A method for comprehensive recovery of scrapped lithium iron phosphate
By calcining calcium hydroxide and multi-step processing, the problem of iron and phosphorus recovery from waste lithium iron phosphate was solved, and iron phosphate and lithium carbonate that meet the requirements of lithium iron phosphate were prepared, simplifying the recycling process and reducing waste residue.
Patent Information
- Application Number
- CN202210662849.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-13
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-06-13
AI Technical Summary
Existing technologies are insufficient to effectively recover iron and phosphorus from scrapped lithium iron phosphate, and the recovered iron phosphate does not meet physical properties, thus affecting the production requirements of lithium iron phosphate.
The process involves calcining a mixture of calcium hydroxide and scrap lithium iron phosphate, followed by water immersion, adsorption filtration, concentration precipitation, slag washing, leaching, oxidation, precipitation, and aging. This process separates and adjusts the crystal form of iron phosphate, producing an iron phosphate precursor and industrial-grade lithium carbonate that meet the requirements of lithium iron phosphate.
It enables efficient recovery of lithium to produce lithium carbonate, and iron and phosphorus to produce iron phosphate that meets the requirements of lithium iron phosphate, reducing the amount of waste residue and processing complexity, and simplifying the process.
Smart Images

Figure CN114976337B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive recovery of lithium iron phosphate, and in particular to a method for comprehensive recovery of scrapped lithium iron phosphate. Background Art
[0002] Lithium iron phosphate is a positive electrode material for lithium-ion batteries. It is generally made by sintering iron phosphate and lithium salt through a pyrolysis method. Its chemical formula is LiFePO4 (LFP for short). The crystal structures of iron phosphate and lithium iron phosphate are similar. Iron phosphate is the main raw material for synthesizing lithium iron phosphate and is called a lithium iron phosphate precursor.
[0003] The traditional method of recycling lithium iron phosphate can only effectively recover the lithium in it. After processing, a large amount of waste slag will be produced, and the iron content of about 35% and the phosphorus content of about 18% are difficult to recover.
[0004] At present, there are methods to recycle the iron phosphate, but the recycled iron phosphate is only a crude product, and the physical performance index of iron phosphate cannot meet the requirements of lithium iron phosphate. It is mainly affected by several reasons: 1) The adhesive in the scrapped lithium iron phosphate battery or positive electrode is not removed during processing; 2) The negative electrode powder is mixed together when the scrapped battery is disassembled, and the negative electrode contains graphite powder and organic matter; 3) The traditional recycling method can only make the chemical impurity index in the iron phosphate meet the requirements of lithium iron phosphate, but it is difficult to meet the requirements of the physical index of lithium iron phosphate. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a method for comprehensive recovery of scrapped lithium iron phosphate, which solves the problems raised in the above-mentioned background technology.
[0006] To achieve the above purpose, the present invention is implemented by the following technical scheme: a method for comprehensive recovery of scrapped lithium iron phosphate, comprising the following steps:
[0007] S1、Crushed Mix
[0008] Calcium hydroxide is screened through a 200-mesh sieve, and only the under-sieve portion is taken and ground together with the lithium iron phosphate scrap material. The amount of calcium hydroxide used is 0.85-1.05 times the theoretical amount. After mixing, it is screened through a 425-mesh sieve and the under-sieve material is kept for later use;
[0009] S2. Calcination
[0010] The material after passing through the 425 mesh sieve in S1 is put into a calcining furnace and calcined for 180-240 minutes at a temperature of 630-750°C. At the same time, compressed air is introduced during the calcination process. The compressed air pressure is controlled at 0.5-0.8MPa and the flow rate is controlled at 18-30m3 / hour.
[0011] S3, Flooding
[0012] After the calcined material is cooled, wet grinding is adopted, and the particle size of the wet grinding is 95% through a 100-mesh sieve. The particle size control is conducive to the water leaching of lithium. After wet grinding, the material enters the water leaching tank for leaching. The leaching is carried out at room temperature. The leaching time is 60-120 minutes. The amount of water added is 1.5-2.5 times that of the calcined material before wet grinding. After water leaching, the filtrate is filtered to obtain lithium hydroxide, and the filter residue is a mixture of iron oxide and calcium phosphate;
[0013] S4, adsorption filtration
[0014] Add activated carbon to lithium hydroxide solution to remove organic impurities and suspended fine particles to purify the lithium hydroxide solution. The temperature of the filtrate is controlled between 35-55°C. The amount of activated carbon added is 0.1-0.5 kg per cubic meter. The reaction time is 30-60 minutes. After the reaction is completed, filter it and then use a 0.05-0.1 micron pore size filter to finely filter and remove fine activated carbon particles.
