a decorative layer, a conductive layer, a thermal conductive layer, and a release layer.
[0315] "Adhesive tape shape, characteristics, etc."
[0316] As long as the adhesive tape of this embodiment has an adhesive layer, its shape and size are not particularly limited. For example, it includes an adhesive tape with a shape and size suitable for attachment to a specified adherend (for example, an adhesive tape in a state after punching), and a sheet-like long strip of adhesive tape (for example, an adhesive tape before being processed into a specific shape).
[0317] In addition, in the pressure-sensitive adhesive tape of the present embodiment, for example, in order to attach to or peel off an adherend, a non-adhesive gripping region may be arbitrarily provided.
[0318] The average thickness of the pressure-sensitive adhesive tape is not particularly limited and may be appropriately selected depending on the average thickness of the pressure-sensitive adhesive layer, but is preferably 15 to 800 μm, more preferably 30 to 540 μm, further preferably 60 to 320 μm, and particularly preferably 70 to 250 μm.
[0319] It should be noted that the above-mentioned "average thickness of the adhesive tape" refers to the average value of the thickness of 25 thicknesses in total, obtained by cutting the adhesive tape at 5 locations in the width direction at intervals of 100 mm in the length direction, and measuring the thickness at 5 locations in the width direction at intervals of 100 mm in each cut surface using a TH104 paper / film thickness measuring machine (manufactured by TESTER SANGYO Co., Ltd.).
[0320] The adhesive tape of this embodiment preferably has a peeling adhesive force (180° peeling adhesive force) of 5N / 20mm or more, more preferably in the range of 15N / 20mm to 50N / 20mm, and further preferably in the range of 15N / 20mm to 45N / 20mm. When the peeling adhesive force is within the above-mentioned preferred range, it does not cause peeling or deviation from the adherend and has a moderate adhesive force, and when the adhesive tape is stretched in the horizontal direction to the vertical direction relative to the attachment surface of the adherend and then peeled off, it can be easily peeled off.
[0321] The peel adhesion of the pressure-sensitive adhesive tape is a value measured in accordance with JIS Z 0237.
[0322] The cleavage adhesive strength of the pressure-sensitive adhesive tape of the present embodiment is preferably 10 to 200 N / cm 2 , more preferably 30 to 150 N / cm 2 The range is more preferably 50 to 100 N / cm 2 When the cleavage adhesive strength is within the above preferred range, it is easy to achieve both removability and adhesiveness.
[0323] The cleavage adhesive strength of the pressure-sensitive adhesive tape is a value measured by the method described in Examples below.
[0324] The hardness (A-type hardness (Shore A hardness)) of the adhesive tape of the present embodiment is preferably 10 to 90, more preferably 20 to 85, and further preferably 64 to 85. When the Shore A hardness of the adhesive tape is within the above-mentioned preferred range, the re-peeling operation by peeling off the adhesive tape becomes easy. In addition, when the Shore A hardness is 10 or more, the adhesive tape is not easy to break when the adhesive tape is stretched and peeled off, and when it is 90 or less, when it is desired to stretch the adhesive tape and peel it off again, the stress used for stretching will not become too high, and re-peeling is easy.
[0325] The rubber hardness of the adhesive tape is Shore A hardness, which is a value measured in accordance with JIS K 6253 using a durometer (spring type rubber durometer) (model: GS-719G, manufactured by TECLOCK Co., Ltd.).
[0326] The stress at 25% elongation of the adhesive tape of the present embodiment is preferably 0.15MPa to 82MPa, more preferably 0.16MPa to 10MPa, further preferably 0.17MPa to 5MPa, and particularly preferably 0.18MPa to 4.5MPa. When the stress at 25% elongation of the adhesive tape is 0.15MPa to 82MPa, a bonding strength suitable for the adhesive tape can be obtained, and it can be relatively easily peeled off even when the elongation is peeled off. In addition, when the stress at 25% elongation of the adhesive tape is above 0.15MPa, the adhesive tape is not easy to peel off even when a load in the shear direction of the adhesive tape is generated while fixing hard adherends to each other. In addition, when the stress at 25% elongation of the adhesive tape is below 82MPa, when peeling the adhesive tape, the force required to elongate the adhesive tape will not be too large, and it is easy to peel off.
[0327] The stress at 25% elongation of the above-mentioned adhesive tape refers to the stress value measured when the adhesive tape is punched into a dumbbell shape with a marking line length of 20 mm and a width of 5 mm, and stretched in the longitudinal direction at a stretching speed of 500 mm / min under the conditions of a measuring atmosphere of 23°C and 50% RH using a Tensilon tensile testing machine (model: RTF-1210, manufactured by A&D Co., Ltd.) and elongated by 25%.
