A device and method for quantifying the solubility of ceramics in glass at different temperatures

By quantifying the temperature-changing solubility of ceramics in glass, the device and method solve the problem of solubility of ceramics in glass, realize effective glass additive screening of ceramic base materials, improve microwave dielectric properties, and fill the gap in the exploration of ceramic-glass matching. blank.

CN115060559BActive Publication Date: 2024-10-22XIDIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210664466.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-14
Publication Date
2024-10-22
Estimated Expiration
2042-06-14

AI Technical Summary

Technical Problem

The existing technology fails to effectively solve the problem of temperature-changing solubility of ceramics in glass, which affects the matching of the microwave dielectric properties of low-temperature co-fired ceramic materials and the glass-ceramic system.

Method used

A device and method were designed to quantify the temperature-changing solubility of ceramics in glass, including an alumina corundum boat, an alumina fixed support plate and a glass melting furnace. By measuring the solubility of ceramics in the liquid phase of glass, transmission electron microscopy was used to analyze the properties of the ceramics. The dissolution-precipitation process, combined with the corrosion degree, reflects the temperature-changing solubility of ceramics.

Benefits of technology

It achieves the ultimate dissolution state of ceramics in glass in a short time, quantifies the solubility of different glasses to ceramic base materials, saves engineering exploration time, reduces trial and error phenomena, and improves the screening of glass additives for ceramic substrates. efficiency, improving microwave dielectric properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115060559B_ABST
    Figure CN115060559B_ABST
Patent Text Reader

Abstract

A device and method for quantifying the variable temperature solubility of ceramics in glass, comprising the steps of isostatically pressing a ceramic base material into a cylindrical shape, sintering the ceramic base material at an optimal sintering temperature to achieve densification, and measuring the diameter of the ceramic base material; placing a glass powder material flat in an alumina corundum boat, inserting the ceramic material, and fixing the ceramic material by a fixed alumina support plate; operating a glass melting furnace to heat the glass powder material to a melting point or slightly above the melting point and keeping the temperature, then quickly taking out the ceramic material and pouring the glass liquid phase formed by melting the glass powder material into deionized water; corroding the ceramic material with concentrated sulfuric acid, and measuring the final diameter of the ceramic material; the variable temperature solubility of the densified ceramic material to be tested in the glass is reflected by the degree of corrosion of the diameter; and performing a transmission electron microscope test on the quenched glass, and according to the crystallization characteristics of the glass powder in the transmission electron microscope, it is proved that the ceramic material is dissolved in the glass liquid phase, and the "dissolve-in-precipitate" mass transfer process is completed, reflecting the variable temperature solubility of the ceramic material in the glass liquid phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic ceramics and their manufacturing, and in particular relates to a device and method for quantifying the temperature-dependent solubility of ceramics in glass. Background Art

[0002] Microwave dielectric ceramics are often used to prepare circuit packaging substrates, dielectric resonator antennas, filters and other components, and are key basic materials for 5G mobile communication applications. Traditional microwave equipment is metal processing, heavy and expensive. As a new type of three-dimensional integrated packaging interconnection technology, low-temperature co-fired ceramics (LTCC) provide a reliable solution for preparing ceramic modules or overall circuits with embedded electrodes. Therefore, the development of dielectric ceramic materials suitable for LTCC technology is a core issue recognized at home and abroad.

[0003] Since the built-in electrodes of LTCC technology are usually Ag or Cu metal, ceramics need to exhibit high-frequency microwave dielectric properties under low temperature conditions (co-fired with Ag below 950°C). Usually, the firing temperature of ceramic materials is relatively high (>1000°C), and researchers use liquid phase activation sintering mechanism to prepare low-temperature sintered ceramics. By introducing low-melting point oxides or glass materials into the ceramic base material, with the help of the low melting point properties of glass and the appearance of liquid phase during the heating process of the ceramic, the liquid phase wets the ceramic particles, and the ceramic particles are rearranged under the action of liquid capillary pressure. Subsequently, the tip parts of small and large particles are more dissolved due to the small radius of curvature and the greater pressure, so they precipitate on the low pressure surface (the side with a large radius of curvature), completing the "dissolution-precipitation" process. This composite material is often based on ceramics and doped with a certain proportion of glass materials, which is called glass-ceramic material.

