Solar cell electrode and method for forming the same

By using a combination of conductive powder and specific glass frit in the solar cell electrode to control the interface reaction, the problems of recombination loss and insufficient adhesion caused by etching the anti-reflective layer are solved, and the open circuit voltage and efficiency of the solar cell are improved. and enhanced adhesion to wafers or bonding wires.

CN114974649BActive Publication Date: 2024-10-11CHANGZHOU JUHE NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110211709.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-10-11
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

The recombination loss caused by the etched anti-reflective coating produced during the electrode firing process of solar cells reduces the open circuit voltage characteristics and efficiency. At the same time, the adhesion to the wafer or bonding wire is insufficient, affecting reliability.

Method used

Using solar cell electrode structures containing conductive powders and different types of glass frits, the recombination loss of etched anti-reflective layers is reduced and adhesion is improved by controlling interfacial reactions during the electrode firing process. The specific method includes using conductive powder and glass frit with a molar ratio of lead oxide to copper oxide between 0.2 and 0.95 in the first electrode layer and the second electrode layer, combined with other element oxides to form an efficient electrode layer .

Benefits of technology

It effectively improves the open circuit voltage characteristics and conversion efficiency of solar cells, improves adhesion to wafers or bonding wires, and improves the overall performance and reliability of solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114974649B_ABST
    Figure CN114974649B_ABST
Patent Text Reader

Abstract

The present invention discloses a solar cell electrode and a preparation method thereof. The solar cell electrode comprises: a first electrode layer, comprising conductive powder and a first glass frit; and a second electrode layer, formed on the first electrode layer, comprising conductive powder and a second glass frit which is different from the first glass frit and has a molar ratio of lead (Pb) oxide / (lead (Pb) oxide+copper (Cu) oxide) greater than 0.2 and less than 0.95.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solar cell electrode and a method for forming the same, and more particularly to a solar cell electrode and a method for forming the same which improves the open circuit voltage characteristics, thereby improving the efficiency of the solar cell and enhancing the adhesion to the wafer or the bonding wire. Background Art

[0002] Solar cells generate electricity by using the photoelectric effect of pn junction, which converts photons of sunlight into electricity. In solar cells, the front electrode and the back electrode are formed on the upper and lower surfaces of the semiconductor wafer or substrate that constitutes the pn junction. Solar cells induce the photoelectric effect of the pn junction by sunlight incident on the semiconductor wafer, and the electrons generated thereby provide current flowing to the outside through the electrodes.

[0003] The electrode of this solar cell can be formed on the surface of the substrate in a predetermined pattern by coating, patterning and firing the electrode forming composition. In order to prepare a high-efficiency solar cell, it is necessary to reduce the factors that reduce the efficiency of the solar cell. The efficiency loss of the solar cell can be roughly divided into optical loss, electron-hole recombination loss, and loss caused by resistance components. Summary of the invention

[0004] An object of the present invention is to provide a solar cell electrode having improved open circuit voltage characteristics by reducing recombination loss caused by etching of an anti-reflective coating (ARC) during electrode firing.

[0005] Another object of the present invention is to provide a solar cell electrode having excellent conversion efficiency.

[0006] Another object of the present invention is to provide a solar cell electrode that has improved adhesion to a wafer or a bonding wire to improve reliability.

[0007] Another object of the present invention is to provide a method for forming the above-mentioned solar cell electrode.

[0008] 1. According to one embodiment, a solar cell electrode is provided. The solar cell electrode may include: a first electrode layer, comprising a conductive powder and a first glass frit; and a second electrode layer, formed on the first electrode layer, comprising a conductive powder and a second glass frit different from the first glass frit and having a molar ratio of lead (Pb) oxide / (lead (Pb) oxide + copper (Cu) oxide) greater than 0.2 and less than 0.95.

[0009] 2. In the above 1, the second glass frit may contain 15 to 75 mol % of lead (Pb) oxide.

[0010] 3. In the above 1 or 2, the second glass frit may contain 3 to 60 mol % of copper (Cu) oxide.

