Upconversion nanoparticles, preparation method and application thereof
By using core-shell structure and sandwich sandwich structure design in rare earth up-conversion nanomaterials, the problem of low luminescence efficiency of rare earth up-conversion nanomaterials is solved, efficient up-conversion efficiency and low energy loss are achieved, and it has expanded its biomedical system. Application in the field.
Patent Information
- Application Number
- CN202210153710.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-02-19
AI Technical Summary
The low luminous efficiency of rare earth upconverting nanomaterials limits their application in the field of biomedical science, especially in the early diagnosis and treatment of cancer.
Upconvert nanoparticles using core-shell structure, the nanocore is a fluoride without rare earth ion doping, plus a near-infrared light absorption sensitization upconverting luminescent layer and isolation layer to form a sandwich sandwich structure, reducing light energy loss and improving upconversion efficiency.
It significantly improves the upconversion efficiency of ultraviolet light, reduces energy loss, and enhances the biolight function of nanoparticles. It is suitable for display, bioimaging and cancer treatment.
Smart Images

Figure CN114958335B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nano luminescent materials, and in particular relates to up-conversion nanoparticles, a preparation method thereof and applications thereof. Background Art
[0002] Rare earth upconversion nanomaterials have the optical property of upconverting near-infrared light into ultraviolet to near-infrared light, and are widely used in display, detection, three-dimensional display, and especially in biomedicine. However, due to the limitations of the upconversion luminescence mechanism and the small light absorption cross-section of rare earth ions, the fluorescence quantum yield and luminescence efficiency of rare earth upconversion nanomaterials are very low, which greatly limits the development of the material. Therefore, it is particularly important to find a method that can effectively improve the luminescence efficiency of rare earth upconversion nanomaterials.
[0003] The core-shell structure material is a composite material, which consists of a core composed of micro-nano-sized particles, and then a layer or multiple layers of uniform materials with the same or similar lattice constants are coated on the core to form a shell. The core and the shell are bonded by electrostatic interaction or chemical bonds. By preparing core-shell rare earth upconversion nanomaterials, the luminescence quenching of interface defects of rare earth upconversion materials can be suppressed, especially the surface defects of the outer cold wind can be passivated and the interference of adverse external factors can be isolated, thereby improving the upconversion efficiency of the material. At the same time, a series of excellent properties can be given to the material. For example: the surface selectively coated with a hydrophilic or hydrophobic single-layer shell can change the hydrophilicity or hydrophobicity of the material surface. In addition, coating with multiple functional shells can enable upconversion nanomaterials to integrate multimodal imaging and visualized precise diagnosis and treatment functions.
[0004] Although the core-shell structure effectively improves the luminescence efficiency of upconversion nanomaterials, it still has the defects of low emission efficiency and large energy loss, which greatly limits the widespread application of upconversion nanoluminescent materials in the early diagnosis and treatment of major diseases such as cancer in the biomedical field.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] In order to solve the above problems, the first object of the present invention is to provide an upconversion nanoparticle, which has a core-shell structure and can effectively reduce the energy loss of photons during the energy conversion process and improve the upconversion efficiency.
[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0008] Upconversion nanoparticles, the upconversion nanoparticles having a core-shell structure, the upconversion nanoparticles comprising, from the inside to the outside, a fluoride nanoparticle core that is not doped with any rare earth ions and fully transmits and does not absorb ultraviolet to near-infrared light, a near-infrared light absorption sensitized upconversion luminescent layer, and an isolation layer;
[0009] The near-infrared light absorption sensitized up-conversion luminescent layer is mainly composed of a matrix material, sensitizing ions and activating ions;
[0010] The fluoride nanoparticle core and the isolation layer have the same material composition.
[0011] The isolation layer is a fluoride nano isolation layer without any rare earth ion doping, which fully transmits and does not absorb ultraviolet to near infrared light.