[0004] However, as the technical steps of glass ceramics say, glass material and ceramics need to have a certain degree of compatibility, which means that the glass material should play a "wetting" role in the ceramics, and the ceramics also need to have a certain solubility in the glass liquid phase. Only by clarifying this key technical point can we realize that when the components of the ceramic system are different, there will be huge differences in the glass materials that are suitable for it, which will help to screen suitable glass materials that are conducive to reducing the firing of ceramic materials, and will be of great benefit to the breakthrough of LTCC ceramic systems with better microwave dielectric properties. However, to date, the technical problem of variable temperature solubility has not been solved. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a device and method for quantifying the variable temperature solubility of ceramics in glass, so as to provide guidance and reference value for the matching exploration of glass-ceramic systems and breakthroughs in microwave dielectric properties.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A device for quantifying the variable temperature solubility of ceramics in glass comprises a characterization device and a measuring device; the characterization device comprises an alumina corundum boat, an alumina fixed support plate and a glass melting furnace; the alumina corundum boat contains glass powder, the alumina fixed support plate is provided with a circular through hole, the alumina fixed support plate is arranged on the top of the alumina corundum boat, the densified ceramic to be tested is cylindrical, passes through the circular through hole and is limited by the circular through hole, is vertically inserted into the glass powder, and the glass powder is dissolved in the glass melting furnace; the measuring device is used to test the original diameter and the final diameter of the densified ceramic to be tested.

[0008] In one embodiment, a circular groove is vertically formed at the bottom of the alumina corundum boat, and the circular groove corresponds to the circular through hole, respectively realizing the position limitation of the densified ceramic to be tested at both ends.

[0009] The present invention also provides a method for quantifying the temperature-dependent solubility of ceramics in glass, comprising the following steps:

[0010] Step 1: The ceramic base material is isostatically pressed into a cylindrical shape and sintered at the optimal sintering temperature to achieve its densification. The densified ceramic to be tested is obtained and its original diameter is measured and recorded as R. 1 ;

[0011] Step 2: Place the glass powder flatly in an alumina corundum boat, insert the densified ceramic to be tested into the glass powder, and use an alumina fixed support plate to limit and fix it;

[0012] Step 3: Place the structure assembled in step 2 into a glass melting furnace, operate the glass melting furnace to heat up to the melting point of the glass powder or slightly above the melting point and keep it warm, then quickly take out the densified ceramic to be tested and pour the glass liquid phase formed by the melting of the glass powder into deionized water;

[0013] Step 4: Place the densified ceramic to be tested in concentrated sulfuric acid to corrode the glass residue attached to the surface, then rinse it clean and measure its final diameter, which is recorded as R. 2 The temperature-dependent solubility of the densified ceramic to be tested in the glass is measured by the degree of corrosion of the diameter, i.e., △R = (R 1 –R 2 ) / R 1 to reflect;

[0014] Step 5: The quenched glass is crushed and ball-milled and dispersed in an acetone solution. The dispersed liquid is placed on a Cu grid of a carbon-coated porous membrane for transmission electron microscopy testing. The precipitated crystals in the "dissolution-precipitation" process of the ceramic dissolving in the glass liquid phase reflect the variable temperature solubility of the ceramic in the glass liquid phase.

[0015] In one embodiment, the ceramic base material is Zn 0.5 Ti 0.5 NbO 4 The best sintering temperature is 1150°C, and the glass powder is Li 2 O–B 2 O 3 –SiO 2 .

[0016] In one embodiment, in step 1, the density test is performed after sintering as follows:

[0017] After the red absorption test, there is no red absorption phenomenon;

[0018] Scanning electron microscope observations at microscales of 1 mm and 10 μm show that there are no microcracks on the cylindrical side, the ceramic grains grow fully, and the microstructure is dense.

[0019] According to density calculation, the density reaches more than 95%;

[0020] Under the premise that all three test conditions are met, the density requirements are considered to be met.

[0021] In one embodiment, in step 2, the height of the glass powder in the alumina corundum boat is 3 / 4 of the height of the alumina corundum boat.

[0022] In one embodiment, in step 3, for the densified ceramic to be tested with a diameter of 10 mm and a height of 20 mm, the ceramic is kept at 900° C. for 5 hours to reach the limit state of dissolution.

