A porous crystalline tungsten oxide film and a method for preparing the porous crystalline tungsten oxide film by electrode electrospraying
The porous crystalline tungsten oxide film is prepared by electrode electrospraying, which solves the shortcomings of the tungsten oxide film in terms of cycle life and modulation ability, and realizes a high-performance and low-cost tungsten oxide electrochromic film, which is suitable for industrial production.
Patent Information
- Application Number
- CN202210634288.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-07
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-06-07
AI Technical Summary
Tungsten oxide electrochromic films have poor cycle life, poor modulation ability, and difficulty in industrial production. In particular, crystalline tungsten oxide films have insufficient modulation capabilities in the solar spectrum, and existing preparation methods are costly or difficult to prepare in large areas.
A porous crystalline tungsten oxide film is prepared by electrode electrospraying. Tungsten powder is reacted with hydrogen peroxide solution and carboxylic acid to generate tungsten precursor powder, which is dispersed in ethanol and then sprayed to form a film. The porosity and pore size are controlled through an annealing process. , improve the performance of the film.
It significantly improves the transmittance modulation ability, cycle stability and response time of the tungsten oxide electrochromic film, and achieves the preparation of high-performance and long-life tungsten oxide films, which is low-cost and suitable for industrial production.
Smart Images

Figure CN114959662B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrode preparation, and in particular relates to a porous tungsten oxide film and a preparation method thereof. Background Art
[0002] Electrochromic has the potential for large-scale application due to its advantage of actively adjusting color change. Tungsten oxide (WO3) is a typical electrochromic material. Under the action of an external electric field, the material undergoes a redox reaction, causing the absorption spectrum of the material to change reversibly. Electrochromic materials have been widely used. The main preparation methods include magnetron sputtering, vacuum evaporation, electrochemical deposition, hydrothermal / solvothermal method, sol-gel method, electrospraying method, etc.
[0003] However, tungsten oxide electrochromic materials have the following problems to be solved: 1. Amorphous tungsten oxide films have poor cycle life and generally fail after 2,000 cycles, which is far from commercial value. 2. Crystalline tungsten oxide films have poor adjustment ability. Due to the low content of defects in crystalline oxides, the color change process is difficult to inject, resulting in poor modulation ability in the solar spectrum band. 3. Industrial production is difficult. Preparation methods such as magnetron sputtering and vacuum evaporation have good film performance, but the instrument cost is high. Hydrothermal / solvothermal method, sol-gel method, and electrochemical deposition cannot be prepared on a large scale. Although the electrospraying method is low in cost, it is difficult to modify the film to ensure performance.
[0004] In summary, the mismatch between lifespan, performance and cost of tungsten oxide electrochromic film severely limits its industrialization potential. Therefore, there is an urgent need for a preparation method that can prepare high-life and high-performance tungsten oxide film at low cost. Summary of the invention
[0005] The purpose of the present invention is to solve the problem that the existing crystalline tungsten oxide film has poor adjustment ability and poor solar spectrum band modulation ability, and to provide a porous crystalline tungsten oxide film and a method for preparing the porous crystalline tungsten oxide film by electrode electrospraying.
[0006] A porous crystalline tungsten oxide film is prepared by using tungsten powder, a hydrogen peroxide solution with a mass fraction of 30% and a carboxylic acid to prepare a tungsten precursor powder, and then using ethanol as a dispersant and electrode electrospraying to prepare the porous crystalline tungsten oxide film. The porosity of the porous crystalline tungsten oxide film is 8% to 12%, and the diameter of the pores in the porous crystalline tungsten oxide film is 50nm to 100nm.
[0007] A method for preparing a porous crystalline tungsten oxide film by electrode electrospraying is specifically completed in the following steps:
[0008] 1. Preparation of tungsten precursor powder: ①, dissolving tungsten powder in a hydrogen peroxide solution with a mass fraction of 30% to obtain a tungsten-hydrogen peroxide solution; the concentration of tungsten element in the tungsten-hydrogen peroxide solution is 0.05mol / L to 0.5mol / L; ②, adding carboxylic acid to the tungsten-hydrogen peroxide solution and mixing to obtain a carboxylic acid-tungsten-hydrogen peroxide solution; the concentration of -COOH in the carboxylic acid-tungsten-hydrogen peroxide solution is 0.05mol / L to 0.5mol / L; ③, evaporating the carboxylic acid-tungsten-hydrogen peroxide solution at a temperature of 40 to 70°C to obtain a tungsten precursor powder;
[0009] 2. Electrode electrospraying: first disperse the tungsten precursor powder in an ethanol solvent to obtain a tungsten precursor-ethanol dispersion; the mass ratio of the tungsten precursor powder to the volume of ethanol is 20g:(10-50)mL, and the tungsten precursor-ethanol dispersion is sprayed on a clean substrate by electrode electrospraying, and then dried at a temperature of 60-80°C for 1h-2h, and finally annealed in an inert atmosphere to obtain a porous crystalline tungsten oxide film.