[0012] The up-conversion nanoparticles provided by the present invention have a nanocore that is a fluoride nanocore without any rare earth ion doping, and the nanocore material does not absorb and fully transmits ultraviolet light to near-infrared light, eliminating the light energy loss caused by the strong absorption of ultraviolet to near-infrared 980nm excitation light energy by the fluoride nanocrystals commonly used as nanocores doped with rare earth ions. The outer layer of the nanocore is a near-infrared light absorption sensitized up-conversion luminescent layer, which is composed of a matrix material, sensitizing ions and activation ions. The sensitizing ions play a role in efficiently absorbing near-infrared light energy transfer and sensitizing the activation ions to emit light. After absorbing the excitation light energy, they transfer the absorbed near-infrared light energy to the neighboring luminescent ions through resonance transmission, and the multi-photon absorption of the luminescent ions is sensitized to a higher energy state to generate up-conversion luminescence. In addition, the isolation layer of the present invention also uses a fluoride nanomaterial without any rare earth ion doping as an isolation layer, and also has no absorption of ultraviolet to near-infrared light, further suppressing the surface defects of the nanoparticles and the loss of 980nm near-infrared excitation light energy by ligand molecules. The nano core and the isolation layer are made of the same material, both of which do not absorb and fully transmit light from ultraviolet to near-infrared. The upconversion luminescent layer is added between the nano core and the isolation shell layer, and is confined in the photon energy deep potential well formed by the nano core and the isolation shell layer. The first layer of near-infrared light high absorption sensitizing shell layer, the second layer of sensitizing luminescent layer and the third layer of near-infrared light high absorption sensitizing shell layer form a sandwich structure. The fourth layer of the deep potential well outer wall isolation layer effectively isolates the outer surface defect states of the composite upconversion nanoparticles and the exchange of surface ligand molecules with the sensitizing ions and luminescent ions in the near-infrared absorption sensitized upconversion luminescent layer, reduces the quenching process of upconversion ultraviolet light, thereby effectively enhancing the upconversion efficiency of ultraviolet light with a wavelength of about 340nm.
[0013] In one aspect of the present invention, the material of the fluoride nanoparticle core includes one of LiYF4, LiLuF4, LiGdF4, NaYF4, NaLuF4, NaGdF4, KYF4, KLuF4, and KGdF4.
[0014] The material of the isolation layer includes one of LiYF4, LiLuF4, LiGdF4, NaYF4, NaLuF4, NaGdF4, KYF4, KLuF4, and KGdF4.
[0015] Preferably, the material of the fluoride nanoparticle core is selected from one of LiYF4, LiLuF4, LiGdF4, NaYF4, NaLuF4, and NaGdF4.
[0016] The material of the isolation layer is selected from one of LiYF4, LiLuF4, LiGdF4, NaYF4, NaLuF4, and NaGdF4.
[0017] Since Li and Na have smaller ionic radii, the material constituting the nanocore and the material constituting the isolation layer are preferably fluorides containing Li and Na.
[0018] In the present invention, the diameter of the particle core is less than 20 nm; preferably, the diameter of the particle core is 15-18 nm.
[0019] In another aspect of the present invention, the near-infrared light absorption sensitization up-conversion luminescent layer comprises, from the inside to the outside, an inner near-infrared light absorption sensitization layer, an up-conversion ultraviolet light emitting layer and an outer near-infrared light absorption sensitization layer.
[0020] The up-conversion ultraviolet light emitting layer is mainly composed of a matrix material, sensitizing ions and activating ions.
[0021] The matrix material of the inner near-infrared light absorption sensitization layer and the matrix material of the outer near-infrared light absorption sensitization layer are both matrix materials with high absorption of near-infrared light.
[0022] The inner near-infrared light absorption sensitizing layer and the outer near-infrared light absorption sensitizing layer have the same material composition.
[0023] The matrix material of the up-conversion ultraviolet light emitting layer is a matrix material that does not absorb near-infrared light.