[0023] In one embodiment, in step 3, different holding times are used to measure the temperature-dependent solubility at different times.

[0024] In one embodiment, the present invention adopts the following formula to fit the variable temperature dissolution property of ceramics in glass. When T gradually increases, ΔR eventually tends to a constant value. Combined with transmission electron microscopy characterization, this value reflects the variable temperature solubility:

[0025]

[0026] Where T represents the holding time.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] (1) By designing the characterization device and method, the limit state of ceramic corrosion in glass was obtained within a short insulation time, and the limit state of variable temperature dissolution was found by combining transmission electron microscopy analysis, which reflects the variable temperature solubility;

[0029] (2) Liquid phase activation sintering mechanism is an important theory to ensure the formation of ceramics by low temperature sintering. However, the theory mentions that whether glass is effective for ceramics is reflected in the fact that the ceramics must have a certain solubility in the glass liquid phase and should have a significant "solubility". Therefore, in combination with the present invention, the effectiveness of different types of glass for specific ceramic base materials can be specifically quantified;

[0030] (3) In engineering practice, decades of research have shown that the research status of "trial and error" exists in the research and development of low-temperature sintered ceramics: that is, by doping a large amount of glass additives into the ceramic system, and then testing the microwave dielectric properties of the glass ceramics, it is reflected whether the glass is effective and whether it can effectively achieve the purpose of reducing the burning. With the help of the present invention, the solubility can be reflected intuitively and quickly through the corrosion limit, and then the glass additive suitable for the ceramic matrix can be found more excellently and quickly, which greatly saves the time of engineering exploration and will greatly overcome the research status of "trial and error". BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the structure of the characterization device of the present invention.

[0032] Figure 2 Schematic diagram of the size of the characterization device in the embodiment of the present invention

[0033] Figure 3 This is the appearance of Examples 1-6 after being dissolved and corroded by concentrated sulfuric acid.

[0034] Figure 4 Undissolved Zn 0.5 Ti 0.5 NbO 4 Lithium Ceramic 2 O–B 2 O 3 –SiO 2 Glass powder and Li after quenching in Example 6 2 O–B 2 O 3 –SiO 2 Transmission electron microscopy image of glass powder. DETAILED DESCRIPTION

[0035] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.

[0036] The invention discloses a device for quantifying the solubility of ceramics in glass at different temperatures, which mainly comprises a characterization device and a measurement device.

[0037] like Figure 1 and Figure 2As shown, the characterization device includes an alumina corundum boat 1, an alumina fixed support plate 2 and a glass melting furnace, and takes a densified ceramic to be tested 4 as the detection object, and its appearance is cylindrical.

[0038] Among them, the alumina corundum boat 1 is used to hold the glass powder 3, the alumina fixed support plate 2 is placed flat on the top of the alumina corundum boat 1, and a circular through hole 21 is set on the alumina fixed support plate 2 for the densified ceramic to be tested 4 to pass through, and it is limited to keep it in a vertical state. The lower end of the densified ceramic to be tested 4 is inserted into the glass powder 3. The glass melting furnace provides a high temperature environment to dissolve the glass powder 3 so as to conduct a variable temperature solubility experiment of the densified ceramic to be tested 4. The highest temperature of the glass melting furnace can reach up to 1600°C. The measuring device is used to test the original diameter and final diameter of the densified ceramic to be tested 4.

[0039] Furthermore, in the present invention, a circular groove 11 is vertically provided at the bottom of the alumina corundum boat 1, and the circular groove 11 corresponds to the circular through hole 21, so as to limit the densified ceramic to be tested 4 at both ends.

[0040] Furthermore, in the present invention, the measuring device also includes equipment for X-ray diffraction and transmission electron microscopy characterization of the glass powder material that has been dissolved and quenched.

[0041] The components required for the characterization device of the present invention are low in cost, and the experimental operation is simple and feasible.

[0042] On this basis, in view of the lack of characterization of the variable temperature solubility of ceramics in glass, the method of quantifying the variable temperature solubility of ceramics in glass of the present invention comprises the following steps:

[0043] Step 1: The ceramic base material is isostatically pressed into a cylindrical shape and sintered at an optimal sintering temperature to achieve its densification, thereby obtaining a densified ceramic 4 to be tested, and measuring its original diameter, which is recorded as R. 1 .