[0010] Advantages of the present invention:
[0011] 1. The present invention optimizes the electrospraying precursor powder, uses carboxylic acid as a ligand in the tungsten precursor powder, and combines it with an annealing process. During the annealing process, the carboxylic acid ligand is oxidized, which can inhibit the growth of grains and form pores. The pore size of the porous crystalline tungsten oxide film can also be controlled by using carboxylic acids of different sizes. Therefore, the present invention realizes the preparation of the porous crystalline tungsten oxide film, improves the performance of the tungsten oxide electrochromic film, and has significant advantages in transmittance modulation capability, cycle stability and coloring time compared with the crystalline film.
[0012] 2. The porous crystalline tungsten oxide film prepared by the present invention has obvious pseudocapacitive characteristics, which are reflected in the characteristics of polycrystalline films. Compared with crystalline films, the modulation performance and response time are significantly improved, and the transmittance change range reaches more than 40%. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 is the XRD pattern of the tungsten precursor powder obtained in step 1 of Example 1;
[0014] Figure 2 is the XRD pattern of the porous crystalline tungsten oxide film obtained in Example 1;
[0015] Figure 3 The transmission spectra of the porous crystalline tungsten oxide film obtained in Example 1 before and after the color change and the faded state are shown;
[0016] Figure 4is a CV curve diagram of the porous crystalline tungsten oxide thin film obtained in Example 1;
[0017] Figure 5 is a SEM image of the porous crystalline tungsten oxide film obtained in Example 1;
[0018] Figure 6 is a SEM image of the porous crystalline tungsten oxide film obtained in Example 2;
[0019] Figure 7 This is a SEM image of a crystalline tungsten oxide film;
[0020] Figure 8 This is a schematic diagram of the separation effect of carboxylic acid on PTA. DETAILED DESCRIPTION
[0021] Specific implementation method 1: This implementation method is a porous crystalline tungsten oxide film, which is made of tungsten powder, 30% by mass hydrogen peroxide solution and carboxylic acid to make a tungsten precursor powder, and then uses ethanol as a dispersant and electrode electrospraying to make a porous crystalline tungsten oxide film. The porosity of the porous crystalline tungsten oxide film is 8% to 12%, and the diameter of the pores in the porous crystalline tungsten oxide film is 50nm to 100nm.
[0022] Specific implementation method 2: This implementation method is a method for preparing a porous crystalline tungsten oxide film by electrode electrospraying, which is specifically completed in the following steps:
[0023] 1. Preparation of tungsten precursor powder: ①, dissolving tungsten powder in a hydrogen peroxide solution with a mass fraction of 30% to obtain a tungsten-hydrogen peroxide solution; the concentration of tungsten element in the tungsten-hydrogen peroxide solution is 0.05mol / L to 0.5mol / L; ②, adding carboxylic acid to the tungsten-hydrogen peroxide solution and mixing to obtain a carboxylic acid-tungsten-hydrogen peroxide solution; the concentration of -COOH in the carboxylic acid-tungsten-hydrogen peroxide solution is 0.05mol / L to 0.5mol / L; ③, evaporating the carboxylic acid-tungsten-hydrogen peroxide solution at a temperature of 40 to 70°C to obtain a tungsten precursor powder;
[0024] 2. Electrode electrospraying: first disperse the tungsten precursor powder in an ethanol solvent to obtain a tungsten precursor-ethanol dispersion; the mass ratio of the tungsten precursor powder to the volume of ethanol is 20g:(10-50)mL, and the tungsten precursor-ethanol dispersion is sprayed on a clean substrate by electrode electrospraying, and then dried at a temperature of 60-80°C for 1h-2h, and finally annealed in an inert atmosphere to obtain a porous crystalline tungsten oxide film.
[0025] Specific embodiment 3: This embodiment differs from specific embodiment 2 in that the carboxylic acid in step 1 is one or more of formic acid, acetic acid, oxalic acid and citric acid. The rest is the same as specific embodiment 2.