[0024] In the present invention, the near-infrared light absorption sensitization up-conversion luminescent layer can be composed of three layers, namely, an inner near-infrared light absorption sensitization layer, an up-conversion ultraviolet light emission layer, and an outer near-infrared light absorption sensitization layer. The inner light absorption sensitization layer and the outer light absorption sensitization layer are both made of matrix materials without any rare earth ion doping, and both efficiently resonate and absorb 980nm near-infrared light. The inner light absorption sensitization layer absorbs 980nm near-infrared light in its material and sensitizes the activation ions of the luminescent layer from the inside in a photon energy resonance mode. The outer light absorption sensitization layer also sensitizes the activation ions of the luminescent layer from the side in a photon energy resonance mode. Due to the symmetrical deep potential well of the inner nanocore and the outermost isolation layer, the loss of near-infrared light is avoided as much as possible, and the most efficient sensitization and activation of the inner and outer sides of the activation ions of the luminescent layer by 980nm near-infrared light is achieved, and the most efficient up-conversion ultraviolet luminescence is obtained. In the present invention, the thickness of the inner near-infrared light absorption sensitization layer is not more than 3nm, preferably 1.5-2.5nm.
[0025] In the present invention, the thickness of the up-conversion ultraviolet light emitting layer is not greater than 3 nm, preferably 1.5-2.5 nm.
[0026] In the present invention, the thickness of the outer near-infrared light absorption sensitization layer is not greater than 3 nm, preferably 1.5-2.5 nm.
[0027] The matrix material of the inner near-infrared light absorption sensitization layer includes one of LiYbF4, NaYbF4, and KYbF4, and the matrix material of the outer near-infrared light absorption sensitization layer includes one of LiYbF4, NaYbF4, and KYbF4.
[0028] The matrix material of the up-conversion ultraviolet light emitting layer has the same material composition as that of the fluoride nanoparticle core, except that the sensitizing ions are substituted or doped with sensitizing ions and activating ions of different concentrations.
[0029] The materials selected for the inner near-infrared light absorption sensitization layer and the outer near-infrared light absorption sensitization layer of the present invention have a very high energy resonance absorption effect on 980nm near-infrared light.
[0030] Preferably, the matrix material of the inner near-infrared light absorption sensitization layer is selected from one of LiYbF4 and NaYbF4.
[0031] The matrix material of the outer near-infrared light absorption sensitization layer is selected from one of LiYbF4 and NaYbF4.
[0032] Furthermore, the sensitizing ions include Yb 3+ , the activation ions include Er 3+ 、Tm 3+ 、Ho 3+ The sensitizing ion is a dual-functional ion of absorption and sensitization.
[0033] The matrix material of the inner near-infrared light absorption sensitization layer and the matrix material of the outer near-infrared light absorption sensitization layer of the present invention have very good energy resonance absorption of 980nm near-infrared light and have energy resonance sensitization effect on the activation ions of the sandwich luminescent layer. The matrix material selected for the up-conversion ultraviolet light emission layer does not absorb ultraviolet to near-infrared light, avoiding the loss of intrinsic matrix energy, and the near-infrared light absorption sensitization ion Yb doped therein 3+ The absorbed 980nm excitation light energy is transferred to the nearest neighboring activation ion Er in a resonant manner 3+ 、Tm 3+ 、Ho 3+ Under the excitation of 980nm near-infrared light, the single-core multi-shell upconversion nanoparticles emit highly efficient upconversion ultraviolet light in the 300-400nm spectral range.
[0034] Preferably, the sensitizing ion is Yb 3+ , the activation ion Tm 3+ . Sensitizing ion Yb 3+ and activation ion Tm 3+ It has good energy resonance transfer and conversion ultraviolet light effect.
[0035] The material composition of the up-conversion ultraviolet light emitting layer includes one of the following components:
[0036] LiYF4: 0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、LiGdF4: 0.5~1.5%Tm 3+ ,20~25%Yb 3+ ,
[0037] LiLuF4: 0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、NaYF4: 0.5~1.5%Tm 3+ ,20~25%Yb 3+ ,
[0038] NaGdF4: 0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、NaLuF4: 0.5~1.5%Tm 3+ ,20~25%Yb 3+ ,
[0039] KGdF4: 0.5~1.5%Tm 3+ ,20~25%Yb 3+ KYF4: 0.5~1.5%Tm 3+ ,20~25%Yb 3+ ,
[0040] KLuF4: 0.5~1.5%Tm 3+ ,20~25%Yb 3+ .