[0044] In the embodiment of the present invention, the ceramic base material is a manganese-tantalum ore structure Zn 0.5 Ti 0.5 NbO 4 , isostatically pressed at 200 MPa into a cylindrical green body with a diameter of 10 mm and a height of 20 mm. The optimal sintering temperature is 1150°C, and a cooked body is obtained after sintering. Glass powder 3 is Li 2 O–B 2 O 3 –SiO 2 The characterization method of the present invention can characterize the dissolution amount and dissolution rate of ceramics in liquid glass at high temperature, and can be applied to different types of ceramic materials and glass.

[0045] The present invention performs density testing after sintering as follows:

[0046] After the red absorption test, no red absorption phenomenon was found; generally, the red absorption test needs to be carried out for 6 hours.

[0047] Scanning electron microscope observations at microscales of 1 mm and 10 μm showed that there were no microcracks on the cylindrical sides, the ceramic grains grew fully, and the microstructure was dense.

[0048] After density calculation, the density reaches more than 95%.

[0049] Under the premise that all three test conditions are met, it is considered to have reached the density requirement, thereby excluding the influence of microcracks and pores on providing channels for glass liquid phase penetration as much as possible. Then, when it is cooled to room temperature, its diameter is measured and recorded as R 1 .

[0050] Step 2: Place a certain amount of glass powder 3 flatly in the alumina corundum boat 1 (the powder height is best to reach 3 / 4 of the corundum boat height), and insert the densified ceramic to be tested 4 into the glass powder 3, and use the alumina fixed support plate 2 to limit and fix it.

[0051] In this embodiment, the size of the alumina corundum boat 1 is 48×24×14 mm, that is, the total length of the opening is 48 mm, the total width is 24 mm, the total height is 14 mm, the outer length of the bottom is 43 mm, and the outer width is 20 mm; the length, width and thickness of the alumina fixed support plate 2 are 32×20×5 mm respectively, and there is a circular through hole 21 with a diameter of 10 mm in the middle. The amount of glass powder 3 used is about 2.75 g.

[0052] Step 3: Place the structure assembled in step 2 into a glass melting furnace, operate the glass melting furnace to heat up to the melting point of the glass powder 3 or slightly above the melting point at a certain heating rate and keep it warm, then quickly remove the alumina fixed support plate 2 for reuse (can be operated by crucible tongs), and quickly take out the densified ceramic to be tested 4, and at the same time pour the glass liquid phase formed by the melting of the glass powder 3 into deionized water.

[0053] In this embodiment, the temperature is raised to 900°C at a heating rate of 3°C / min and kept at this temperature for 0 to 5 hours. In each experiment, different holding times can be used, that is, the densified ceramic to be tested 4 is dissolved in the glass liquid phase for different times, and the variable temperature solubility at different times is measured. For the densified ceramic to be tested 4 with a diameter of 10 mm and a height of 20 mm in this embodiment, the limit state of dissolution can be reached by keeping at 900°C for 5 hours.

[0054] Step 4: Place the densified ceramic 4 to be tested in concentrated sulfuric acid for a period of time (e.g., 48 hours) to corrode the glass residue attached to the surface, then take it out and rinse it, and measure its final diameter, which is recorded as R2 The variable temperature solubility of the densified ceramic 4 in glass can be determined by the degree of corrosion of the diameter, i.e., ΔR = (R 1 –R 2 ) / R 1 To reflect.

[0055] Step 5: The quenched glass is crushed and ball-milled to be made into ultrafine powder, and the powder is dispersed in an acetone solution. The dispersed liquid is placed on a Cu grid of a carbon-coated porous membrane for transmission electron microscopy testing. The purpose of this step is that according to the technical steps of glass ceramics, when the ceramic is dissolved in the glass liquid phase and undergoes the "dissolution-precipitation" process, crystals will precipitate, which can provide an experimental basis for crystallization, and at the same time, combined with the solubility limit state, provide evidence to support the existence of variable temperature solubility. Therefore, the precipitated crystals in the "dissolution-precipitation" process of the ceramic dissolved in the glass liquid phase can reflect the variable temperature solubility of the ceramic in the glass liquid phase.