[0026] Specific embodiment 4: This embodiment differs from specific embodiment 2 or 3 in that the clean substrate in step 2 is obtained by the following operation: the substrate is firstly acid-washed, then sequentially cleaned with ethanol and deionized water, and dried to obtain a clean substrate. The rest is the same as specific embodiment 2 or 3.
[0027] Specific embodiment 5: This embodiment differs from specific embodiment 4 in that the substrate is ITO glass, FTO glass, AZO glass or PET-ITO transparent conductive film. Other aspects are the same as those of specific embodiment 4.
[0028] Specific embodiment 6: This embodiment differs from specific embodiment 4 or 5 in that the substrate is first ultrasonically cleaned with 1 mol / L sulfuric acid solution for 20 minutes, then ultrasonically cleaned with ethanol for 20 minutes, and finally ultrasonically cleaned with deionized water for 20 minutes, and dried to obtain a clean substrate. The rest is the same as specific embodiment 4 or 5.
[0029] Specific embodiment 7: This embodiment differs from specific embodiments 2 to 6 in that the voltage of the electrode electrospraying method in step 2 is 17 kV, and the distance between the spray head and the clean substrate is 15 cm. Other aspects are the same as specific embodiments 2 to 6.
[0030] Specific embodiment 8: This embodiment differs from specific embodiments 2 to 7 in that the inert atmosphere gas in step 2 is argon or nitrogen. The rest is the same as specific embodiments 2 to 6.
[0031] Specific embodiment 9: This embodiment differs from specific embodiments 2 to 8 in that the annealing parameters in step 2 are: the annealing temperature is 400° C. to 600° C., and the annealing time is 10 min to 120 min. The rest is the same as specific embodiments 2 to 8.
[0032] Specific embodiment 10: This embodiment differs from specific embodiments 2 to 9 in that in step 2, the temperature is raised to the annealing temperature at a heating rate of 5°C / min, and then annealed in an inert atmosphere. The rest is the same as specific embodiments 2 to 9.
[0033] The content of the present invention is not limited to the content of the above-mentioned embodiments. The combination of one or several specific embodiments can also achieve the purpose of the invention.
[0034] The following test is used to verify the effect of the present invention:
[0035] Example 1: A method for preparing a porous crystalline tungsten oxide film by electrode electrospraying, which is specifically completed by the following steps:
[0036] 1. Preparation of tungsten precursor powder: ①. Dissolve 1.8 g of tungsten powder in 20 mL of 30% hydrogen peroxide solution to obtain a tungsten-hydrogen peroxide solution; ②. Add 2.2 g of oxalic acid to the tungsten-hydrogen peroxide solution and mix well to obtain a carboxylic acid-tungsten-hydrogen peroxide solution; ③. Evaporate the carboxylic acid-tungsten-hydrogen peroxide solution at 60°C to dryness to obtain a tungsten precursor powder;
[0037] 2. Electrode electrospraying: first disperse 20g of tungsten precursor powder in 20mL of ethanol solvent to obtain a tungsten precursor-ethanol dispersion; spray the tungsten precursor-ethanol dispersion on a clean substrate by electrode electrospraying, then dry at 80°C for 2h, and finally anneal at 450°C for 60min in a nitrogen atmosphere to obtain a porous crystalline tungsten oxide film; the porosity of the porous crystalline tungsten oxide film is 9.8%, and the average diameter of the pores in the porous crystalline tungsten oxide film is about 51nm.
[0038] The clean substrate described in step 2 of Example 1 is obtained by the following operation: the substrate is first ultrasonically cleaned with a 1 mol / L sulfuric acid solution for 20 min, then ultrasonically cleaned with ethanol for 20 min, and finally ultrasonically cleaned with deionized water for 20 min, and dried to obtain a clean substrate; the substrate is ITO glass.
[0039] The voltage of the electrode electrospraying method in step 2 of Example 1 is 17 kV, and the distance between the nozzle and the clean substrate is 15 cm.
[0040] The tungsten precursor powder obtained in step 1 of Example 1 and the porous crystalline tungsten oxide film obtained in Example 1 were characterized by XRD. Figure 1 and Figure 2 As shown, Figure 1 is the XRD pattern of the tungsten precursor powder obtained in step 1 of Example 1, Figure 2 is the XRD pattern of the porous crystalline tungsten oxide film obtained in Example 1. Figure 2 and Figure 1 By comparison, it can be seen that the prepared precursor powder is a composite product of WO3 and oxalic acid.