[0011] 4. In any one of 1 to 3 above, the second glass frit may further include one or more elements selected from the group consisting of tellurium (Te), bismuth (Bi), lithium (Li), boron (B), phosphorus (P), germanium (Ge), gallium (Ga), cerium (Ce), iron (Fe), silicon (Si), zinc (Zn), tungsten (W), magnesium (Mg), cesium (Cs), strontium (Sr), molybdenum (Mo), titanium (Ti), tin (Sn), indium (In), vanadium (V), barium (Ba), nickel (Ni), sodium (Na), potassium (K), arsenic (As), cobalt (Co), zirconium (Zr), manganese (Mn) and aluminum (Al).

[0012] 5. In any one of 1 to 4 above, the second glass frit may further include one or more of silicon (Si) oxide, titanium (Ti) oxide, and iron (Fe) oxide.

[0013] 6. In any one of 1 to 5 above, the second glass frit may further contain 5 to 25 mol % of silicon (Si) oxide.

[0014] 7. In any one of 1 to 6 above, the second glass frit may further include 0.3 to 15 mol % of titanium (Ti) oxide.

[0015] 8. In any one of 1 to 7 above, the second glass frit may further contain 1 to 5 mol % of iron (Fe) oxide.

[0016] 9. In any one of 1 to 8 above, the second glass frit may further include one or more of boron (B) oxide, sodium (Na) oxide, aluminum (Al) oxide, tungsten (W) oxide, and molybdenum (Mo) oxide.

[0017] 10. According to another embodiment, a method for forming a solar cell electrode according to any one of 1 to 9 above is provided. The method may include: applying a first solar cell electrode-forming composition comprising a conductive powder, a first glass frit, and an organic vehicle to form a first electrode layer, applying a second solar cell electrode-forming composition comprising a conductive powder, a second glass frit, and an organic vehicle to form a second electrode layer, and a firing step.

[0018] 11. In the above 10, the above-mentioned first solar cell electrode forming composition or the above-mentioned second solar cell electrode forming composition may also contain one or more of a dispersant, a thixotropic agent, a plasticizer, a viscosity stabilizer, a defoaming agent, a pigment, a UV stabilizer, an antioxidant and a coupling agent.

[0019] 12. In the above 10 or 11, the first solar cell electrode forming composition may include 60 to 95 weight percent of the conductive powder, 0.1 to 20 weight percent of the first glass frit and 1 to 30 weight percent of the organic carrier, and the second solar cell electrode forming composition may include 60 to 95 weight percent of the conductive powder, 0.1 to 20 weight percent of the second glass frit and 1 to 30 weight percent of the organic carrier.

[0020] The present invention has the effect of providing a solar cell electrode and a method for forming the same, which improves the open circuit voltage characteristics by controlling the interface reaction generated during the electrode firing process, has excellent conversion efficiency, and has improved adhesion. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The structure of a solar cell according to an example of the present invention is briefly shown. DETAILED DESCRIPTION

[0022] In the present specification, singular expressions include plural expressions unless there is a clear difference in context.

[0023] The terms including or having in the present specification mean the existence of the features or structural elements described in the specification, and do not preclude the possibility of adding one or more other features or structural elements.

[0024] The terms "first", "second", etc. used in this specification may be used to describe various structural elements, but the structural elements are not limited to the terms. The terms are used only to distinguish one structural element from other structural elements.

[0025] When interpreting structural elements, they are interpreted as including the range of errors even if there is no additional explicit description.

[0026] In the present specification, “to” in “a to b” indicating a numerical range is defined as ≥a and ≤b.

[0027] Solar cell electrodes

[0028] According to one embodiment, a solar cell electrode is provided. The solar cell electrode may include: a first electrode layer, including a conductive powder and a first glass frit; and a second electrode layer, formed on the first electrode layer, including a conductive powder and a second glass frit different from the first glass frit and having a molar ratio of lead (Pb) oxide / (lead (Pb) oxide+copper (Cu) oxide) greater than 0.2 and less than 0.95.

[0029] The conductive powder may include, for example, one or more metal powders of silver (Ag), gold (Au), platinum (Pt), palladium (Pd), aluminum (Al) and nickel (Ni), but is not limited thereto. According to one example, the conductive powder may include silver powder.

[0030] The particle shape of the conductive powder is not particularly limited, and particles of various shapes can be used, for example, particles of spherical, plate-like or amorphous shapes can be used.

