Porous alumina and catalyst
By reasonably adding silica and barium oxide to alumina, porous alumina with excellent heat resistance and coking resistance is formed, the problem of α-phase transformation and coking of porous alumina at high temperature is solved, and the problem of porous alumina at high temperature is realized. Maintaining large specific surface area and improving the stability of the catalyst.
Patent Information
- Application Number
- CN202180013686.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-26
- Filing Date
- 2021-02-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-02-18
AI Technical Summary
The existing porous alumina materials are easily converted into the alpha phase at high temperatures, resulting in a decrease in specific surface area and are prone to coking and inactivation in hydrocarbon reactions.
By adding an appropriate amount of silica and barium oxide to the alumina, the amount of addition is adjusted to form porous alumina with excellent heat resistance and coking resistance. The combination of silica and barium oxide is used to inhibit the alpha phase transition by inhibiting the alpha phase transition by using the combination of silica and barium oxide. and coke.
The heat resistance of maintaining a large specific surface area at high temperature is achieved, and the coking of the catalyst is suppressed, which significantly improves the stability and activity of the catalyst.
Smart Images

Figure CN115066396B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to porous alumina obtained by adding silicon dioxide and a solid basic oxide to alumina, and a catalyst using the porous alumina as a catalyst carrier, and particularly to porous alumina and a catalyst to which barium oxide is added as a solid basic oxide. Background Art
[0002] Porous alumina materials having a large specific surface area, such as γ-alumina, are useful as catalyst supports for supporting catalyst substances, filters, and the like, and studies have been conducted to improve their properties (see, for example, Patent Documents 1 to 5, etc.).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2004-203654
[0006] Patent Document 2: International Publication No. 2014 / 051091
[0007] Patent Document 3: International Publication No. 2012 / 096386
[0008] Patent Document 4: International Publication No. 2013 / 111457
[0009] Patent Document 5: Japanese Patent Application Publication No. 2009-061383
[0010] Non-patent literature
[0011] Non-patent document 1: Toru Numaguchi, “Evaluation of the activity and carbon precipitation of methane steam reforming catalysts”, Journal of Petroleum Science, Vol. 39, No. 3, 1996.
[0012] Non-patent document 2: Ki-Yong Lee, et al., "Deactivation by coke deposition on the HZSM-5catalysts in the methanol-to-hydrocarbon conversion", Journal of Physics and Chemistry of Solids 73 (2012) 1542–1545. Summary of the invention
[0013] Problems to be solved by the invention
[0014] However, existing porous alumina materials with large specific surface areas, such as γ-alumina, are easily transformed into α phases when subjected to high temperatures above 1000°C for a very short time, or even at relatively low temperatures for a long time, and their specific surface areas are significantly reduced. The transformation to the α phase tends to be more pronounced in a water vapor atmosphere and under high pressure.
[0015] If solid acidic additives such as silicon dioxide (SiO2) are used to suppress the transformation to the α phase, the heat resistance is greatly improved, and a large specific surface area can be maintained even at high temperatures. On the other hand, the solid acidity of the porous alumina material increases. Therefore, when a porous alumina material containing a solid acidic additive is used as a catalyst carrier, carbon precipitation (coking) is likely to occur on the catalyst surface in a reaction with hydrocarbons, which causes catalyst deactivation. Therefore, for catalyst carriers used in reactions using hydrocarbons such as steam reforming reactions, not only heat resistance but also anti-coking properties are required. In addition, it is well known that if the solid acidity of a porous carrier increases, coking is likely to occur, as is also disclosed in the above-mentioned non-patent documents 1 and 2.
[0016] Figure 1 The relationship between the SiO2 addition rate and the specific surface area of porous alumina with only silicon dioxide added, prepared by the same kneading method as the comparative sample described later, is shown in FIG. The specific surface areas of sample A obtained by calcining at 1000°C for 5 hours in air, sample B obtained by heat treatment at 1200°C for 5 hours with respect to sample A, and sample C obtained by heat treatment at 1200°C for 30 hours with respect to sample A were measured by the nitrogen adsorption BET method. Figure 1 As shown, as the SiO2 addition rate increases, the specific surface area after heat treatment is greatly improved, which shows that silica is effective in improving the heat resistance of porous alumina.
[0017] Figure 2 The figure shows the results of measuring the amount of solid acid and solid base on the surface of porous alumina by temperature rise desorption method (TPD, base probe molecule: NH3, acid probe molecule: CO2) for sample A. It can be seen that as the SiO2 addition rate increases, the amount of NH3 adsorption increases, the amount of CO2 adsorption decreases, the amount of solid acid on the surface of porous alumina increases, and the amount of solid base decreases.