[0041] Electrochemical cyclic voltammetric characteristics and spectral analysis: The transmittance spectra of the porous crystalline tungsten oxide film obtained in Example 1 in the colored state and the bleached state were detected. Figure 3 As shown, Figure 31 is a transmission spectrum of the porous crystalline tungsten oxide film obtained in Example 1 before and after color change and in a faded state; the CV curve of the porous crystalline tungsten oxide film obtained in Example 1 is detected in a 0.1 mol / L lithium sulfate aqueous solution, as shown in FIG. Figure 4 As shown, Figure 4 is the CV curve of the porous crystalline tungsten oxide film obtained in Example 1; Figure 3 From the above, we can see that there are relatively certain capacitance charge and discharge characteristics, which indicates that the surface pores play a significant adsorption role. Figure 4 From the above, the modulation ability of the transmitted spectrum in the near-infrared region has been significantly improved, which is very beneficial to the entire injection process. It can not only effectively enhance the near-infrared modulation ability, but also improve the response rate, and to a certain extent realize the combination of the advantages of amorphous and crystalline states; therefore, through Figure 3 From the perspective of the film, it can be seen that the film has obvious pseudocapacitive characteristics. Figure 4 From the perspective of colorization, the modulation of the colored state and the faded state at the near-infrared 950nm is about 50%, and the response time is about 20s, which reflects the characteristics of the polycrystalline film. Compared with the crystalline film, the modulation performance and response time have been significantly improved.
[0042] Example 2: A method for preparing a porous crystalline tungsten oxide film by electrode electrospraying, which is specifically completed by the following steps:
[0043] 1. Prepare tungsten precursor powder: ①. Dissolve 1.8g of tungsten powder in 20mL of 30% hydrogen peroxide solution to obtain a tungsten-hydrogen peroxide solution; ②. Add 2.2g of citric acid to the tungsten-hydrogen peroxide solution and mix well to obtain a carboxylic acid-tungsten-hydrogen peroxide solution; ③. Evaporate the carboxylic acid-tungsten-hydrogen peroxide solution at 60°C to obtain a tungsten precursor powder;
[0044] 2. Electrode electrospraying: first disperse 20 g of tungsten precursor powder in 20 mL of ethanol solvent to obtain a tungsten precursor-ethanol dispersion; spray the tungsten precursor-ethanol dispersion on a clean substrate by electrode electrospraying, then dry at 80°C for 2 hours, and finally anneal at 450°C for 60 minutes in a nitrogen atmosphere to obtain a porous crystalline tungsten oxide film; the porosity of the porous crystalline tungsten oxide film is 10.6%, and the average diameter of the pores in the porous crystalline tungsten oxide film is about 93 nm.
[0045] The clean substrate described in step 2 of Example 2 is obtained by the following operation: the substrate is first ultrasonically cleaned with a 1 mol / L sulfuric acid solution for 20 min, then ultrasonically cleaned with ethanol for 20 min, and finally ultrasonically cleaned with deionized water for 20 min, and dried to obtain a clean substrate; the substrate is ITO glass.
[0046] The voltage of the electrode electrospraying method in step 2 of Example 2 is 17 kV, and the distance between the nozzle and the clean substrate is 15 cm.
[0047] The surface morphologies of the porous crystalline tungsten oxide film obtained in Example 1, the porous crystalline tungsten oxide film obtained in Example 2, and the existing crystalline tungsten oxide film were characterized by SEM. Figure 5 , Figure 6 and Figure 7 As shown, Figure 5 is a SEM image of the porous crystalline tungsten oxide film obtained in Example 1. Figure 6 is a SEM image of the porous crystalline tungsten oxide film obtained in Example 2. Figure 7 This is a SEM image of a crystalline tungsten oxide film; Figure 5 and Figure 6 It can be seen that the surface grain size is only about tens of nanometers, and there are many tiny pores between the grains. The larger volume occupied by the citrate ions effectively separates the ion complex and increases the diffusion distance, so that the grain growth is most obviously inhibited during the annealing process. Figure 5 and Figure 6 and Figure 7 By comparison, the film deposited by pure PTA (polyperoxytungstic acid) has the lowest porosity, which is only composed of large clusters and is very large in size. However, due to the strong bonding between the tightly packed clusters, there is no stratification and pores between the clusters, which is not conducive to the injection of ions. At the same time, the specific surface area is much smaller than that of the film with carboxylic acid. In the film with carboxylic acid, the porosity increases due to stratification, which is largely due to the separation effect of the conjugate base. This separation effect on PTA containing oxalic acid is less than that on PTA containing citric acid. PTA contains citric acid, and the separation between individual particles is the largest, so the porosity is the largest.