[0041] The above components may be, for example:
[0042] LiYF4:0.5%Tm 3+ ,20%Yb 3+ 、LiYF4:1%Tm 3+ ,20%Yb 3+ 、LiYF4:1.5%Tm 3+ ,25%Yb 3+ ,
[0043] LiGdF4:0.5%Tm3+ ,20%Yb 3+ 、LiGdF4:1%Tm 3+ ,20%Yb 3+ 、LiGdF4:1.5%Tm 3+ ,25%Yb 3 + 、
[0044] LiLuF4:0.5%Tm 3+ ,20%Yb 3+ 、LiLuF4:1%Tm 3+ ,20%Yb 3+ 、NaYF4:1.5%Tm 3+ ,25%Yb 3 + 、
[0045] NaGdF4:0.5%Tm 3+ ,20%Yb 3+ 、NaGdF4:1%Tm 3+ ,20%Yb 3+ 、NaGdF4:1.5%Tm 3+ ,25%Yb 3 + 、
[0046] NaLuF4:0.5%Tm 3+ ,20%Yb 3+ 、NaLuF4:1%Tm 3+ ,20%Yb 3+ 、NaLuF4:1.5%Tm 3+ ,25%Yb 3 + 、
[0047] KGdF4:0.5%Tm 3+ ,20%Yb 3+ 、KGdF4:1%Tm 3+ ,20%Yb 3+ 、KGdF4:1.5%Tm 3+ ,25%Yb 3+ 、
[0048] KYF4:0.5%Tm 3+ ,20%Yb 3+ 、KYF4:1%Tm 3+ ,20%Yb 3+ 、KYF4:1.5%Tm 3+ ,25%Yb 3+ 、
[0049] KLuF4:0.5%Tm 3+ ,20%Yb 3+ 、KLuF4:1%Tm 3+ ,20%Yb 3+ 、KLuF4:1.5%Tm 3+ ,25%Yb 3+ .
[0050] The selection and dosage of matrix materials, sensitizing ions and activating ions are particularly important for the conversion efficiency of infrared light. Excessive dosage of activating ions and insufficient dosage of matrix materials will cause the quenching effect of the activator photons themselves. In the present invention, the specific composition of the matrix material, sensitizing ions and activating ions of the above-mentioned up-conversion ultraviolet light emitting layer can make the up-conversion ultraviolet light emitting layer have a more excellent light conversion efficiency.
[0051] In the present invention, the diameter of the above-mentioned upconversion nanoparticles is 32-35 nm.
[0052] The upconversion nanoparticles have a small diameter and can be prepared into drugs for treating cancer. They can easily pass through the cell membrane and enter the interior of cancer cells, thereby exerting their therapeutic effects.
[0053] The present invention provides a method for preparing the above-mentioned upconversion nanoparticles, comprising sequentially coating near-infrared light absorption sensitized upconversion luminescent layer material and isolation layer material on fluoride nanoparticles which are not doped with any rare earth ions and fully transmit and do not absorb ultraviolet to near-infrared light;
[0054] Preferably, the inner near-infrared light absorption sensitization layer material, the up-conversion ultraviolet light emission layer material, the outer near-infrared light absorption sensitization layer material and the isolation layer material are sequentially coated on the outside of the fluoride nanoparticles which are not doped with any rare earth ions and fully transmit and do not absorb ultraviolet to near-infrared light.
[0055] The present invention also provides applications of the above-mentioned up-conversion nanoparticles in display, biological imaging, and preparation of cancer treatment drugs.