[0031] The conductive powder may be a powder having a nanometer or micrometer particle size, for example, a conductive powder having a size of tens or hundreds of nanometers or a conductive powder having a size of several to tens of micrometers. Furthermore, two or more conductive powders of different sizes may be mixed and used as the conductive powder.

[0032] The average particle size of the conductive powder (D 50 ) can be 0.1 to 10 μm, for example, 0.5 to 5 μm. Within the above range, the contact resistance and the series resistance are likely to be reduced. The average particle size (D) can be measured using the 1064LD model produced by CI LAS after ultrasonic dispersion of the conductive powder in isopropyl alcohol (IPA) for 3 minutes at 25°C. 50 ).

[0033] The glass frit is used to etch the anti-reflection film in the firing process of the electrode-forming composition, melt the conductive powder and generate crystalline particles of the conductive powder in the emitter region. In addition, the glass frit improves the bonding strength between the conductive powder and the wafer, and is softened during sintering to induce the effect of further lowering the firing temperature.

[0034] The first glass frit included in the first electrode layer and the second glass frit included in the second electrode layer may be different. For example, the first glass frit and the second glass frit may contain different types of elements or different contents of elements.

[0035] The first glass frit may generally be a glass frit used in the preparation of solar cell electrodes. For example, the first glass frit may include one or more elements selected from the group consisting of lead (Pb), tellurium (Te), bismuth (Bi), lithium (Li), boron (B), phosphorus (P), germanium (Ge), gallium (Ga), cerium (Ce), iron (Fe), silicon (Si), zinc (Zn), tungsten (W), magnesium (Mg), cesium (Cs), strontium (Sr), molybdenum (Mo), titanium (Ti), tin (Sn), indium (In), vanadium (V), barium (Ba), nickel (Ni), copper (Cu), sodium (Na), potassium (K), arsenic (As), cobalt (Co), zirconium (Zr), manganese (Mn), and aluminum (Al).

[0036] According to one example, the first glass frit may include one or more of Bi-Te-O glass frit, Pb-Bi-O glass frit, Pb-Te-O glass frit, Pb-Te-Bi-O glass frit, Te-BO glass frit, Te-Ag-O glass frit, Pb-Si-O glass frit, Bi-Si-O glass frit, Te-Zn-O glass frit, Bi-Te-Li-Zn-O glass frit, Pb-Te-Si-Na-WO glass frit, Bi-BO glass frit, Pb-BO glass frit, Bi-MoO glass frit, Mo-BO glass frit, and Te-Si-O glass frit. In this case, there may be an advantage of excellent balance of electrical characteristics of the solar cell electrode.

[0037] The second glass frit is different from the first glass frit and contains lead (Pb) oxide and copper (Cu) oxide, and the molar ratio of lead (Pb) oxide / (lead (Pb) oxide+copper (Cu) oxide) can be greater than 0.2 and less than 0.95. In this case, the open circuit voltage characteristics and solar cell efficiency are improved by reducing the recombination loss caused by etching the ARC layer during the electrode firing process, and the adhesion to the wafer-gate line interface or the gate line-welding line interface can also be excellent. According to one example, in the second glass frit, the molar ratio of lead (Pb) oxide / (lead (Pb) oxide+copper (Cu) oxide) can be 0.23 to 0.93, according to another example, it can be 0.23 to 0.87, according to another example, it can be 0.23 to 0.80, but it is not limited thereto.

[0038] According to one example, lead (Pb) oxide may contain 15 to 75 mole percent (for example, 17 to 75 mole percent, and as another example, 17 to 70 mole percent) based on the total molar amount of the second glass frit. Within the above range, the open circuit voltage characteristics and solar cell efficiency are improved by reducing the recombination loss caused by etching the ARC layer during the electrode firing process, and the adhesion to the wafer-gate line interface or the gate line-bonding wire interface can also be excellent, but it is not limited to this.

[0039] According to one example, copper (Cu) oxide may contain 3 to 60 mole percent (for example, 5 to 60 mole percent, and as another example, 5 to 58 mole percent) based on the total molar amount of the second glass frit. Within the above range, the open circuit voltage characteristics and solar cell efficiency are improved by reducing the recombination loss caused by etching the ARC layer during the electrode firing process, and the adhesion to the wafer-gate line interface or the gate line-bonding line interface may also be excellent, but it is not limited to this.