[0015] S5. Concentration and precipitation
[0016] The lithium hydroxide solution after fine filtration is heated and evaporated in a reactor into which carbon dioxide is introduced to obtain lithium carbonate precipitation. The carbon dioxide pressure is 0.2-0.5MPa, the introduction amount is 10-30m3 / hour, and the reaction time is 120-180 minutes. Lithium carbonate is obtained after filtration, and the mother liquor is returned to the adsorption filtration process.
[0017] S6, slag washing
[0018] The slag after water immersion in step S3, whose main components are graphite, iron oxide, calcium phosphate, copper, aluminum, etc., is put into a slag washing tank, pure water is added to adjust the slurry, the temperature is controlled at 55-70°C, the pH value is controlled at 3.0-4.5 with sulfuric acid, and the reaction time is 60-90 minutes, mainly to remove the residual lithium therein.
[0019] S7, Leaching
[0020] The slag washed in step S6 is put into a leaching tank, and phosphoric acid is first added in an amount of 0.9-1.1 times the theoretical amount of dissolved iron oxide. The reaction temperature is 65-95°C and the reaction time is 60-90 minutes. Iron powder is then added to adjust the pH value to less than 1. The reaction is continued for 60-90 minutes. The iron powder is used to supplement the iron content in the solution. After the reaction is completed, a phosphorus and iron complex solution is obtained by filtering. The slag mainly contains graphite, calcium phosphate, copper, aluminum, etc.
[0021] S8, Oxidation
[0022] After leaching and filtration, the liquid is heated to 85-95°C, and iron powder is added. The amount of iron powder is 0.01-0.2 kg per cubic meter, and the reaction time is 30-60 minutes. The purpose is to continue to replenish the iron ions in the solution and promote the precipitation of excess iron and phosphorus to achieve a balanced phosphorus-iron ratio. After the reaction of adding iron powder is completed, hydrogen peroxide is added to oxidize the divalent iron ions in the solution into trivalent iron ions. A small amount of precipitation will be produced during the oxidation process, which needs to be finely filtered to remove the precipitation. The finely filtered solution enters the next process.
[0023] S9, precipitation
[0024] The fine filtrate and sodium hydroxide are added to the precipitation reaction tank in parallel, and the crystal form and growth rate of iron phosphate are controlled by controlling the flow rates of the two. The flow rates of the fine filtrate and sodium hydroxide are calculated based on their residence time in the reactor for 2-4 hours, that is, when the effective volume of the reactor is 1 cubic meter, the sum of the flow rates of the two is 0.5-0.25 cubic meters per hour.
[0025] S10, Ripening
[0026] After the reaction is completed, the slurry is transferred to another reactor and the stirring speed is reduced to 1 / 2-1 / 3 of the original reactor. The main purpose is to modify the crystal appearance of iron phosphate under low stirring intensity. In addition, the fine particles produced previously are dissolved during the aging process to correct the particle size distribution of iron phosphate. The aging temperature is controlled at 50-60°C for 30-60 minutes. After aging, it is filtered.
[0027] S11. Washing
[0028] The solid after filtration is iron phosphate. The iron phosphate is washed with pure water at a temperature of 45-60°C. The washing is performed three times. After each washing, the water needs to be dried before the next washing. The total amount of washing water is 8-12 cubic meters per ton of iron phosphate. Finally, the iron phosphate is dried to obtain the finished iron phosphate product.
[0029] Furthermore, the purpose of the crushing and mixing in the step S1 is to crush the lithium iron phosphate to a certain extent and fully mix it with the calcium hydroxide;
[0030] Furthermore, the calcination reaction process in step S2 is as follows:
[0031] 2LiFePO4+3Ca(OH)2+1 / 2O2=2LiOH+Fe2O3+Ca3(PO4)2+2H2O.