[0056] The beneficial effects of the present invention are as follows:
[0057] (1) The upconversion nanoparticles of the present invention, the particle core and the isolation layer are made of fluoride nanomaterials that are completely transparent and non-absorbent to ultraviolet to near-infrared light without any rare earth ion doping, and the materials of the two are the same. Not only do they not absorb and fully transmit 980nm near-infrared light, but the two also form a symmetrical deep energy potential well in the "sandwich" structure, which has a strong limiting effect on photon energy, effectively avoiding the exchange of ultraviolet photon energy converted by the light absorption sensitive layer and the light emitting layer with the surface defect states of the composite upconversion nanoparticles and the vibration energy of the surface ligand molecules, reducing the quenching process of the upconversion ultraviolet light, thereby effectively enhancing the upconversion efficiency of ultraviolet light with a wavelength of about 340nm. In addition, in the "sandwich" structure within this symmetrical deep potential well, the near-infrared light absorption sensitized upconversion luminescent layer can be further composed of an inner light absorption sensitized layer, a near-infrared absorption sensitized upconversion ultraviolet light emitting layer, and an outer near-infrared light sensitized layer. Since the inner light absorption sensitized layer and the outer light absorption sensitized layer have 100% Yb 3+ The composition has high absorption of 980nm near-infrared light, and forms a symmetrical injection layer with high optical density of 980nm near-infrared light for the up-conversion ultraviolet light emission layer in the middle, which greatly improves the absorption efficiency of 980nm near-infrared light and the emission efficiency of up-conversion ultraviolet light by the activated ions in the up-conversion ultraviolet light emission layer. Therefore, the up-conversion nanoparticle biophotofunctional system of the present invention greatly reduces the energy loss of photons during the energy conversion process and has very excellent up-conversion efficiency. (2) The preparation method of the up-conversion nanoparticles provided by the present invention is simple.
[0058] (3) The upconversion nanoparticles provided by the present invention have a small particle size, very low energy loss and excellent upconversion efficiency, and therefore have a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0060] Figure 1 LiYF4@LiYbF4@LiYF4:1%Tm prepared in Example 1 3+ ,20%Yb 3+ Flow chart of the preparation of upconversion nanoparticles of @LiYbF4@LiYF4;
[0061] Figure 2 The bare-core LiYF4 nanocrystal prepared in Example 1
[0062] Figure 3 LiYF4@LiYbF4@LiYF4:1%Tm prepared in Example 1 3+,20%Yb 3+ Scanning electron microscope image of @LiYbF4@LiYF4
[0063] Figure 4 LiYF4:1%Tm 3+ ,20%Yb 3+ @LiYbF4@LiYF4 structured upconversion nanoparticles and LiYF4@LiYbF4@LiYF4 prepared in Example 1: 1% Tm 3+ ,20%Yb 3+ Upconversion spectrum of @LiYbF4@LiYF4 structure upconversion nanoparticles. DETAILED DESCRIPTION
[0064] In order to more clearly explain the overall concept of the present application, the following is described in detail in conjunction with the accompanying drawings of the specification by way of embodiment. In the following description, a large number of specific details are provided to provide a more thorough understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present invention, some technical features well known in the art are not described.
[0065] If no specific conditions are specified in the examples, the experiments were carried out according to conventional conditions or conditions recommended by the manufacturer.
[0066] Unless otherwise specified, in the following embodiments, the reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.
[0067] Example 1
[0068] (1) Preparation of LiYF4: Dissolve 1 nmol CF3COOLi and 1 nmol Y(CF3COO)3 in 10 ml of oleylamine and stir at 100°C for 30 minutes to obtain a LiYF4 precursor solution.
[0069] (2) Preparation of LiYbF4: Dissolve 1 nmol CF3COOLi and 1 nmol Yb(CF3COO)3 in 10 ml of oleylamine and stir at 100°C for 30 minutes to obtain a LiYbF4 precursor solution.
[0070] (3) LiYF4: 1% Tm 3+ ,20%Yb 3+Preparation: 1 nmol of CF3COOLi, 0.79 nmol of Y(CF3COO)3, 0.2 nmol of Yb(CF3COO)3 and 0.01 nmol of Tm(CF3COO)3 were dissolved in 10 ml of oleylamine and stirred at 100 °C for 30 minutes to obtain LiYF4:1%Tm 3+ ,20%Yb 3+ Precursor solution.