[0328] The breaking stress of the adhesive tape of the present embodiment is preferably 10MPa to 100.0MPa, more preferably 15MPa to 90.0MPa, further preferably 30MPa to 90.0MPa, and particularly preferably 40MPa to 90.0MPa. When the breaking stress of the adhesive tape is within the above-mentioned preferred range, even when the adhesive tape is rapidly stretched and peeled off, the adhesive tape can be suppressed from rupturing, and the load used to extend the adhesive tape will not be excessively excessive, so the re-peeling operation using peeling becomes easy. In addition, when the breaking stress of the adhesive tape is more than 10MPa, when the adhesive tape is rapidly stretched and peeled off, the adhesive tape is not easy to break, and when it is less than 100.0MPa, when the adhesive tape is stretched and peeled off again, it can be fully stretched and easy to peel off again.
[0329] The breaking stress of the above-mentioned adhesive tape refers to the stress value measured when the adhesive tape is punched into a dumbbell shape with a marking line length of 20 mm and a width of 5 mm, and stretched in the longitudinal direction at a stretching speed of 500 mm / min using a Tensilon tensile tester (model: RTF1210, manufactured by A&D Co., Ltd.) under the conditions of a measuring atmosphere of 23°C and 50% RH, and when the tape breaks.
[0330] The elongation at break of the adhesive tape of the present embodiment is preferably 400% to 2000%, more preferably 500% to 1800%, and further preferably 600% to 1200%. When the elongation at break of the adhesive tape is 400% or more, even when the adhesive tape is firmly bonded to the adherend, when the adhesive tape is peeled off again, the stress for stretching in the horizontal direction to the vertical direction relative to the adherend's attachment surface will not become too large, and when peeling off, the adhesive tape will not be excessively stretched, and can be easily peeled off. In addition, when the elongation at break is less than 2000%, when the adhesive tape is peeled off again, the stretching distance in the horizontal direction to the vertical direction relative to the adherend's attachment surface will not become too long, and the operation can be performed in a small space.
[0331] The elongation at break of the above-mentioned adhesive tape refers to the tensile elongation measured when the adhesive tape is punched into a dumbbell shape with a marking line length of 20 mm and a width of 5 mm, and stretched in the longitudinal direction at a tensile speed of 500 mm / min using a Tensilon tensile tester (model: RTF-1210, manufactured by A&D Co., Ltd.) under the conditions of a measuring atmosphere of 23°C and 50% RH.
[0332] The storage elastic modulus G' (23°C) of the pressure-sensitive adhesive tape of the present embodiment is preferably 1.0×10 4 ~1.0×10 8 Pa, more preferably 5.0×10 4 ~5.0×10 7 Pa, more preferably 1.0×10 5 ~1.0×10 7 Pa, more preferably 3.0×10 5 ~8.0×10 6 Pa. By making the storage elastic modulus of the adhesive tape within the above range, it is easy to follow the deformation of the adherend, etc., and it is easy to obtain excellent bonding strength, and the dimensional stability of the adhesive tape can also be ensured, so that suitable attachment workability can be obtained. It is also conceivable that the adherend of the adhesive tape is a hard adherend such as metal or plastic and is a large-area adherend. Generally speaking, the larger the adherend is, the more difficult it is to suppress deformation and perform molding. However, if it is an adhesive tape with a storage elastic modulus in the above range, the adhesive tape can follow the deformation of the adherend as described above, and suitable bonding strength can be obtained.
[0333] "Method for producing adhesive tape"
[0334] The manufacturing method of the adhesive tape of the present embodiment is not particularly limited and can be appropriately selected from known methods. In the manufacturing method of the adhesive tape of the present embodiment, it is preferably included in the adhesive layer forming step. In addition, when the adhesive tape has a substrate layer, it is preferably included in the adhesive layer forming step, the substrate layer forming step and the lamination step, and further includes other layer forming steps as required. In addition, when the adhesive tape has a substrate layer, it can also be manufactured by simultaneously performing a multi-layer simultaneous forming step of the adhesive layer forming step and the substrate layer forming step.
[0335] The adhesive layer forming step is not particularly limited as long as it can form an adhesive layer, and can be appropriately selected according to the purpose, and examples thereof include a method of forming an adhesive layer on the surface of the release sheet by a hot press method, a casting method based on extrusion molding, a uniaxial stretching method, a sequential secondary stretching method, a simultaneous biaxial stretching method, an inflation method, a tube method, a calendaring method, a solution method, etc. Among them, a casting method based on extrusion molding and a solution method are preferably used.
[0336] The release sheet is not particularly limited and can be appropriately selected according to the purpose, for example, kraft paper, glassine paper, high-grade paper, etc.; resin films such as polyethylene, polypropylene (biaxially stretched polypropylene (OPP), uniaxially stretched polypropylene (CPP)), polyethylene terephthalate (PET), etc.; laminated paper formed by laminating the above paper with a resin film, paper formed by subjecting one or both sides of the above paper to a caulking treatment with clay, polyvinyl alcohol, etc. to a release treatment of silicone resin, etc., etc. These can be used alone or in combination of two or more.