[0032] Furthermore, the reaction between the lithium hydroxide solution and carbon dioxide during the concentration and precipitation process in step S5 is as follows: 2LiOH+CO2=Li2CO3↓+H2O.
[0033] Furthermore, the reaction during the leaching process in step S7 is specifically as follows:
[0034] Fe+2H3PO4=Fe(H2PO4)2+H2↑
[0035] Fe2O3+4H3PO4=2HFe(HPO4)2+3H2O
[0036] Fe2O3+4H3PO4=2H3Fe(PO4)2+3H2O.
[0037] Furthermore, in the precipitation process of step S9, the principle of precipitation is that iron phosphate will produce precipitation when the pH is 1.8-2.0, and the flow ratio of iron phosphate to sodium hydroxide is controlled by controlling the endpoint pH value at 1.8-2.0.
[0038] The invention provides a method for comprehensive recovery of scrapped lithium iron phosphate, which has the following beneficial effects: the method for comprehensive recovery of scrapped lithium iron phosphate reduces the introduction of impurities as much as possible during the recovery process, recovers lithium into crude lithium carbonate, controls the synthesis process of iron phosphate to be made into an iron phosphate precursor that meets the requirements for producing lithium iron phosphate, adopts a method of calcining with calcium hydroxide to convert the lithium therein into water-soluble lithium hydroxide, and iron and phosphorus generate insoluble oxides and salts that enter the slag, and the lithium hydroxide is prepared into industrial-grade lithium carbonate, and the iron and phosphorus in the slag are dissolved by phosphoric acid and supplemented with a certain proportion of iron to prepare iron phosphate, and the crystal shape of the iron phosphate is controlled by adjusting the precipitation process to meet the requirements for lithium iron phosphate production, the method prepares lithium into industrial-grade lithium carbonate that can be directly used for the firing of positive electrode materials, and prepares phosphorus and iron into iron phosphate products that can be directly used for the firing of lithium iron phosphate, and at the same time directly solidifies the electrolyte and adhesive of the battery during the treatment process, thereby reducing the treatment amount of waste gas, and has the advantages of simple treatment process, short flow, and less amount of waste slag generated during the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a schematic diagram of the process flow of the method for comprehensive recovery of scrapped lithium iron phosphate according to the present invention. DETAILED DESCRIPTION
[0040] A method for comprehensive recovery of scrapped lithium iron phosphate, comprising the following steps:
[0041] S1、Crushed Mix
[0042] Calcium hydroxide is passed through a 200-mesh sieve, and only the part under the sieve is taken to be ground together with the scrapped lithium iron phosphate. The amount of calcium hydroxide used is 0.85-1.05 times the theoretical amount. The purpose of crushing and mixing is to crush the lithium iron phosphate to a certain extent and fully mix it with calcium hydroxide. After mixing, it is passed through a 425-mesh sieve. The purpose of sieving is to remove impurities such as metals, and the material under the sieve enters the next process;
[0043] S2. Calcination
[0044] The material under the 425 mesh sieve is put into a calcining furnace and calcined for 180-240 minutes at a temperature of 630-750°C. During the calcination process, compressed air is introduced, and the compressed air pressure is controlled at 0.5-0.8MPa and the flow rate is controlled at 18-30m3 / hour. The reaction of the calcination process is as follows:
[0045] 2LiFePO4+3Ca(OH)2+1 / 2O2=2LiOH+Fe2O3+Ca3(PO4)2+2H2O;
[0046] S3, Flooding
[0047] After the calcined material is cooled, wet grinding is adopted, and the particle size of the wet grinding is 95% through a 100-mesh sieve. The particle size control is conducive to the water leaching of lithium. After wet grinding, the material enters the water leaching tank for leaching. The leaching is carried out at room temperature. The leaching time is 60-120 minutes. The amount of water added is 1.5-2.5 times that of the calcined material before wet grinding. After water leaching, the filtrate is filtered to obtain lithium hydroxide, and the filter residue is a mixture of iron oxide and calcium phosphate;
[0048] S4, adsorption filtration
[0049] Add activated carbon to lithium hydroxide solution to remove organic impurities and suspended fine particles to purify the lithium hydroxide solution. The temperature of the filtrate is controlled between 35-55°C. The amount of activated carbon added is 0.1-0.5 kg per cubic meter. The reaction time is 30-60 minutes. After the reaction is completed, filter it and then use a 0.05-0.1 micron pore size filter to finely filter and remove fine activated carbon particles.