[0040] The second glass frit may contain, in addition to lead (Pb) and copper (Cu) elements, one or more elements selected from, for example, tellurium (Te), bismuth (Bi), lithium (Li), boron (B), phosphorus (P), germanium (Ge), gallium (Ga), cerium (Ce), iron (Fe), silicon (Si), zinc (Zn), tungsten (W), magnesium (Mg), cesium (Cs), strontium (Sr), molybdenum (Mo), titanium (Ti), tin (Sn), indium (In), vanadium (V), barium (Ba), nickel (Ni), sodium (Na), potassium (K), arsenic (As), cobalt (Co), zirconium (Zr), manganese (Mn) and aluminum (Al).

[0041] According to one example, the second glass frit may further include silicon (Si) oxide. In this case, it may have an adhesion improvement effect. The silicon (Si) oxide may include, for example, 5 to 25 mole percent based on the total molar amount of the second glass frit, 5 to 20 mole percent as another example, and 6 to 15 mole percent as another example. Within the above range, the adhesion improvement effect may be further improved, but is not limited thereto.

[0042] According to another example, the second glass frit may further include titanium (Ti) oxide. In this case, it may have an adhesion improvement effect. The titanium (Ti) oxide may include, for example, 0.3 to 13 mole percent based on the total molar amount of the second glass frit, 0.3 to 11 mole percent as another example, and 0.3 to 10 mole percent as another example. Within the above range, the adhesion improvement effect may be further excellent, but it is not limited thereto.

[0043] According to another example, the second glass frit may further include iron (Fe) oxide. In this case, it may have an adhesion improvement effect. The iron (Fe) oxide may include, for example, 1 to 5 mole percent based on the total molar amount of the second glass frit, and may include 1.2 to 4 mole percent as another example, and may include 1.2 to 3.6 mole percent as another example. Within the above range, the adhesion improvement effect may be further improved, but is not limited thereto.

[0044] According to another example, the second glass frit may further include boron (B) oxide. In this case, it is easy to prepare glass and can have an adhesion improvement effect. Boron (B) oxide may include, for example, 0.1 to 20 mole percent based on the total molar amount of the second glass frit. As another example, it may include 0.1 to 15 mole percent. Within the above range, it is easy to prepare glass and can have an adhesion improvement effect, but it is not limited thereto.

[0045] According to another example, the second glass frit may further include sodium (Na) oxide. In this case, it may have a resistance improvement effect. The sodium (Na) oxide may include, for example, 1 to 8 mole percent based on the total molar amount of the second glass frit, and may include 1.5 to 6 mole percent as another example, and may include 1.5 to 5 mole percent as another example. Within the above range, it may have a resistance improvement effect, but is not limited thereto.

[0046] According to another example, the second glass frit may further include aluminum (Al) oxide. In this case, it may have an adhesion improvement effect. The aluminum (Al) oxide may include, for example, 0.1 to 2 mole percent based on the total molar amount of the second glass frit. Within the above range, it may have an adhesion improvement effect, but is not limited thereto.

[0047] According to another example, the second glass frit may further include tungsten (W) oxide. In this case, it may have an adhesion improvement effect. The tungsten (W) oxide may include, for example, 0.1 to 5 mole percent based on the total molar amount of the second glass frit, and may include 0.1 to 3.5 mole percent as another example, and may include 0.1 to 3 mole percent as another example. Within the above range, it may have an adhesion improvement effect, but is not limited thereto.

[0048] According to another example, the second glass frit may further include molybdenum (Mo) oxide. In this case, it may have an open circuit voltage improvement effect. The molybdenum (Mo) oxide may include, for example, 0.1 to 5 mole percent based on the total molar amount of the second glass frit. Within the above range, it may have an open circuit voltage improvement effect, but it is not limited thereto.

[0049] According to another example, the second glass frit may not contain tellurium (Te) element. In this case, it may have a resistance improvement effect.

[0050] The shape and size of the glass frit are not particularly limited. For example, the shape of the glass frit can be spherical or amorphous, and the average particle size (D 50 ) can be 0.1 to 10 μm. After ultrasonic dispersion of the glass frit in isopropanol at 25°C for 3 minutes, the average particle size (D 50 ).