[0337] The above-mentioned substrate layer formation operation is just not particularly limited as long as it can form the substrate layer, and can be suitably selected according to the purpose, for example, hot pressing method, the casting method based on extrusion molding, uniaxial stretching method, successive secondary stretching method, biaxial stretching method, inflation method, tube method, calendering method, solution method etc. can be enumerated. These methods can be used alone or in combination with more than two kinds. Wherein, from the aspect that substrate layer is given suitable flexibility, elongation, it is preferred to use the casting method, inflation method, tube method, calendering method, solution method based on extrusion molding.
[0338] In addition, the substrate layer may be a substrate layer subjected to a surface treatment in order to further improve the adhesion with the adhesive layer.
[0339] There are no particular restrictions on the surface treatment method, and it can be appropriately selected from known methods within the range that does not impair the properties of the adhesive tape. Examples include sandblasting, surface grinding and friction, corona discharge treatment, chromic acid treatment, flame treatment, hot air treatment, ozone treatment, ultraviolet irradiation treatment, and oxidation treatment.
[0340] The above-mentioned lamination process is a process of laminating a substrate layer and an adhesive layer. There is no particular restriction on the method of laminating the substrate layer and the adhesive layer, and it can be appropriately selected from known methods, for example, a method of laminating the adhesive layer and the substrate layer in a state of being attached to a release sheet formed in the adhesive layer forming process by pressurizing the adhesive layer and the substrate layer, etc. can be cited.
[0341] "Uses of Adhesive Tape"
[0342] The adhesive tape of this embodiment can be suitable for use in various industrial fields such as fixing metal plates to each other that constitute relatively large electronic devices such as thin televisions, home appliances, OA equipment, fixing exterior parts to casings, fixing exterior parts of relatively small electronic devices such as portable electronic terminals, cameras, personal computers, and rigid parts such as batteries, temporary fixing of such parts, and labels displaying product information.
[0343] As mentioned above, although embodiment of this invention was described, the adhesive tape of this invention is not limited to the said embodiment, It can change suitably.
[0344] Example
[0345] Hereinafter, the contents of the present invention will be described in detail using examples, but the scope of the present invention is not limited to the following examples.
[0346] The measurement and evaluation of the base material layer, the adhesive layer, and the adhesive tape obtained in each of the Examples and Comparative Examples were performed based on the following methods.
[0347] (1) Determination of breaking stress and breaking elongation of substrate layer
[0348] Each substrate layer was punched into a dumbbell shape with a line length of 20 mm and a width of 5 mm, and stretched in the longitudinal direction at a stretching speed of 500 mm / min using a Tensilon tensile tester (model: RTF1210, manufactured by A&D Co., Ltd.) under the conditions of a measuring atmosphere of 23°C and 50% RH, thereby measuring the breaking stress and breaking elongation of the substrate layer. The results are shown in Table 1 below.
[0349] (2) Measurement of 50% modulus of substrate layer
[0350] Each substrate layer was punched into a dumbbell shape with a marking line length of 20 mm and a width of 5 mm. Under the conditions of a measuring atmosphere of 23°C and 50% RH, it was stretched in the longitudinal direction at a stretching speed of 500 mm / min using a Tensilon tensile testing machine (model: RTF1210, manufactured by A&D Co., Ltd.) to measure the stress value when the substrate layer was elongated by 50%.
[0351] (3) Measurement of thickness of substrate layer and adhesive layer
[0352] The substrate layer and the adhesive layer were cut at 5 locations in the width direction at intervals of 100 mm in the length direction, and the thickness of each cut surface was measured at 5 locations in the width direction at intervals of 100 mm using a TH104 paper / film thickness measuring machine (manufactured by Tester Sangyo Co., Ltd.). The thickness of the total of 25 points was averaged as the thickness of the substrate layer and the adhesive layer.
[0353] (4) Determination of the average particle size D50 of filler particles
[0354] The average particle size (primary particle size) of the filler particles was measured using a measuring machine (Microtrac) utilizing a laser diffraction scattering method.
[0355] (5) Evaluation of 180° peel adhesion
[0356] 180° peeling adhesive force is measured according to JIS Z 0237. Specifically, each adhesive tape is cut into a length of 150 mm and a width of 20 mm, and a PET film of 25 μm thickness is used to line one side of the adhesive tape. Then, the other side of the above-mentioned adhesive tape is attached to a stainless steel plate (length 100 mm, width 30 mm, thickness 3 mm) under the conditions of an atmosphere of 23°C and 50% RH, and a load of 2 kg is applied to the laminated structure of the above-mentioned adhesive tape and the above-mentioned stainless steel plate while reciprocatingly pressing the laminated structure with a roller once to make it crimped, and then the laminated structure is left to stand for 1 hour under the conditions of an atmosphere of 23°C and 50% RH, and the laminated structure is used as a test piece. Then, under the conditions of an atmosphere of 23°C and 50% RH, a Tensilon tensile tester (model: RTF1210, manufactured by A&D Co., Ltd.) is used to stretch the adhesive tape in the above-mentioned test piece in a 180° direction (horizontal direction) at a tensile speed of 300 mm / min, and the 180° peeling adhesive force of the above-mentioned adhesive tape is measured.