[0050] S5. Concentration and precipitation
[0051] The lithium hydroxide solution after fine filtration is heated and evaporated in a reactor into which carbon dioxide is introduced to obtain lithium carbonate precipitation. The carbon dioxide pressure is 0.2-0.5MPa, the amount introduced is 10-30m3 / hour, the reaction time is 120-180 minutes, and lithium carbonate is obtained after filtration. The mother liquor is returned to the adsorption filtration process. The specific reaction is as follows: 2LiOH+CO2=Li2CO3↓+H2O.
[0052] S6, slag washing
[0053] The slag after water immersion in step S3, whose main components are graphite, iron oxide, calcium phosphate, copper, aluminum, etc., is put into a slag washing tank, pure water is added to adjust the slurry, the temperature is controlled at 55-70°C, the pH value is controlled at 3.0-4.5 with sulfuric acid, and the reaction time is 60-90 minutes, mainly to remove the residual lithium therein.
[0054] S7, Leaching
[0055] The washed slag in step S6 is put into a leaching tank, and phosphoric acid is first added, the amount of phosphoric acid added is 0.9-1.1 times the theoretical amount of dissolved iron oxide, the reaction temperature is 65-95°C, the reaction time is 60-90 minutes, and then iron powder is added, the pH value is adjusted to less than 1, and the reaction is carried out for 60-90 minutes. The iron powder supplements the iron content in the solution. After the reaction is completed, the complex solution of phosphorus and iron is obtained by filtering. The slag mainly contains graphite, calcium phosphate, copper, aluminum, etc. The reaction is as follows:
[0056] Fe+2H3PO4=Fe(H2PO4)2+H2↑
[0057] Fe2O3+4H3PO4=2HFe(HPO4)2+3H2O
[0058] Fe2O3+4H3PO4=2H3Fe(PO4)2+3H2O.
[0059] S8, Oxidation
[0060] After leaching and filtration, the liquid is heated to 85-95°C, and iron powder is added. The amount of iron powder is 0.01-0.2 kg per cubic meter. The reaction time is 30-60 minutes. The purpose is to continue to replenish the iron ions in the solution and promote the precipitation of excess iron and phosphorus to achieve a balanced phosphorus-iron ratio. After the reaction of adding iron powder is completed, hydrogen peroxide is added to oxidize the divalent iron ions in the solution into trivalent iron ions. The specific reaction is as follows:
[0061] 2Fe(H2PO4)2+H2O2=2FePO4+H2O+2H3PO4
[0062] HFe(HPO4)2+H2O2=FePO4+H2O+H3PO4+1 / 2O2↑
[0063] H3Fe(PO4)2+H2O2=FePO4+H2O+H3PO4+1 / 2O2↑
[0064] The oxidation process will produce a small amount of precipitation, which needs to be removed by fine filtration. The filtered solution enters the next process.
[0065] S9, precipitation
[0066] The principle of precipitation is that iron phosphate will produce precipitation when the pH is 1.8-2.0. The present invention is to add the fine filtrate and sodium hydroxide to the precipitation reaction tank in a parallel flow manner, and control the crystal form and growth rate of iron phosphate by controlling the flow rate of the two. The flow rate of the fine filtrate and sodium hydroxide is calculated by staying in the reactor for 2-4 hours, that is, when the effective volume of the reactor is 1 cubic meter, the sum of the flow rates of the two is 0.5-0.25 cubic meters per hour. The flow ratio of iron phosphate to sodium hydroxide is controlled by controlling the endpoint pH value at 1.8-2.0.
[0067] S10, Ripening
[0068] After the reaction is completed, the slurry is transferred to another reactor and the stirring speed is reduced to 1 / 2-1 / 3 of the original reactor. The main purpose is to modify the crystal appearance of iron phosphate under low stirring intensity. In addition, the fine particles produced previously are dissolved during the aging process to correct the particle size distribution of iron phosphate. The aging temperature is controlled at 50-60°C for 30-60 minutes. After aging, it is filtered.