[0051] Glass frit can be prepared from the above elements and / or element oxides by conventional methods, for example, by mixing the above elements and / or element oxides using a ball mill or a planetary mill, melting the mixed composition at 800° C. to 1300° C., quenching at 25° C., and then crushing the resultant by a disk mill or a planetary mill.

[0052] Method for forming solar cell electrode

[0053] According to another embodiment, a method for forming the above-mentioned solar cell electrode is provided. The method for forming the solar cell electrode may include: applying a first solar cell electrode-forming composition comprising a conductive powder, a first glass frit, and an organic carrier to form a first electrode layer, applying a second solar cell electrode-forming composition comprising a conductive powder, a second glass frit, and an organic carrier to form a second electrode layer, and a firing step.

[0054] The first solar cell electrode forming composition can be prepared by mixing a conductive powder, a first glass frit, and an organic vehicle, and the second solar cell electrode forming composition can be prepared by mixing a conductive powder, a second glass frit, and an organic vehicle. Since the conductive powder, the first glass frit, and the second glass frit have been described in detail, the specific description is omitted.

[0055] The amount of the conductive powder used is not particularly limited, for example, the conductive powder may be included in an amount of 60 to 95 weight percent, for example, 70 to 90 weight percent, relative to the total weight of the first or second solar cell electrode forming composition. Within the above range, the conversion efficiency of the solar cell is excellent and the paste can be smoothly performed.

[0056] The amount of glass frit used is not particularly limited, for example, relative to the total weight of the first or second solar cell electrode forming composition, the glass frit may be included in an amount of 0.1 to 20 weight percent, for example, 0.1 to 10 weight percent. Within the above range, the solar cell efficiency can be improved through excellent open circuit voltage, and the adhesion can be improved.

[0057] The composition for forming a solar cell electrode may include an organic vehicle that is mechanically mixed with an inorganic component of the composition to impart viscosity and rheological properties suitable for printing to the composition. The organic vehicle may generally be an organic vehicle used in the composition for forming a solar cell electrode, and may include a binder resin and a solvent, etc.

[0058] As the binder resin, an acrylic resin or a cellulose resin can be used. According to one example, ethyl cellulose can be used as the binder resin. According to another example, as the binder resin, ethyl hydroxyethyl cellulose, nitrocellulose, a mixture of ethyl cellulose and a phenolic resin, an alkyd resin, a phenolic resin, an acrylic resin, a xylene resin, a polybutylene resin, a polyester resin, a urea resin, a melamine resin, a vinyl acetate resin, a wood rosin, or polymethyl acrylate of ethanol can be used.

[0059] As the solvent, for example, hexane, toluene, ethyl cellosolve, cyclohexanone, butyl cellosolve, butyl carbitol (diethylene glycol monobutyl ether), dibutyl carbitol (diethylene glycol dibutyl ether), butyl carbitol acetate (diethylene glycol monobutyl ether acetate), propylene glycol monomethyl ether, hexylene glycol, terpineol, methyl ethyl ketone, benzyl alcohol, γ-butyrolactone, ethyl lactate or 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (for example, ester alcohol) can be used alone or in combination.

[0060] The amount of the organic vehicle used is not particularly limited, for example, the organic vehicle may be included in an amount of 1 to 30 weight percent, for example, 3 to 25 weight percent, relative to the total weight of the first or second solar cell electrode forming composition. Within the above range, sufficient bonding strength and excellent printability can be ensured.

[0061] In order to improve the flow characteristics, process characteristics and stability, the composition for forming a solar cell electrode may contain, in addition to the above-mentioned components, a dispersant, a thixotropic agent, a plasticizer, a viscosity stabilizer, a defoaming agent, a pigment, a UV stabilizer, an antioxidant, a coupling agent, etc., alone or in combination. These components may be contained in an amount of 0.1 to 5 weight percent relative to the total weight of the first or second composition for forming a solar cell electrode, but their content may be changed as needed.

[0062] A method for forming a solar cell electrode may include, for example: a step of applying a first solar cell electrode forming composition on a substrate surface in a prescribed pattern, followed by drying to form a first electrode layer; a step of applying a second solar cell electrode forming composition on the substrate having the first electrode layer formed thereon, followed by drying to form a second electrode layer; and a step of firing the electrode pattern formed by the first and second solar cell electrode forming compositions.

[0063] The solar cell electrode forming composition can be applied by, for example, screen printing, gravure offset printing, rotary screen printing, lift-off method or the like, but is not limited thereto.