[0357] (6) Evaluation of cleavage adhesion
[0358] The double-sided adhesive tape was cut into 30 mm × 50 mm pieces and used as test pieces. The release liner on one side of the test piece was peeled off and attached to the surface of a 3 mm thick stainless steel (SUS) plate. The release liner on the other side was peeled off and attached to the 10 mm side of a 10 mm × 10 mm × 40 mm long test piece. The test piece was subjected to a 50 N / cm 2 The adhesive patch was obtained by pressing for 10 seconds.
[0359] Immediately after the patch was attached in an atmosphere of 23°C and 50% RH, the stainless steel sheet constituting the test piece of the patch was stretched at a rate of 1000 mm / min in an atmosphere of 23°C and 50% RH to measure the peel strength of the stainless steel sheet.
[0360] (7) Evaluation of high load holding capacity
[0361] On a 25mm wide × 80mm wide SUS304 steel plate specified in JIS Z0237, one side of each adhesive tape cut into 25mm wide × 25mm long was pressed back and forth once at a speed of 300mm per minute with a roller weighing 5kg at room temperature and then placed under the conditions of 23°C and 30 minutes. Then, the opposite side of the test piece was pressed back and forth once at a speed of 300mm per minute with a roller weighing 5kg at room temperature and bonded to a 25mm wide × 80mm wide SUS304 steel plate specified in JIS Z0237. Then, it was placed in an atmosphere of 40°C for 30 minutes. Then, a 5kg weight was installed on the gripping part of the test piece, and the test was started by hanging it down, and the time until it fell at 23°C 50% RH was measured. Regarding high load holding power, the case where the falling time is more than 120 minutes is qualified, and the case where the falling time is less than 120 minutes is unqualified.
[0362] (8) Evaluation of removability
[0363] The removability evaluation was conducted by pulling the grip portion provided at one end of the adhesive tape in the longitudinal direction at 90° to the longitudinal direction (90° direction).
[0364] (Repeelability over time in repeelability (90° direction))
[0365] When the 10mm wide × 60mm long adhesive tape is attached to a clean and smooth aluminum plate, in order to use the 10mm wide × 10mm long portion of the adhesive tape as a gripping handle, the gripping handle is attached in a state where it extends from the aluminum plate. Then, the opposite side of the adhesive tape is attached to the lithium-ion battery surface (rough surface) of Apple's iPhone X, and a 2kg load is applied while reciprocating pressure is applied once with a roller to use it as a test piece. After attachment, it is placed in an atmosphere of 23°C and 50% RH for 3 days, and the gripping handle portion is stretched by hand at a speed of about 300mm / min in a direction 90° relative to the length direction of the adhesive tape at 23°C and 50% RH.
[0366] The test was conducted 10 times, and the degree of breakage of the pressure-sensitive adhesive tape and the degree of residual pressure-sensitive adhesive on the adherend after the pressure-sensitive adhesive tape was peeled off were visually evaluated according to the following criteria.
[0367] ◎: The adhesive tape was peeled off cleanly without any breakage or adhesive residue in all 10 times.
[0368] ○: The adhesive tape was peeled off without breaking in all 10 times, but adhesive residue was generated at least once.
[0369] △: 6 to 9 times: The adhesive tape was not broken and the adhesive was not left, and the adhesive was peeled off cleanly.
[0370] ×: The adhesive tape was broken or adhesive residue occurred in 5 to 10 times, or the adhesive tape could not be stretched and peeled off.
[0371] Next, the materials and the like used in Examples and Comparative Examples are described below.
[0372] <Base material (1)>
[0373] As a substrate material used in the substrate (1), a resin composition (1) of styrene-ethylene butylene-styrene copolymer and styrene-ethylene butylene copolymer is used. The resin composition (1) uses a resin composition in which the structural unit derived from styrene represented by the above chemical formula (A) is 29% by weight and the ratio of the styrene-ethylene butylene copolymer to the total amount of the resin composition is 0.5% by weight.
[0374] The resin composition (1) was used to prepare a substrate (1) having a thickness of 50 μm by hot pressing (pressure 0.5 MPa, platen temperature 130° C., pressing time 2 minutes). The substrate (1) had a breaking stress of 80 MPa. The breaking elongation was 700%. In addition, the stress (modulus) at 50% elongation was 3 MPa.
[0375] <Base material (2)>
[0376] As a substrate material used in the substrate (2), a resin composition (2) of a styrene-isoprene copolymer and a styrene-isoprene-styrene copolymer is used. The resin composition (2) uses a resin composition in which the structural unit derived from styrene shown in the above chemical formula (A) is 25% by weight and the ratio of the styrene-isoprene copolymer to the total amount of the resin composition (2) is 16% by weight. The above resin composition (2) is made into a substrate (2) with a thickness of 50 μm by hot pressing (pressure 0.5 MPa, platen temperature 130° C., pressing time 2 minutes). The breaking stress of the substrate (2) is 10 MPa. The elongation at break is 1200%. In addition, the stress (modulus) at 50% elongation is 1 MPa.