[0071] (4) Add 5 ml of LiYF4 precursor solution to a three-necked flask, gradually heat it to 320°C under argon protection, the heating rate is about 10°C / min, stir and keep reacting for 30 minutes to form LiYF4 nanocrystals as a bare core colloidal solution, cool the core solution to 150°C, drip 2 ml of LiYbF4 precursor solution dropwise, the dripping rate is about 0.5 ml / min, gradually heat it to 320°C under argon protection, the heating rate is about 10°C / min, stir and keep reacting for 30 minutes to form LiYF4@LiYbF4 nanostructures. Cool down to 150°C, drip LiYF4:1%Tm dropwise 3+ ,20%Yb 3+ The precursor solution was 2 ml, and the drop rate was about 0.5 ml / min. Under argon protection, the temperature was gradually raised to 320°C at a rate of about 10°C / min. The reaction was stirred and maintained for 30 minutes to form LiYF4@LiYbF4@LiYF4:1%Tm 3+ ,20%Yb 3+ The temperature was lowered to 150°C, and 2 ml of LiYbF4 precursor solution was added dropwise at a rate of about 0.5 ml / min. Under argon protection, the temperature was gradually raised to 320°C at a rate of about 10°C / min. The reaction was stirred and maintained for 30 minutes to form LiYF4@LiYbF4@LiYF4:1%Tm 3+ ,20%Yb 3+ @LiYbF4 particles. Cool down to 150℃, drip 2ml of LiYF4 precursor solution drop by drop, with a drip rate of about 0.5ml / min, gradually heat up to 320℃ under argon protection, with a heating rate of about 10℃ / min, stir and keep reacting for 30 minutes to form LiYF4@LiYbF4@LiYF4:1%Tm 3+ ,20%Yb 3+ @LiYbF4@LiYF4.
[0072] Example 2
[0073] (1) Preparation of NaYF4: Dissolve 1 nmol CF3COONa and 1 nmol Y(CF3COO)3 in 10 ml of oleylamine and stir at 100°C for 30 minutes to obtain a NaYF4 precursor solution.
[0074] (2) Preparation of NaYbF4: Dissolve 1 nmol CF3COONa and 1 nmol Yb(CF3COO)3 in 10 ml of oleylamine and stir at 100°C for 30 minutes to obtain a NaYbF4 precursor solution.
[0075] (3) NaYF4: 1% Tm 3+ ,20%Yb 3+ Preparation: Dissolve 1 nmol of CF3COONa, 0.79 nmol of Y(CF3COO)3, 0.2 nmol of Yb(CF3COO)3 and 0.01 nmol of Tm(CF3COO)3 in 10 ml of oleylamine and stir at 100°C for 35 minutes to obtain NaYF4:1%Tm 3+ ,20%Yb 3+ Precursor solution.
[0076] (4) Add 5 ml of NaYF4 precursor solution to a three-necked flask, gradually heat it to 295°C under argon protection, the heating rate is about 10°C / min, stir and keep reacting for 30 minutes, form NaYF4 nanocrystals as bare core colloidal solution, cool the core solution to 150°C, drip 2 ml of NaYbF4 precursor solution drop by drop, the dripping rate is about 0.5 ml / min, gradually heat it to 320°C under argon protection, the heating rate is about 10°C / min, stir and keep reacting for 30 minutes, form NaYF4@NaYbF4 nanostructure. Cool down to 150°C, drip NaYF4:1%Tm drop by drop 3+ ,20%Yb 3+ The precursor solution was 2 ml, and the drop rate was about 0.5 ml / min. Under argon protection, the temperature was gradually raised to 295°C at a rate of about 10°C / min. The reaction was stirred and maintained for 30 minutes to form NaYF4@NaYbF4@NaYF4:1%Tm 3+ ,20%Yb 3+ The temperature was lowered to 150°C, and 2 ml of NaYbF4 precursor solution was added dropwise at a rate of about 0.5 ml / min. Under argon protection, the temperature was gradually raised to 320°C at a rate of about 10°C / min. The reaction was stirred and maintained for 30 minutes to form NaYF4@NaYbF4@NaYF4:1%Tm 3+ ,20%Yb 3+@NaYbF4 particles. Cool down to 150℃, drip 2ml of LiYF4 precursor solution drop by drop, with a drip rate of about 0.5ml / min, gradually heat up to 295℃ under argon protection, with a heating rate of about 10℃ / min, stir and keep reacting for 30 minutes to form NaYF4@NaYbF4@NaYF4:1%Tm 3+ ,20%Yb 3+ @NaYbF4@NaYF4.