[0018] Because the acid points and alkaline points on the solid surface are difficult to neutralize, they coexist. Silica, alumina and their mixed oxides are both solid acids and solid bases. Figure 2 As shown, both the amount of solid acid and the amount of solid base are measured without neutralization on the solid surface.
[0019] Depend on Figure 1 and Figure 2It is known that it is difficult to improve the heat resistance of γ-alumina and suppress the increase of solid acidity (anti-coking property) by simply adding solid acidic silica. In addition, for the purpose of improving heat resistance, it is reported that methods of adding barium and lanthanum to alumina do not have sufficient heat resistance (see Patent Documents 4 and 5).
[0020] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a porous alumina having excellent heat resistance and coking resistance, and also to provide a catalyst using the porous alumina as a catalyst carrier.
[0021] Means of solving the problem
[0022] As a result of intensive research, the inventors of the present application discovered that by combining silica with barium oxide as a solid alkaline oxide as an additive to porous alumina having a large specific surface area such as γ-alumina, and appropriately adjusting the amounts of silica and barium oxide added, it is possible to obtain porous alumina having excellent heat resistance and anti-coking properties compared to porous alumina to which only silica is added, thereby arriving at the invention shown below.
[0023] A porous alumina obtained by adding silicon dioxide (SiO2) and barium oxide (BaO) to aluminum oxide (Al2O3), wherein the silicon dioxide and the barium oxide are added to the alumina in the following manner:
[0024] The ratio of the amount of SiO2 added to the total mass of the amount of alumina and SiO2 added is defined as the SiO2 addition rate (mass %).
[0025] The ratio of the amount of BaO added to the total mass of the amount of alumina and the amount of SiO2 added is defined as the BaO addition rate (mass %).
[0026] The amount of SiO2 added is the amount obtained by converting the silicon (Si) content in the porous alumina into the SiO2 content.
[0027] The BaO addition amount is the amount obtained by converting the barium (Ba) content in the porous alumina into the BaO content.
[0028] In the range of the SiO2 addition rate being 3% by mass or less and the BaO addition rate being 14% by mass or less,
[0029] After the porous alumina is heat treated at 1200°C for 30 hours, the specific surface area measured by a prescribed measuring method is greater than a benchmark specific surface area, which is the specific surface area measured in the same manner as a benchmark porous alumina for comparison, with the SiO2 addition rate set to 3% by mass and the BaO addition rate set to 0% by mass.
[0030] The specific surface area is measured by the same method as for the porous alumina of the present invention and the reference porous alumina for comparison, but for example, the specific surface area can be measured by the same method as for the porous alumina of the present invention and the reference porous alumina for comparison. Figure 1 The specific surface area shown is measured by the well-known nitrogen adsorption BET method.
[0031] In addition, the amount of SiO2 added is defined as the amount obtained by converting the silicon (Si) content in the porous alumina into the SiO2 content, and the amount of barium added is defined as the amount obtained by converting the barium (Ba) content in the porous alumina into the BaO content. These provisions are obtained by taking into account the following: in the prepared porous alumina, each added amount is measured as the amount of silicon and barium elements by an X-ray fluorescence analyzer, rather than being measured as the added amount of silica and barium oxide; in addition, it can also be imagined that a part of the added silica enters the alumina skeleton as silicon, and that the added silica and barium oxide form an aluminate phase through a solid phase reaction with alumina.
[0032] According to the porous alumina of the first feature mentioned above, within the range of the SiO2 addition rate being below 3 mass %, the BaO addition rate being below 14 mass %, the solid acid amount is below the reference solid acid amount, and the SiO2 addition rate and the BaO addition rate are set so that the specific surface area after heat treatment at 1200°C for 30 hours becomes above the reference specific surface area. Therefore, based on the reasons described below, a porous alumina having better heat resistance and anti-coking properties can be obtained compared to the porous alumina to which only silica is added.
[0033] First, the reason why porous alumina having SiO2 addition rate and BaO addition rate of 3 mass % and 0 mass %, respectively, was used as a reference porous alumina for evaluating heat resistance and coking resistance is described below.
[0034] Figure 3 The results show that for a steam reforming reaction, a porous alumina carrier with a SiO2 addition rate in the range of 0.5 mass % to 20 mass % and a BaO addition rate of 0 mass % was used as a steam reforming catalyst loaded with Ni (15 mass %) and La (10 mass % calculated as La2O3) and the amount of coking was evaluated.
[0035] The porous alumina was prepared in the same manner as a comparative sample having a BaO addition ratio of 0 mass % prepared by a kneading method described later.