[0377] <Adhesive composition>
[0378] The adhesive compositions used in Examples and Comparative Examples contained the following fillers and adhesive resins.
[0379] (filler)
[0380] ·Silicone particles (1)
[0381] As silicone particles (1), particles having a silicone resin surface and a silicone rubber interior (manufactured by Shin-Etsu Chemical Co., Ltd., KMP-602, volume average particle size: 30 μm, particle size distribution (D 90 / D 10 ):5.2).
[0382] Silicone particles (2)
[0383] As silicone particles (2), particles having a silicone resin surface and a silicone rubber interior (manufactured by Shin-Etsu Chemical Co., Ltd., KMP-600, volume average particle size: 5 μm, particle size distribution (D 90 / D 10 ):3.2).
[0384] Silicone particles (3)
[0385] As silicone particles (3), particles having a silicone resin surface and a silicone rubber interior (manufactured by Shin-Etsu Chemical Co., Ltd., KMP-601, volume average particle size: 12 μm, particle size distribution (D 90 / D 10 ):4.4).
[0386] Acrylic particles (1)
[0387] As acrylic particles (1), particles of polymethyl methacrylate (manufactured by Nippon Exlan Industries, Ltd., FH-S010, volume average particle size: 10 μm, particle size distribution (D 90 / D 10 ):2.8).
[0388] <Binder resin>
[0389] <<Synthesis of triblock copolymer>>
[0390] (Synthesis example 1)
[0391] In a flask with an internal volume of 1000 ml replaced with argon, 500 ml of dry toluene and 80 ml of a dry toluene solution of 0.75 g of a bis(pentamethylcyclopentadienyl)samarium·tetrahydrofuran complex [(C5Me5)2SmMe(THF)] as a polymerization initiator were added to prepare a mixed solution. To the mixed solution, 12.0 ml of methyl methacrylate (MMA) was added at 0°C, and stirred at 0°C for 30 minutes. Then, 20 ml of the solution (sample 1) was sampled from the system. After the polymerization of the above MMA, the polymerization reaction system was cooled to -78°C, 88.0 ml of n-butyl acrylate (nBA) was added as the second monomer, and stirred at -78°C for 3 hours. Then, 20 ml of the solution (sample 2) was sampled from the system. After the polymerization of the above nBA, 12.0 ml of MMA was added to the polymer system at -78°C as the third monomer, and the solution was stirred. After the solution becomes uniform, it is heated to 0°C and further stirred for 1 hour. 50 ml of methanol is added to the obtained reaction mixture, and the reaction is carried out at room temperature for 2 hours to stop the polymerization. The reaction solution after the polymerization is stopped is injected into a large amount of hexane to obtain a precipitated white precipitate. Then, a portion of the white precipitate is sampled (sample 3).
[0392] NMR measurement, DSC measurement, and GPC (gel permeation chromatography) measurement were performed on each polymer in the above samples 1 to 3. Then, based on the measurement results, the number average molecular weight (Mn), PMMA / PnBA (polymethyl methacrylate block / poly-n-butyl acrylate block) ratio, etc. were calculated, and the results confirmed that the above white precipitate was a triblock copolymer of polymethyl methacrylate (PMMA) block-poly-n-butyl acrylate (PnBA) block-polymethyl methacrylate (PMMA) block (PMMA-b-PnBA-b-PMMA). In addition, it was confirmed that the syndiotactic stereoregularity of the PMMA block portion of the triblock copolymer (PMMA-b-PnBA-b-PMMA, hereinafter referred to as triblock copolymer (1)) was 71%, the glass transition temperature of the block portion was 113.7°C, the glass transition temperature of the PnBA block portion was -46.8°C, the Mn of the copolymer as a whole was 95936, the Mw / Mn (molecular weight distribution) of the copolymer as a whole was 1.09, and the ratio of each polymer block was PMMA (11 wt%)-PnBA (78 wt%)-PMMA (11 wt%).
[0393] (Synthesis example 2)
[0394] In a flask with an internal volume of 1000 ml replaced with argon, 500 ml of dry toluene and 80 ml of a dry toluene solution of 0.75 g of a bis(pentamethylcyclopentadienyl)samarium·tetrahydrofuran complex [(C5Me5)2SmMe(THF)] as a polymerization initiator were added to prepare a mixed solution. To the mixed solution, 6.0 ml of methyl methacrylate (MMA) was added at 0°C, and stirred at 0°C for 30 minutes. Then, 20 ml of the solution was sampled from the system (sample 4). After the polymerization of the above MMA, the polymerization reaction system was cooled to -78°C, 27.2 ml of n-butyl acrylate (nBA) and 22.1 ml of 2-ethylhexyl acrylate (2EHA) were added as the second monomer, and stirred at -78°C for 3 hours. 20 ml of the solution was sampled from the system (sample 5). After the polymerization of the above nBA, 6.0 ml of MMA was added to the polymer system at -78°C as the third monomer, and the solution was stirred. After the solution becomes uniform, it is heated to 0°C and stirred for another hour. 50 ml of methanol is added to the obtained reaction mixture, and the reaction is carried out at room temperature for 2 hours to stop the polymerization. The reaction solution after the polymerization is stopped is injected into a large amount of hexane to obtain a precipitated white precipitate. Then, a portion of the white precipitate is sampled (sample 6).