[0077] (5) Centrifugal separation and ultrasonic washing with cyclohexane to obtain product upconversion nanoparticles
[0078] NaYF4@NaYbF4@NaYF4:1%Tm 3+ ,20%Yb 3+ @NaYbF4@NaYF4.
[0079] Example 3
[0080] The difference from Example 1 is that in step (2), the preparation of LiLuF4 is to replace Yb(CF3COO)3 in Example 1 with Lu(CF3COO)3, and the rest of the preparation method is the same as that in Example 1. In step (4), the precursor solution of LiYbF4 is replaced with the precursor solution of LiLuF4 to prepare LiYF4@LiLuF4@LiYF4:1%Tm 3+ ,20%Yb 3+ @LiLuF4@LiYF4.
[0081] Example 4
[0082] The difference from Example 1 is that in step (2), the preparation of LiGdF4 is to replace Yb(CF3COO)3 in Example 1 with Gd(CF3COO)3, and the rest of the preparation method is the same as that in Example 1. In step (4), the precursor solution of LiYbF4 is replaced with the precursor solution of LiGdF4 to prepare LiYF4@LiGdF4@LiYF4:1%Tm 3+ ,20%Yb 3+ @LiGdF4@LiYF4.
[0083] Example 5
[0084] The substance containing the Li element in Example 1 is replaced by a substance containing the K element.
[0085] Example 6
[0086] The difference from Example 1 is that: Step (3) LiYF4: 1.5% Tm 3+ ,25%Yb 3+Preparation: 1 nmol of CF3COOLi, 0.735 nmol of Y(CF3COO)3, 0.25 nmol of Yb(CF3COO)3 and 0.015 nmol of Tm(CF3COO)3 were dissolved in 10 ml of oleylamine and stirred at 100 °C for 30 minutes to obtain LiYF4: 1.5% Tm 3+ ,25%Yb 3+ Precursor solution.
[0087] Example 7
[0088] The difference from Example 1 is that: Step (3) LiYF4: 0.5% Tm 3+ ,20%Yb 3+ Preparation: 1 nmol of CF3COOLi, 0.795 nmol of Y(CF3COO)3, 0.20 nmol of Yb(CF3COO)3 and 0.005 nmol of Tm(CF3COO)3 were dissolved in 10 ml of oleylamine and stirred at 100 °C for 30 minutes to obtain LiYF4: 0.5% Tm 3+ ,20%Yb 3+ Precursor solution.
[0089] Comparative Example 1
[0090] This comparative example measures the LiYF4@LiYbF4@LiYF4:1%Tm prepared in Example 1. 3+ ,20%Yb 3+ @LiYbF4@LiYF4 structural upconversion nanoparticles and the commonly used LiYF4:1%Tm 3+ ,20%Yb 3+ Upconversion spectra of upconversion nanoparticles with @LiYbF4@LiYF4 structure, LiYF4:1%Tm 3+ ,20%Yb 3+ The preparation method of @LiYbF4@LiYF4 can be obtained by referring to the method in Example 1 of the present invention. From the spectrum, it can be seen that LiYF4@LiYbF4@LiYF4:1%Tm 3+ ,20%Yb 3+ @
[0091] The UV light of LiYbF4@LiYF4 nanostructure upconversion particles is better than that of LiYF4 commonly used in research: 1% Tm 3+ ,20%Yb 3+ @
[0092] The ultraviolet light intensity of upconversion nanoparticles with LiYbF4@LiYF4 core-shell composite structure is much higher.