[0036] The steam reforming catalyst was prepared by the impregnation method according to the following principles. The porous alumina was immersed in a mixed aqueous solution of nickel nitrate and lanthanum nitrate at room temperature for 1 hour, evaporated to dryness using an evaporator, and then calcined at 450°C for 5 hours. The powder catalyst loaded with Ni-La was pressed and molded using a press, and then crushed in a mortar until it became granular, and sieved to size 180 μm or more and 250 μm or less.
[0037] The steam reforming reaction was carried out according to the following procedures. 0.5 ml of the catalyst was weighed in a measuring bucket and placed in a stainless steel reaction tube. The catalyst was pre-treated by reduction treatment at 600°C in a hydrogen flow for 1 hour. Thereafter, the steam reforming reaction was carried out at flow rates of C3H8: 60 ml / min, N2: 60 ml / min, H2: 6 ml / min, and H2O: 360 ml / min. The reaction conditions at this time were S / C = 2.0, SV = 60000 h -1 The temperature was raised from room temperature at a rate of 10°C / min and maintained at 600°C for 43 minutes. The generated gas was sampled every 100°C from 400°C and the composition of the generated gas was analyzed by gas chromatography.
[0038] The amount of coking was measured using a carbon-sulfur analyzer (manufactured by LECO Japan United Co., Ltd.: CS-200). A sample of 0.03 g of a catalyst sample that had undergone a steam reforming reaction and 1 g of a combustion-supporting material (tin-plated copper) was placed in a crucible, and oxygen was used as a carrier gas (flow rate 3 L / min) in a high-frequency combustion furnace to burn the carbon in the sample. The carbon content was measured by detecting the vaporized carbon by infrared absorption through high-temperature combustion.
[0039] Figure 4 As shown in the figure, use Figure 3 The phase transition temperature to the α phase was measured using five samples of porous alumina (denoted by ●) having an SiO2 addition rate in the range of 0 mass % to 5 mass % and a BaO addition rate of 0 mass % prepared by the same preparation method as the porous alumina for steam reforming catalyst, and one sample of porous alumina (denoted by ○) having an SiO2 addition rate of 1 mass % and a BaO addition rate of 5 mass % prepared by the kneading method described later and in the same manner as the evaluation sample.
[0040] The phase transition temperature was measured by placing 20 mg of the sample in a Pt dish using a thermogravimetric measuring device (Rigaku, differential thermal balance, Therrmo plus EVO2TG-DTA TG8120) and heating the sample from room temperature at a rate of 20°C / min. An exothermic reaction was observed when alumina transformed from δ and θ-alumina to α-alumina. Therefore, the exothermic peak temperature of the differential thermal analysis (DTA) curve was obtained as the phase transition temperature.
[0041] according to Figure 3 The measurement results of the coking amount shown show that when the SiO2 addition rate is below 3 mass%, almost no coking occurs. In contrast, if the SiO2 addition rate increases and exceeds 3 mass%, the coking amount increases roughly in proportion to the SiO2 addition rate.
[0042] Depend on Figure 4 The measurement results of the phase transition temperature shown show that when the BaO addition rate is 0 mass%, the phase transition temperature increases to 1201°C, 1282°C, 1290°C, 1396°C, and 1416°C as the SiO2 addition rate increases to 0 mass%, 1 mass%, 2 mass%, 3 mass%, and 5 mass%. As the SiO2 addition rate increases, the heat resistance improves. Here, when the SiO2 addition rate increases from 0 mass% to 3 mass%, the phase transition temperature increases from 1201°C to 1396°C, an increase of 195°C. In contrast, when the SiO2 addition rate increases from 3 mass% to 5 mass%, the phase transition temperature increases from 1396°C to 1416°C, an increase of only 20°C. Therefore, the improvement effect of heat resistance accompanying the increase in the SiO2 addition rate is significant when the SiO2 addition rate is 3 mass% or less. Figure 4 The measurement results are consistent with the above Figure 1 The relationship shown is consistent.
[0043] On the other hand, if two samples with SiO2 addition rate of 1 mass% and BaO addition rate of 0 mass% and 5 mass% are compared, it can be seen that if the BaO addition rate increases from 0 mass% to 5 mass%, the phase transition temperature increases from 1282°C to 1411°C, which is 129°C.
[0044] Depend on Figure 3 and Figure 4 The measurement results shown show that the heat resistance can be greatly improved by suppressing the increase in coking amount by suppressing the SiO2 addition rate to below 3 mass% and setting the BaO addition rate within a prescribed appropriate range including 5 mass% when the SiO2 addition rate is below 3 mass%.