[0069] S11. Washing
[0070] The solid after filtration is iron phosphate. The iron phosphate is washed with pure water at a temperature of 45-60°C. The washing is performed three times. After each washing, the water needs to be dried before the next washing. The total amount of washing water is 8-12 cubic meters per ton of iron phosphate. Finally, the iron phosphate is dried to obtain the finished iron phosphate product.
[0071] In summary, the method for comprehensive recovery of scrapped lithium iron phosphate includes the following specific steps:
[0072] S1、Crushed Mix
[0073] Calcium hydroxide is passed through a 200-mesh sieve, and only the part under the sieve is taken to be ground together with the scrapped lithium iron phosphate. The amount of calcium hydroxide used is 0.85-1.05 times the theoretical amount. The purpose of crushing and mixing is to crush the lithium iron phosphate to a certain extent and fully mix it with calcium hydroxide. After mixing, it is passed through a 425-mesh sieve. The purpose of sieving is to remove impurities such as metals, and the material under the sieve enters the next process;
[0074] S2. Calcination
[0075] The material under the 425 mesh sieve is put into a calcining furnace and calcined for 180-240 minutes at a temperature of 630-750°C. During the calcination process, compressed air is introduced, and the compressed air pressure is controlled at 0.5-0.8MPa and the flow rate is controlled at 18-30m3 / hour;
[0076] S3, Flooding
[0077] After the calcined material is cooled, wet grinding is adopted, and the particle size of the wet grinding is 95% through a 100-mesh sieve. The particle size control is conducive to the water leaching of lithium. After wet grinding, the material enters the water leaching tank for leaching. The leaching is carried out at room temperature. The leaching time is 60-120 minutes. The amount of water added is 1.5-2.5 times that of the calcined material before wet grinding. After water leaching, the filtrate is filtered to obtain lithium hydroxide, and the filter residue is a mixture of iron oxide and calcium phosphate;
[0078] S4, adsorption filtration
[0079] Add activated carbon to lithium hydroxide solution to remove organic impurities and suspended fine particles to purify the lithium hydroxide solution. The temperature of the filtrate is controlled between 35-55°C. The amount of activated carbon added is 0.1-0.5 kg per cubic meter. The reaction time is 30-60 minutes. After the reaction is completed, filter it and then use a 0.05-0.1 micron pore size filter to finely filter and remove fine activated carbon particles.
[0080] S5. Concentration and precipitation
[0081] The lithium hydroxide solution after fine filtration is heated and evaporated in a reactor into which carbon dioxide is introduced to obtain lithium carbonate precipitation. The carbon dioxide pressure is 0.2-0.5MPa, the introduction amount is 10-30m3 / hour, and the reaction time is 120-180 minutes. After filtration, lithium carbonate is obtained, and the mother liquor is returned to the adsorption filtration process.
[0082] S6, slag washing
[0083] The slag after water immersion in step S3, whose main components are graphite, iron oxide, calcium phosphate, copper, aluminum, etc., is put into a slag washing tank, pure water is added to adjust the slurry, the temperature is controlled at 55-70°C, the pH value is controlled at 3.0-4.5 with sulfuric acid, and the reaction time is 60-90 minutes, mainly to remove the residual lithium therein.
[0084] S7, Leaching
[0085] The slag washed in step S6 is put into a leaching tank, and phosphoric acid is first added in an amount of 0.9-1.1 times the theoretical amount of dissolved iron oxide. The reaction temperature is 65-95°C and the reaction time is 60-90 minutes. Iron powder is then added to adjust the pH value to less than 1. The reaction is continued for 60-90 minutes. The iron powder is used to supplement the iron content in the solution. After the reaction is completed, a phosphorus and iron complex solution is obtained by filtering. The slag mainly contains graphite, calcium phosphate, copper, aluminum, etc.
[0086] S8, Oxidation
[0087] After leaching and filtration, the liquid is heated to 85-95°C, and iron powder is added. The amount of iron powder is 0.01-0.2 kg per cubic meter, and the reaction time is 30-60 minutes. The purpose is to continue to replenish the iron ions in the solution and promote the precipitation of excess iron and phosphorus to achieve a balanced phosphorus-iron ratio. After the reaction of adding iron powder is completed, hydrogen peroxide is added to oxidize the divalent iron ions in the solution into trivalent iron ions. A small amount of precipitation will be produced during the oxidation process, which needs to be finely filtered to remove the precipitation. The finely filtered solution enters the next process.