[0093] The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field. The above description is only the embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. An upconversion nanoparticle having a core-shell structure, wherein the upconversion nanoparticle comprises, from the inside to the outside, a fluoride nanoparticle core which is completely transparent to ultraviolet to near-infrared light and does not absorb any rare earth ions, a near-infrared light absorption sensitized upconversion luminescent layer, and an isolation layer; The near-infrared light absorption sensitized up-conversion luminescent layer is mainly composed of a matrix material, sensitizing ions and activating ions; The fluoride nanoparticle core and the isolation layer have the same material composition; The material of the fluoride nanoparticle core is selected from one of LiYF4, LiLuF4, LiGdF4, NaYF4, NaLuF4, and NaGdF4. The material of the isolation layer is selected from one of LiYF4, LiLuF4, LiGdF4, NaYF4, NaLuF4, and NaGdF4; The particle core has a diameter of 15-18 nm; The near-infrared light absorption sensitization up-conversion luminescent layer includes, from the inside to the outside, an inner near-infrared light absorption sensitization layer, an up-conversion ultraviolet light emission layer and an outer near-infrared light absorption sensitization layer. The up-conversion ultraviolet light emitting layer is mainly composed of a matrix material, sensitizing ions and activating ions. The matrix material of the inner near-infrared light absorption sensitization layer and the matrix material of the outer near-infrared light absorption sensitization layer are both matrix materials with high absorption of near-infrared light. The material composition of the inner near-infrared light absorption sensitization layer and the outer near-infrared light absorption sensitization layer is the same; the matrix material of the inner near-infrared light absorption sensitization layer is selected from one of LiYbF4, NaYbF4, and KYbF4, and the matrix material of the outer near-infrared light absorption sensitization layer is selected from one of LiYbF4, NaYbF4, and KYbF4.
2. The upconversion nanoparticle according to claim 1, characterized in that: The matrix material of the up-conversion ultraviolet light emitting layer has the same material composition as that of the fluoride nanoparticle core.
3. The upconversion nanoparticle according to claim 2, characterized in that: The matrix material of the inner near-infrared light absorption sensitization layer is selected from one of LiYbF4 and NaYbF4, The matrix material of the outer near-infrared light absorption sensitization layer is selected from one of LiYbF4 and NaYbF4.
4. The upconversion nanoparticle according to claim 1, characterized in that: The sensitizing ions include Yb 3+ , the activating ion is selected from Er 3+ 、Tm 3+ 、Ho 3+ One of them.
5. The upconversion nanoparticle according to claim 4, characterized in that: The ion is Yb 3+ , the activating ion is Tm 3+ .
6. The upconversion nanoparticle according to claim 4, characterized in that: The material composition of the up-conversion ultraviolet light emitting layer includes one of the following components: LiYF4:0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、LiGdF4:0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、LiLuF4:0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、NaYF4:0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、NaGdF4:0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、NaLuF4:0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、KGdF4:0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、KYF4:0.5~1.5%Tm 3+ ,20~25%Yb 3+ 、KLuF4:0.5~1.5%Tm 3+ ,20~25%Yb 3+ 。 7. The upconversion nanoparticle according to claim 1, characterized in that: The diameter of the upconversion nanoparticles is 32-35 nm.
8. The method for preparing upconversion nanoparticles according to any one of claims 1 to 7, characterized in that: The near-infrared light absorption sensitization up-conversion luminescent layer material and the isolation layer material are sequentially coated on the fluoride nanoparticles which are not doped with any rare earth ions and fully transmit and do not absorb ultraviolet to near-infrared light.
9. The method for preparing upconversion nanoparticles according to claim 8, characterized in that: An inner near-infrared light absorption sensitization layer material, an up-conversion ultraviolet light emission layer material, an outer near-infrared light absorption sensitization layer material and an isolation layer material are sequentially coated on the outside of fluoride nanoparticles which are not doped with any rare earth ions and fully transmit and do not absorb ultraviolet to near-infrared light.
10. Use of the upconversion nanoparticles according to any one of claims 1 to 7 in the preparation of biological imaging displays and the preparation of drugs for treating cancer.