[0395] NMR measurement, DSC measurement, and GPC (gel permeation chromatography) measurement were performed on each polymer in the above samples 4 to 6. Then, based on the measurement results, the number average molecular weight (Mn), PMMA / PnBA / P2EHA (polymethyl methacrylate / poly-n-butyl acrylate / poly-2-ethylhexyl acrylate) ratio, etc. were calculated, and the results confirmed that the above white precipitate was a triblock copolymer of polymethyl methacrylate (PMMA) block-poly-n-butyl acrylate (PnBA) / poly-2-ethylhexyl acrylate (2EHA) block-polymethyl methacrylate (PMMA) block (PMMA-b-PnBA / 2EHA-b-PMMA). Furthermore, it was confirmed that the syndiotactic stereoregularity of the PMMA block portion of the triblock copolymer (PMMA-b-PnBA / 2EHA-b-PMMA, hereinafter referred to as triblock copolymer (2)) was 75%, the glass transition temperature of the block portion was 105.8°C, the glass transition temperature of the PnBA block portion was -53.6°C, the Mn of the copolymer as a whole was 51370, the Mw / Mn (molecular weight distribution) of the copolymer as a whole was 1.15, and the ratio of each polymer block was PMMA (10 wt%)-PnBA (44 wt%) / 2EHA (36 wt%)-PMMA (10 wt%).
[0396] <<Other binder resins>>
[0397] (Synthesis example 3)
[0398] As the binder resin, an acrylic random copolymer obtained by the following synthesis was used. 97.97 parts by mass of n-butyl acrylate, 2 parts by mass of acrylic acid, and 0.03 parts by mass of 4-hydroxybutyl acrylate were supplied to ethyl acetate containing 0.2 parts by mass of azobisisobutyronitrile as a polymerization initiator, and solution polymerization was performed at 77° C. for 8 hours to obtain an acrylic random copolymer. Mw was 700,000, and Mw / Mn (molecular weight distribution) was 4.7.
[0399] <Preparation of Adhesive Resin Composition>
[0400] Adhesive composition (1)
[0401] 50 parts by mass of a terpene phenolic tackifier resin (Tamanol T-803L, Arakawa Chemical Industries, Ltd., softening point 150° C.) was mixed and stirred with 100 parts by mass of the triblock copolymer (1) obtained in Synthesis Example 1, and then ethyl acetate was added to obtain a binder resin solution (1) having a solid content of 35% by mass. Next, 30 parts by mass of silicone particles (1) and ethyl acetate were added to 100 parts by mass of the solid content of the binder resin solution (1), and the mixture was stirred and mixed to obtain a uniform binder composition (1) having a solid content of 40% by mass.
[0402] Adhesive composition (2)
[0403] 50 parts by mass of a terpene phenolic tackifier resin (Tamanol T-803L, Arakawa Chemical Industries, Ltd., softening point 150° C.) was mixed and stirred with 100 parts by mass of the triblock copolymer (1) obtained in Synthesis Example 1, and then ethyl acetate was added to obtain a binder resin solution (1) having a solid content of 35% by mass. Next, 30 parts by mass of silicone particles (2) and ethyl acetate were added to 100 parts by mass of the solid content of the binder resin solution (1), and the mixture was stirred and mixed to obtain a uniform binder composition (2) having a solid content of 40% by mass.
[0404] Adhesive composition (3)
[0405] 50 parts by mass of a terpene phenolic tackifier resin (Tamanol T-803L, Arakawa Chemical Industries, Ltd., softening point 150° C.) was mixed and stirred with 100 parts by mass of the triblock copolymer (1) obtained in Synthesis Example 1, and then ethyl acetate was added to obtain a binder resin solution (1) having a solid content of 35% by mass. Next, 30 parts by mass of silicone particles (3) and ethyl acetate were added to 100 parts by mass of the solid content of the binder resin solution (1), and the mixture was stirred and mixed to obtain a uniform binder composition (3) having a solid content of 40% by mass.
[0406] Adhesive composition (4)
[0407] 50 parts by mass of a terpene phenolic tackifier resin (Tamanol T-803L, Arakawa Chemical Industries, Ltd., softening point 150° C.) was mixed and stirred with 100 parts by mass of the triblock copolymer (2) obtained in Synthesis Example 2, and then ethyl acetate was added to obtain a binder resin solution (4) having a solid content of 35% by mass. Next, 30 parts by mass of silicone particles (1) and ethyl acetate were added to 100 parts by mass of the solid content of the binder resin solution (4), and the mixture was stirred and mixed to obtain a uniform binder composition (4) having a solid content of 40% by mass.