[0088] S9, precipitation
[0089] The principle of precipitation is that iron phosphate will produce precipitation when the pH is 1.8-2.0. The present invention is to add the fine filtrate and sodium hydroxide to the precipitation reaction tank in a parallel flow manner, and control the crystal form and growth rate of iron phosphate by controlling the flow rate of the two. The flow rate of the fine filtrate and sodium hydroxide is calculated by staying in the reactor for 2-4 hours, that is, when the effective volume of the reactor is 1 cubic meter, the sum of the flow rates of the two is 0.5-0.25 cubic meters per hour. The flow ratio of iron phosphate to sodium hydroxide is controlled by controlling the endpoint pH value at 1.8-2.0.
[0090] S10, Ripening
[0091] After the reaction is completed, the slurry is transferred to another reactor and the stirring speed is reduced to 1 / 2-1 / 3 of the original reactor. The main purpose is to modify the crystal appearance of iron phosphate under low stirring intensity. In addition, the fine particles produced previously are dissolved during the aging process to correct the particle size distribution of iron phosphate. The aging temperature is controlled at 50-60°C for 30-60 minutes. After aging, it is filtered.
[0092] S11. Washing
[0093] The solid after filtration is iron phosphate. The iron phosphate is washed with pure water at a temperature of 45-60°C. The washing is performed three times. After each washing, the water needs to be dried before the next washing. The total amount of washing water is 8-12 cubic meters per ton of iron phosphate. Finally, the iron phosphate is dried to obtain the finished iron phosphate product.
Claims
1. A method for comprehensive recovery of scrapped lithium iron phosphate, characterized in that: The following steps are involved: S1、Crushed Mix Calcium hydroxide is screened through a 200-mesh sieve, and only the under-sieve portion is taken and ground together with the lithium iron phosphate scrap material. The amount of calcium hydroxide used is 0.85-1.05 times the theoretical amount. After mixing, it is screened through a 425-mesh sieve and the under-sieve material is kept for later use; S2. Calcination The material after passing through the 425 mesh sieve in S1 is put into a calcining furnace and calcined for 180-240 minutes at a temperature of 630-750°C. At the same time, compressed air is introduced during the calcination process. The compressed air pressure is controlled at 0.5-0.8MPa and the flow rate is controlled at 18-30m3 / hour. S3, Flooding After the calcined material is cooled, wet grinding is adopted, and the particle size of the wet grinding is 95% through a 100-mesh sieve. The particle size control is conducive to the water leaching of lithium. After wet grinding, the material enters the water leaching tank for leaching. The leaching is carried out at room temperature. The leaching time is 60-120 minutes. The amount of water added is 1.5-2.5 times that of the calcined material before wet grinding. After water leaching, the filtrate is filtered to obtain lithium hydroxide, and the filter residue is a mixture of iron oxide and calcium phosphate; S4, adsorption filtration Add activated carbon to lithium hydroxide solution to remove organic impurities and suspended fine particles to purify the lithium hydroxide solution. The temperature of the filtrate is controlled between 35-55°C. The amount of activated carbon added is 0.1-0.5 kg per cubic meter. The reaction time is 30-60 minutes. After the reaction is completed, filter it and then use a 0.05-0.1 micron pore size filter to finely filter and remove fine activated carbon particles. S5. Concentration and precipitation The lithium hydroxide solution after fine filtration is heated and evaporated in a reactor into which carbon dioxide is introduced to obtain lithium carbonate precipitation. The carbon dioxide pressure is 0.2-0.5MPa, the introduction amount is 10-30m3 / hour, and the reaction time is 120-180 minutes. After filtration, lithium carbonate is obtained, and the mother liquor is returned to the adsorption filtration step; S6, slag washing The slag after water immersion in step S3, whose main components are graphite, iron oxide, calcium phosphate, copper and aluminum, is put into a slag washing tank, pure water is added to adjust the slurry, the temperature is controlled at 55-70°C, the pH value is controlled at 3.0-4.5 with sulfuric acid, and the reaction time is 60-90 minutes, mainly to remove the residual lithium therein; S7, Leaching The washed slag in step S6 is put into a leaching tank, phosphoric acid is first added, the