[0064] The solar cell electrode forming composition may be dried at, for example, about 200° C. to about 400° C. for about 10 seconds to about 60 seconds, but the present invention is not limited thereto.

[0065] For example, the firing process may be performed at about 400 to about 980° C. (eg, about 600 to about 950° C.) for about 60 to about 210 seconds, but is not limited thereto.

[0066] Solar Cells

[0067] According to another embodiment, a solar cell including the above-mentioned solar cell electrode is provided.

[0068] Figure 1 The structure of a solar cell 100 according to an example of the present invention is briefly shown.

[0069] Reference Figure 1 , the solar cell 100 may include: a substrate 10 including a p-layer (or n-layer) 11 and an n-layer (or p-layer) 12 as an emitter; a rear electrode 21 and a front electrode 23. The rear electrode 21 or the front electrode 23 may include a first electrode layer formed on the substrate 10 and a second electrode layer formed on the first electrode layer, the first electrode layer may include a conductive powder and a first glass frit, and the second electrode layer may include a conductive powder and a second glass frit.

[0070] The solar cell 100, for example, prints a first solar cell electrode forming composition on the front of the substrate 10, dries it to form a first electrode layer, prints a second solar cell electrode forming composition, dries it to form a second electrode layer, performs a preliminary preparation step for the front electrode 23, prints aluminum paste on the back of the substrate 10, dries it, performs a preliminary preparation step for the back electrode 21, and then can be fired for preparation.

[0071] The present invention will be described in further detail below with reference to the following examples, but these are provided as preferred examples of the present invention and should not be construed as limiting the present invention to these examples.

[0072] Example

[0073] Preparation Example 1

[0074] At 60°C, 2 parts by weight of ethyl cellulose (STD4, Dow Chemical) as a binder resin was fully dissolved in 6.5 parts by weight of terpene alcohol (Nippon Terpine) as a solvent, and 90 parts by weight of spherical silver powder (4-8F, Dowa) with an average particle size of 2.0 μm and 1.0 μm of the first layer (1 stThe mixture was uniformly mixed with 1.5 parts by weight of a glass frit layer and then dispersed by a three-roll kneading mill to prepare a first solar cell electrode forming composition.

[0075] Preparation Example 2 to Preparation Example 11

[0076] A second solar cell electrode-forming composition was prepared by the same method as in Preparation Example 1 except that the glass frits A to J described in Table 1 below were used.

[0077]

Table 1

[0078] (Unit: mole percentage)

[0079]

[0080] Examples 1 to 8 and Comparative Examples 1 and 2

[0081] After printing aluminum paste on the back of a wafer (a monocrystalline wafer on which silicon nitride (SiNx:H) is formed as an anti-reflection film after texturing the front of a p-type wafer doped with boron, forming an n+ layer with POCl3), the wafer was dried at 300°C for 30 seconds. Subsequently, the first solar cell electrode forming composition according to Preparation Example 1 was screen-printed on the front of the wafer, dried at 300°C for 30 seconds to form the first electrode layer, and then the second solar cell electrode forming composition according to any one of Preparation Examples 2 to 11 was screen-printed thereon, dried at 300°C for 30 seconds to form the second electrode layer. Using a belt firing furnace, the cell formed by the above process was fired at 940°C for 70 seconds to prepare a solar cell.

[0082] Evaluation Example 1: Electrical Characteristics

[0083] Using a solar cell efficiency measuring device (Halm, Fortix tech), the short-circuit current (Isc, unit: A), open-circuit voltage (Voc, unit: mV), series resistance (Rs, unit: Ω), fill factor (FF, unit: %) and conversion efficiency (Eff., unit: %) of the solar cell sheets prepared in Examples 1 to 8 and Comparative Examples 1 and 2 were measured, and the results are shown in Table 2 below.

[0084] Evaluation Example 2: Adhesion

[0085] Flux (952S, Kester) was coated on the second electrode layer of the solar cell prepared in Examples 1 to 8 and Comparative Examples 1 and 2, and a soldering wire (62Sn / 36Pb / 2Ag, thickness 0.18 mm, width 1.5 mm) was bonded using an electric soldering iron at 360°C. Then, a tester (Mocel H5K-T, Tinius Olsen) was used to fix the end of the solder wire at an angle of 180 degrees, and the wire was pulled at a speed of 50 mm / min to measure the value. The results are shown in Table 2 below.