[0408] Adhesive composition (5)
[0409] 50 parts by mass of a terpene phenolic tackifier resin (Tamanol T-803L, Arakawa Chemical Industries, Ltd., softening point 150° C.) was mixed and stirred with 100 parts by mass of the triblock copolymer (1) obtained in Synthesis Example 1, and then ethyl acetate was added to obtain a binder resin solution (1) having a solid content of 35% by mass. Next, 30 parts by mass of acrylic particles (1) and ethyl acetate were added to 100 parts by mass of the solid content of the binder resin solution (1), and the mixture was stirred and mixed to obtain a uniform binder composition (5) having a solid content of 40% by mass.
[0410] Adhesive composition (6)
[0411] 50 parts by mass of a terpene phenolic tackifier resin (Tamanol T-803L, Arakawa Chemical Industries, Ltd., softening point 150° C.) was mixed and stirred with 100 parts by mass of the triblock copolymer (1) obtained in Synthesis Example 1, and then ethyl acetate was added to obtain a binder resin solution (1) having a solid content of 35% by mass. Next, 10 parts by mass of silicone particles (3) and ethyl acetate were added to 100 parts by mass of the solid content of the binder resin solution (1), and the mixture was stirred and mixed to obtain a uniform binder composition (6) having a solid content of 40% by mass.
[0412] Adhesive composition (7)
[0413] 100 parts by mass of the acrylic random copolymer obtained in Synthesis Example 3 was mixed with 5 parts by mass of a rosin-based tackifier resin (Haritack PCJ, Harima Chemicals Co., Ltd., softening point 135°C) and 45 parts by mass of a petroleum-based tackifier resin (FTR6125, Mitsui Chemicals, Inc., softening point 125°C) and stirred, and then ethyl acetate was added to obtain a binder resin solution (7) having a solid content of 35% by mass. Next, 30 parts by mass of silicone particles (1) and ethyl acetate were added to 100 parts by mass of the solid content of the binder resin solution (7), and the mixture was stirred and mixed to obtain a uniform binder composition (7) having a solid content of 40% by mass.
[0414] Adhesive composition (8)
[0415] 50 parts by mass of a terpene phenolic tackifier resin (Tamanol T-803L, Arakawa Chemical Industries, Ltd., softening point 150° C.) was mixed and stirred with 100 parts by mass of the triblock copolymer (1) obtained in Synthesis Example 1, and then ethyl acetate was added to obtain a binder resin solution (8) having a solid content of 40% by mass.
[0416] "Manufacture of adhesive tape"
[0417] [Example 1]
[0418] The adhesive composition (1) was applied to a release liner (FilmBina 75E-0010GT, manufactured by Fujimori Industries, Ltd., hereinafter the same) using an applicator so that the thickness after drying was 50 μm, and dried at 80° C. for 3 minutes to prepare an adhesive layer. Next, both sides of the substrate (1) as a substrate layer were subjected to corona treatment so that the wetting tension became 52 mN / m, and then the adhesive layer was attached to both sides. The laminated structure of the substrate layer and the adhesive layer was pressed at 0.2 MPa to laminate, thereby preparing an adhesive tape of Example 1. The adhesive tape obtained by the above method was evaluated, and the results are shown in Table 1.
[0419] [Example 2]
[0420] The pressure-sensitive adhesive tape of Example 2 was produced in the same manner as in Example 1 except that the thickness of the pressure-sensitive adhesive layer was changed from 50 μm to 30 μm. The pressure-sensitive adhesive tape obtained by the above-described method was evaluated. The results are shown in Table 1.
[0421] [Example 3]
[0422] The pressure-sensitive adhesive tape of Example 3 was produced in the same manner as in Example 1 except that the pressure-sensitive adhesive composition (1) was changed to the pressure-sensitive adhesive composition (2). The pressure-sensitive adhesive tapes obtained were evaluated by the above-mentioned methods. The results are shown in Table 1.
[0423] [Example 4]
[0424] The pressure-sensitive adhesive tape of Example 4 was produced in the same manner as in Example 1 except that the pressure-sensitive adhesive composition (1) was changed to the pressure-sensitive adhesive composition (3). The pressure-sensitive adhesive tapes obtained by the above-mentioned methods were evaluated. The results are shown in Table 1.
[0425] [Example 5]
[0426] The pressure-sensitive adhesive tape of Example 5 was produced in the same manner as in Example 1 except that the pressure-sensitive adhesive composition (1) was changed to the pressure-sensitive adhesive composition (4). The pressure-sensitive adhesive tapes obtained were evaluated by the above-mentioned methods. The results are shown in Table 1.