amount of phosphoric acid added is 0.9-1.1 times the theoretical amount of dissolved iron oxide, the reaction temperature is 65-95°C, the reaction time is 60-90 minutes, and then iron powder is added, the pH value is adjusted to less than 1, and the reaction is carried out for 60-90 minutes. The iron powder supplements the iron content in the solution. After the reaction is completed, the complex solution of phosphorus and iron is obtained by filtering. The slag mainly contains graphite, calcium phosphate, copper and aluminum; S8, Oxidation After leaching and filtration, the liquid is heated to 85-95°C, and iron powder is added. The amount of iron powder is 0.01-0.2 kg per cubic meter, and the reaction time is 30-60 minutes. The purpose is to continue to replenish the iron ions in the solution and promote the formation of precipitation between the excess iron and phosphorus to achieve a balanced phosphorus-iron ratio. After the reaction of adding iron powder is completed, hydrogen peroxide is added to oxidize the divalent iron ions in the solution into trivalent iron ions. A small amount of precipitation will be produced during the oxidation process, which needs to be finely filtered to remove the precipitation. The finely filtered solution enters the next process; S9, precipitation The fine filtrate and sodium hydroxide are added to the precipitation reaction tank in parallel, and the crystal form and growth rate of iron phosphate are controlled by controlling the flow rate of the two. The flow rate of the fine filtrate and sodium hydroxide is calculated based on staying in the reactor for 2-4 hours, that is, when the effective volume of the reactor is 1 cubic meter, the sum of the flow rates of the two is 0.5-0.25 cubic meters / hour; S10, Ripening After the reaction is completed, the slurry is transferred to another reactor and the stirring speed is reduced to 1 / 2-1 / 3 of the original reactor. The main purpose is to modify the crystal appearance of the iron phosphate under the condition of low stirring intensity. In addition, the fine particles produced before are dissolved during the aging process to correct the particle size distribution of the iron phosphate. The aging temperature is controlled at 50-60°C for 30-60 minutes. After the aging is completed, it is filtered; S11. Washing The solid after filtration is iron phosphate. The iron phosphate is washed with pure water at a temperature of 45-60°C. The washing is performed three times. After each washing, the water needs to be dried before the next washing. The total amount of washing water is 8-12 cubic meters per ton of iron phosphate. Finally, the iron phosphate is dried to obtain the finished iron phosphate product.
2. The method for comprehensive recovery of scrapped lithium iron phosphate according to claim 1, characterized in that: The purpose of the crushing and mixing process in step S1 is to crush the lithium iron phosphate to a certain extent and fully mix it with the calcium hydroxide.
3. The method for comprehensive recovery of scrapped lithium iron phosphate according to claim 1, characterized in that: The calcination reaction process in step S2 is as follows: 2LiFePO4+3Ca(OH)2+1 / 2O2=2LiOH+Fe2O3+Ca3(PO4)2+2H2O.
4. The method for comprehensive recovery of scrapped lithium iron phosphate according to claim 1, characterized in that: The reaction between the lithium hydroxide solution and the carbon dioxide during the concentration precipitation process in step S5 is as follows: 2LiOH+CO2=Li2CO3↓+H2O.
5. The method for comprehensive recovery of scrapped lithium iron phosphate according to claim 1, characterized in that: The reaction during the leaching process in step S7 is as follows: Fe+2H3PO4=Fe(H2PO4)2+H2↑ Fe2O3+4H3PO4=2HFe(HPO4)2+3H2O Fe2O3+4H3PO4=2H3Fe(PO4)2+3H2O.
6. The method for comprehensive recovery of scrapped lithium iron phosphate according to claim 1, characterized in that: In the precipitation process of step S9, the principle of precipitation is that iron phosphate will produce precipitation when the pH is 1.8-2.0, and the flow ratio of iron phosphate to sodium hydroxide is controlled by controlling the end point pH value at 1.8-2.0.
Citation Information
Patent Citations
Recycling treatment technology of lithiumironphosphate waste
CN107857244A
Method for preparing battery-grade iron phosphate and industrial-grade lithium phosphate in waste lithium iron phosphate battery
CN109775678A
Recovery method of waste lithium iron phosphate battery positive electrode material
CN110482511A
Method for preparing iron phosphate precursor by using zinc hydrometallurgy high-iron solution
CN113716539A