[0048] Figure 8 This is a schematic diagram of the separation effect of carboxylic acid on PTA. Figure 8 It can be seen that during the annealing process, the carboxylic acid ligands wrapped around the outside of the dissolved PTA ions were oxidized during the annealing process, inhibiting the growth of grains and forming pores. At the same time, the pore size of the film can be further controlled by using carboxylic acids of different sizes.
Claims
1. A method for preparing a porous crystalline tungsten oxide film by electrode electrospraying, characterized in that The porous crystalline tungsten oxide film is made of tungsten powder, 30% by mass hydrogen peroxide solution and carboxylic acid to prepare tungsten precursor powder, and then ethanol is used as a dispersant and electrode electrospraying is used to prepare the porous crystalline tungsten oxide film. The porosity of the porous crystalline tungsten oxide film is 8% to 12%, and the diameter of the pores in the porous crystalline tungsten oxide film is 50nm to 100nm. The preparation of the porous crystalline tungsten oxide film is completed according to the following steps:
1. Prepare tungsten precursor powder: ①, dissolve tungsten powder in a hydrogen peroxide solution with a mass fraction of 30% to obtain a tungsten-hydrogen peroxide solution; the concentration of tungsten element in the tungsten-hydrogen peroxide solution is 0.05mol / L~0.5mol / L; ②, add carboxylic acid to the tungsten-hydrogen peroxide solution, mix well to obtain a carboxylic acid-tungsten-hydrogen peroxide solution; The concentration of -COOH in the carboxylic acid-tungsten-hydrogen peroxide solution is 0.05 mol / L to 0.5 mol / L; ③, evaporating the carboxylic acid-tungsten-hydrogen peroxide solution at a temperature of 40 to 70° C. to obtain a tungsten precursor powder; The carboxylic acid is one or more of formic acid, acetic acid, oxalic acid and citric acid; 2. Electrode electrospraying: first disperse the tungsten precursor powder in an ethanol solvent to obtain a tungsten precursor-ethanol dispersion; the mass ratio of the tungsten precursor powder to the volume of ethanol is 20g:(10~50)mL, and the tungsten precursor-ethanol dispersion is sprayed on a clean substrate by electrode electrospraying, and then dried at a temperature of 60~80℃ for 1h~2h, and finally annealed in an inert atmosphere to obtain a porous crystalline tungsten oxide film; The voltage of the electrode electrospraying method is 17 kV, and the distance between the nozzle and the clean substrate is 15 cm; The gas of the inert atmosphere is argon or nitrogen; The annealing parameters are as follows: the annealing temperature is 400°C to 600°C, and the annealing time is 10min to 120min; The temperature was raised to the annealing temperature at a heating rate of 5°C / min, and then annealed in an inert atmosphere.
2. The method for preparing a porous crystalline tungsten oxide thin film by electrode electrospraying according to claim 1, characterized in that The clean substrate in step 2 is obtained by the following operations: the substrate is firstly acid-washed, then cleaned with ethanol and deionized water in sequence, and dried to obtain a clean substrate.
3. The method for preparing a porous crystalline tungsten oxide thin film by electrode electrospraying according to claim 2, characterized in that The substrate is ITO glass, FTO glass, AZO glass or PET-ITO transparent conductive film.
4. The method for preparing a porous crystalline tungsten oxide thin film by electrode electrospraying according to claim 3, characterized in that The substrate was first ultrasonically cleaned with a 1 mol / L sulfuric acid solution for 20 min, then ultrasonically cleaned with ethanol for 20 min, and finally ultrasonically cleaned with deionized water for 20 min, and dried to obtain a clean substrate.
Citation Information
Patent Citations
Preparing method of porous tungsten oxide film
CN101660124A
Method for preparing large-area porous electrochromic film through spray process
CN105859151A
Preparation method of tungsten-oxide electrochromic electrode
CN108663868A
Great-modulation capability crystalline tungsten trioxide electrochromic film and preparation method thereof
CN108863101A
Preparation method of gasochromic film
CN113200683A