[0056] In this embodiment, the ball milling is carried out in an alumina pot for 2 hours, and then the ball milling is carried out in an oven at 100°C and sieved through a 200-mesh sieve to obtain a uniform powder. 0.5 g of the fine powder is weighed and dispersed in an acetone solution, and the upper clear liquid after dispersion is placed on the Cu grid of the carbon-coated porous membrane for transmission electron microscopy testing.

[0057] The following table is a specific embodiment of various parameter combinations of the present invention:

[0058]

[0059] Figure 3 The morphology diagrams of Examples 5 and 6 after dissolution and acid corrosion show that, as the insulation time increases, the degree of corrosion of the diameter of the ceramic cylinder increases, reflecting the change in the dissolution process.

[0060] Figure 4 Undissolved Zn 0.5 Ti 0.5 NbO 4 Lithium Ceramic 2 O–B 2 O 3 –SiO 2 Glass and Li after quenching in Example 6 2 O–B 2 O 3 –SiO 2Transmission electron microscope image of the glass powder. Figure (a) is the microscopic morphology and electron diffraction pattern of the glass powder. It can be found that the sample is an amorphous structure with no diffraction spots or diffraction rings. In Figure (b), it is clearly found that crystalline spots and diffraction rings appeared in the sample after 5 hours of dissolution, indicating that the ceramic was dissolved in the glass liquid phase and underwent a "dissolution-precipitation" mass transfer process.

[0061] From the table data, it can be seen that in Examples 1-6, when Zn 0.5 Ti 0.5 NbO 4 The ceramic is dissolved in Li at 900℃ 2 O–B 2 O 3 –SiO 2 When the ceramic is in the glass, the corrosion rate gradually increases with the extension of the insulation time. In Examples 1 to 3, the degree of change of the corrosion rate is rapid, while in Examples 4 to 6, it can be clearly seen that although the corrosion rate is increasing, the increase is very slow, indicating that the dissolution process of the ceramic in the glass liquid phase has reached the maximum. Using nonlinear fitting methods to correlate the change of the corrosion rate with the insulation time, it can be found that when the following formula is used for fitting (where T represents the insulation time), the goodness of fit reaches 99.95%. As the insulation time continues to extend, the corrosion rate will theoretically approach 57% infinitely, indicating that at 900°C, Zn 0.5 Ti 0.5 NbO 4 Ceramics in Li 2 O–B 2 O 3 –SiO 2 The dissolution in the glass reaches its maximum at 5h, and the corrosion rate at this time is 58.26%. This corrosion rate represents the variable temperature dissolution property of ceramics in glass at 900℃. When T gradually increases, △R eventually tends to a constant value. Combined with transmission electron microscopy characterization, this value reflects the variable temperature solubility:

[0062]

[0063] The △R in this formula is a theoretical value obtained by fitting the △R actually tested in step 4, and the goodness of fit can reach 99.95%. There will be a slight error between the two, but the change trend is consistent.

[0064] This characterization method can be extended to other different types of ceramic materials. By evaluating the temperature system and insulation conditions when the ceramic base material reaches the solubility limit state in the glass, combined with transmission electron microscopy analysis, the variable temperature solubility of the ceramic in the glass can be reflected. Therefore, the design of this method is simple and feasible both in theory and in practice. In addition, this method is low-cost, highly efficient, and the test results are reliable and easy to repeat. It is suitable for any material system with liquid phase activation sintering, especially for the process exploration of LTCC ceramics to match suitable glass materials, and is expected to fill the gap in the characterization of ceramic "variable temperature solubility", becoming a key technical essential for screening out glass types that match ceramic base materials, and will also guide the exploration of ceramic-glass material matching and the breakthrough direction of improving the performance of microwave dielectric ceramics under low temperature sintering.

[0065] In summary, the present invention provides a method for quantifying Zn at different temperatures. 0.5 Ti 0.5 NbO 4 Ceramics in Li 2 O–B 2 O 3 –SiO 2 A method for measuring solubility in glass is designed. This characterization technology has no limitations and can be applied to any ceramic system. It also provides guidance for the matching of ceramics and glass and the exploration of the microwave dielectric properties of glass-ceramics.