[0086]

Table 2

[0087]

[0088] From Table 2 above, it can be confirmed that the solar cells of Examples 1 to 8 have higher open circuit voltages and exhibit superior conversion efficiencies than the solar cells of Comparative Examples 1 and 2, which indicates that they also have superior adhesion.

[0089] So far, mainly the embodiments of the present invention have been described. A person skilled in the art to which the present invention belongs will understand that the present invention can be implemented in a deformed form within the scope of the essential characteristics of the present invention. Therefore, the disclosed embodiments should be considered from the perspective of illustration rather than limitation. The scope of the present invention appears in the claims rather than in the foregoing description, and all differences within the equivalent scope thereof should be interpreted as included in the present invention.

Claims

1. A solar cell electrode, characterized in that: include: The first electrode layer comprises a conductive powder and a first glass frit, wherein the first glass frit is a Pb-Te-Si-Na-WO type glass frit; as well as The second electrode layer is formed on the first electrode layer and comprises a conductive powder and a second glass frit which is different from the first glass frit and has a molar ratio of lead (Pb) oxide / (lead (Pb) oxide + copper (Cu) oxide) greater than 0.2 and less than 0.

95.

2. The solar cell electrode according to claim 1, characterized in that: The second glass frit contains 15 to 75 mol % of lead (Pb) oxide.

3. The solar cell electrode according to claim 1, characterized in that: The second glass frit contains 3 to 60 mol % of copper (Cu) oxide.

4. The solar cell electrode according to claim 1, characterized in that: The second glass frit further includes one or more elements selected from the group consisting of tellurium (Te), bismuth (Bi), lithium (Li), boron (B), phosphorus (P), germanium (Ge), gallium (Ga), cerium (Ce), iron (Fe), silicon (Si), zinc (Zn), tungsten (W), magnesium (Mg), cesium (Cs), strontium (Sr), molybdenum (Mo), titanium (Ti), tin (Sn), indium (In), vanadium (V), barium (Ba), nickel (Ni), sodium (Na), potassium (K), arsenic (As), cobalt (Co), zirconium (Zr), manganese (Mn) and aluminum (Al).

5. The solar cell electrode according to claim 1, characterized in that: The second glass frit further includes one or more of silicon (Si) oxide, titanium (Ti) oxide, and iron (Fe) oxide.

6. The solar cell electrode according to claim 1, characterized in that: The second glass frit further includes 5 to 25 mol % of silicon (Si) oxide.

7. The solar cell electrode according to claim 1, characterized in that: The second glass frit further includes 0.3 to 13 mol % of titanium (Ti) oxide.

8. The solar cell electrode according to claim 1, characterized in that: The second glass frit further includes 1 to 5 mol % of iron (Fe) oxide.

9. The solar cell electrode according to claim 1, characterized in that: The second glass frit further includes one or more of boron (B) oxide, sodium (Na) oxide, aluminum (Al) oxide, tungsten (W) oxide, and molybdenum (Mo) oxide.

10. A method for forming a solar cell electrode according to any one of claims 1 to 9, characterized in that: include: The step of applying a first solar cell electrode-forming composition comprising a conductive powder, a first glass frit and an organic vehicle to form a first electrode layer, a step of applying a second solar cell electrode-forming composition comprising a conductive powder, a second glass frit and an organic vehicle to form a second electrode layer, and Firing step.

11. The method for forming a solar cell electrode according to claim 10, wherein: The first solar cell electrode forming composition or the second solar cell electrode forming composition further includes one or more of a dispersant, a thixotropic agent, a plasticizer, a viscosity stabilizer, a defoaming agent, a pigment, a UV stabilizer, an antioxidant, and a coupling agent.

12. The method for forming a solar cell electrode according to claim 10, wherein: The first solar cell electrode forming composition comprises 60 to 95 weight percent of the conductive powder, 0.1 to 20 weight percent of the first glass frit, and 1 to 30 weight percent of the organic vehicle. The second solar cell electrode forming composition comprises 60 to 95 weight percent of the conductive powder, 0.1 to 20 weight percent of the second glass frit, and 1 to 30 weight percent of the organic vehicle.