[0427] [Example 6]
[0428] The pressure-sensitive adhesive tape of Example 6 was produced in the same manner as in Example 1 except that the pressure-sensitive adhesive composition (1) was changed to the pressure-sensitive adhesive composition (5). The pressure-sensitive adhesive tapes obtained were evaluated by the above-mentioned methods. The results are shown in Table 1.
[0429] [Example 7]
[0430] The pressure-sensitive adhesive tape of Example 7 was produced in the same manner as in Example 1 except that the pressure-sensitive adhesive composition (1) was changed to the pressure-sensitive adhesive composition (6). The pressure-sensitive adhesive tapes obtained were evaluated by the above-mentioned methods. The results are shown in Table 1.
[0431] [Example 8]
[0432] The pressure-sensitive adhesive tape of Example 8 was produced in the same manner as in Example 1 except that the substrate (1) was changed to the substrate (2). The pressure-sensitive adhesive tapes obtained by the above-mentioned methods were evaluated. The results are shown in Table 1.
[0433] [Comparative Example 1]
[0434] A pressure-sensitive adhesive tape of Comparative Example 1 was produced in the same manner as in Example 1 except that the pressure-sensitive adhesive composition (1) was changed to the pressure-sensitive adhesive composition (7). The pressure-sensitive adhesive tape obtained was evaluated by the above-mentioned method. The results are shown in Table 2.
[0435] [Comparative Example 2]
[0436] The pressure-sensitive adhesive tape of Comparative Example 2 was produced in the same manner as in Example 1 except that the thickness of the pressure-sensitive adhesive was changed from 50 μm to 10 μm. The pressure-sensitive adhesive tape obtained was evaluated by the above-mentioned method. Table 2 shows the results.
[0437] [Comparative Example 3]
[0438] A pressure-sensitive adhesive tape of Comparative Example 3 was produced in the same manner as in Example 1 except that the pressure-sensitive adhesive composition (1) was changed to the pressure-sensitive adhesive composition (8). The pressure-sensitive adhesive tape obtained was evaluated by the above-mentioned method. The results are shown in Table 2.
[0439] [Table 1]
[0440]
[0441] [Table 2]
[0442]
[0443] As can be seen from Tables 1 and 2, the pressure-sensitive adhesive tapes of Examples have high load holding power, high peeling adhesion, and high cleavage adhesion, but are also excellent in removability. In particular, it can be seen that the smaller the D50 / T, the better the peeling adhesion and cleavage adhesion.
Claims
1. An adhesive tape comprising an adhesive layer, in, The adhesive layer comprises a tackifying resin, filler particles and a triblock copolymer having repeating units represented by the following general formula (1): In the above general formula (1), A, B and C each independently represent a repeating unit, A and C each independently represent an alkyl methacrylate monomer unit, B represents an alkyl acrylate monomer unit, p, q and r each independently represent the degree of polymerization of each monomer unit, A and C are the same or are alkyl methacrylate monomer units with different chemical structures. In the above general formula (1), * represents the bonding position with other atoms. D50 / T, which is the relationship between the average particle size D50 of the filler particles and the average thickness T of the adhesive layer, is in the range of 0.05 to 1.
0. The filler particles are selected from polystyrene fillers, benzoguanamine fillers, polyethylene fillers, polypropylene fillers, silicone fillers, urea-formalin fillers, styrene / methacrylic acid copolymers, fluorine fillers, acrylic fillers, polycarbonate fillers, polyurethane fillers, polyamide fillers, epoxy resin fillers, and thermosetting resin hollow fillers. The particle size distribution (D90 / D10) of the filler particles is 2.5 to 20, The weight average molecular weight Mw of the triblock copolymer is 50,000 to 130,000. The adhesive layer contains 50 to 100% by mass of the triblock copolymer relative to the entire binder resin. In the triblock copolymer, "-(A) p The syndiotacticity of the polymer block in the -" part shows a ratio of rr triads of more than 65%, The triblock copolymer "-(C) r The syndiotacticity of the polymer block in the -" part shows a ratio of rr triads of more than 65%, The average thickness T of the adhesive layer is 5 μm to 150 μm.
2. The adhesive tape according to claim 1, in, The pressure-sensitive adhesive tape further includes a base layer in contact with one surface of the pressure-sensitive adhesive layer.
3. The adhesive tape according to claim 1 or 2, in, The adhesive tape has a peel adhesion of 5 N / 20 mm or more.
4. The adhesive tape according to claim 1 or 2, in, The splitting adhesive force of the adhesive tape is 10 to 200 N / cm 2 .
5. The adhesive tape according to claim 1, in, The adhesive layer contains 10 to 150 parts by mass of the tackifier resin based on 100 parts by mass of the triblock copolymer.
6. The adhesive tape according to claim 2, in, The substrate layer has a breaking stress of 1 to 100 MPa, a breaking elongation of 400 to 3000%, and a 50% modulus of 0.1 to 5 MPa.
7. The adhesive tape according to claim 1 or 2, in, The adhesive tape can be stretched and peeled.