Claims

1. A method for quantifying the solubility of ceramics in glass at different temperatures, which is implemented by using a device for quantifying the solubility of ceramics in glass at different temperatures, wherein the device for quantifying the solubility of ceramics in glass at different temperatures comprises a characterization device and a measurement device; the characterization device comprises an alumina corundum boat (1), an alumina fixed support plate (2) and a glass melting furnace; the alumina corundum boat (1) contains glass powder (3), the alumina fixed support plate (2) is provided with a circular through hole (21), the alumina fixed support plate (2) is arranged on the top of the alumina corundum boat (1), and the alumina fixed support plate (2) is arranged on the top of the alumina corundum boat (1), and the glass powder (3) is placed on the alumina corundum boat (1). The densified ceramic to be tested (4) is cylindrical, passes through the circular through hole (21) and is limited by the circular through hole (21), is vertically inserted into the glass powder (3), and the glass powder (3) is dissolved in the glass melting furnace; the measuring device is used to test the original diameter and final diameter of the densified ceramic to be tested (4); a circular groove (11) is vertically provided at the bottom of the alumina corundum boat (1), and the circular groove (11) corresponds to the circular through hole (21), and the position of the densified ceramic to be tested (4) is limited at both ends; It is characterized in that The steps include: Step 1: isostatically press the ceramic base material into a cylindrical shape, and sinter it at an optimal sintering temperature to achieve its densification, thereby obtaining a densified ceramic to be tested (4), and measuring its original diameter, which is recorded as R1; the ceramic base material is Zn 0.5 Ti 0.5 NbO4, the best sintering temperature is 1150℃; Step 2: Lay the glass powder (3) flat in the alumina corundum boat (1), insert the densified ceramic to be tested (4) into the glass powder (3), and use the alumina fixed support plate (2) to limit and fix it, wherein the glass powder (3) is Li2O-B2O3-SiO2; Step 3: Place the structure assembled in step 2 into a glass melting furnace, operate the glass melting furnace to raise the temperature to the melting point of the glass powder (3) or slightly above the melting point and keep the temperature, then quickly take out the densified ceramic to be tested (4) and pour the glass liquid phase formed by the melting of the glass powder (3) into deionized water; Step 4: The densified ceramic to be tested (4) after being dissolved is placed in concentrated sulfuric acid to corrode the glass residue attached to the surface, and then rinsed clean, and its final diameter is measured, which is recorded as R2; the variable temperature solubility of the densified ceramic to be tested (4) in glass is reflected by the degree of diameter corrosion, that is, △R = (R1–R2) / R1; Step 5: The quenched glass is crushed and ball-milled and dispersed in an acetone solution. The dispersed liquid is placed on a Cu grid of a carbon-coated porous membrane for transmission electron microscopy testing. The precipitated crystals in the "dissolution-precipitation" process of the ceramic dissolving in the glass liquid phase reflect the variable temperature solubility of the ceramic in the glass liquid phase. In step 3, different holding times are used to measure the variable temperature solubility at different times, and the variable temperature solubility properties of ceramics in glass are obtained by fitting using the following formula: T As the temperature increases gradually, △R eventually tends to a constant value. Combined with the transmission electron microscopy characterization, this value reflects the variable temperature solubility: In the formula T Represents the holding time.

2. The method for quantifying the solubility of ceramics in glass at different temperatures according to claim 1, characterized in that: In step 1, the density test is performed after sintering as follows: After the red absorption test, there is no red absorption phenomenon; Scanning electron microscopy showed that at the microscale of 1 mm and 10 μm, there were no microcracks on the cylindrical side, the ceramic grains grew fully, and the microstructure was dense. According to density calculation, the density reaches more than 95%; Under the premise that all three test conditions are met, the density requirements are considered to be met.

3. The method for quantifying the temperature-dependent solubility of ceramics in glass according to claim 1, characterized in that: In the step 2, the height of the glass powder (3) in the alumina corundum boat (1) is 3 / 4 of the height of the alumina corundum boat (1).

4. The method for quantifying the solubility of ceramics in glass at different temperatures according to claim 1, characterized in that: In step 3, the densified ceramic to be tested (4) with a diameter of 10 mm and a height of 20 mm is kept at 900° C. for 5 hours to reach the limit state of dissolution.