[0045] As can be seen from the above description, the porous alumina (benchmark porous alumina) with SiO2 addition rate and BaO addition rate of 3% by mass and 0% by mass, respectively, has temporary heat resistance and coking resistance. However, if the SiO2 addition rate is lower than 3% by mass, the heat resistance decreases, and conversely, if the SiO2 addition rate increases to more than 3% by mass, the coking resistance decreases, so the SiO2 addition rate of 3% by mass is a special point that can take into account both heat resistance and coking resistance. In other words, it is essentially impossible for the porous alumina to which only silica is added to have heat resistance and coking resistance that exceed the benchmark porous alumina. Therefore, in the porous alumina to which both silica and barium oxide are added, when achieving improvements in both heat resistance and coking resistance, the benchmark porous alumina can be said to be suitable as an evaluation benchmark for heat resistance and coking resistance relative to the porous alumina to which only silica is added.
[0046] The effect of improving heat resistance by adding barium oxide in addition to silicon dioxide can be explained as follows.
[0047] The ionic radius of Si is roughly the same as that of aluminum (Al), and Si ions are incorporated into the structure of γ-alumina by decomposing the alumina precursor at around 450°C. In γ-alumina with a spinel structure, there are a large number of vacancies at the octahedral site. By adding Si ions to alumina, the Al ions at the tetrahedral site are replaced by Si ions, and the total number of vacancies is reduced, so alpha is suppressed and heat resistance is improved. In addition, the addition of silica is effective in preventing the clogging of alumina micropores, and shows an effect of improving heat resistance in the temperature range below 1100°C.
[0048] It is known that Ba ions exist as aluminates (barium hexaaluminate: BaO·6Al2O3, barium aluminate: BaO·Al2O3) through solid phase reaction with alumina at high temperatures above 1000°C (refer to Fig. 9 and Fig.10 ). Aluminate is generated on the surface of alumina particles, which inhibits the alpha transformation inside the alumina particles. The aluminate on the particle surface is a cubic crystal (fcc) and has the same structure as γ-alumina, so it shares the oxygen ions on the surface of the alumina particles and interacts strongly. With this interaction, the alpha transformation inside the alumina particles is inhibited.
[0049] When Ba is added to alumina alone, aluminate needs to be generated based on a solid phase reaction. For this purpose, calcination at 1000°C or above is required. During the heating process before aluminate generation, alpha formation is not suppressed, the micropores of alumina disappear, and the specific surface area is greatly reduced. However, alumina in which silica coexists can suppress the clogging of micropores and the reduction of specific surface area in the temperature range below 1100°C during the heating process before aluminate generation by utilizing the effect of silica addition. In addition, at high temperatures above this temperature range, aluminate is generated through the solid phase reaction of Ba, which can suppress the alpha formation of alumina.
[0050] In addition, at a given SiO2 addition rate of 3 mass % or less, if the BaO addition rate is increased from 0 mass % within a range of 14 mass % or less, the specific surface area after heat treatment at 1200°C for 30 hours increases to be higher than the reference specific surface area, and if the maximum value is exceeded, the specific surface area decreases toward the reference specific surface area, as described later, and this point has been confirmed by the inventors of the present application through intensive research (refer to Fig.11 and Fig.14 ). Therefore, within the range of SiO2 addition rate of 3 mass % or less and the range of BaO addition rate of 14 mass % or less, the specific surface area after heat treatment at 1200°C for 30 hours is taken as the reference specific surface area or more. In other words, there is a combination of SiO2 addition rate and BaO addition rate that improves the heat resistance compared with the reference porous alumina (SiO2 addition rate: 3 mass %, BaO addition rate: 0 mass %), and the heat resistance is indeed improved by adopting this combination.
[0051] In addition, the following Fig.13 and Fig.15 The relationship between the SiO2 addition rate and the BaO addition rate and the amount of solid acid shown in the figure shows that, at a given SiO2 addition rate of less than 3% by mass, if the BaO addition rate is increased, the amount of solid acid decreases monotonically (solid acidity decreases). Therefore, as mentioned above, if the solid acidity of the porous carrier increases, coking is likely to occur. Therefore, by suppressing the SiO2 addition rate to less than 3% by mass and then increasing the BaO addition rate, the increase in the amount of coking can be further suppressed, and the anti-coking property is improved. In other words, if a combination of the SiO2 addition rate and the BaO addition rate with improved heat resistance is adopted, the anti-coking property is also improved reliably.
[0052] Therefore, when only silica is added, it is difficult to achieve both heat resistance and anti-coking properties. However, by reducing the amount of silica added and adding barium oxide in addition to silica, both heat resistance and anti-coking properties can be greatly improved compared to the case where only silica is added.
[0053] In addition, the porous alumina of the first characteristic mentioned above is preferably such that the silicon dioxide and the barium oxide are respectively added to the alumina in a range where the SiO2 addition rate is greater than 0.7 mass % and less than 3 mass %, so that the specific surface area of the porous alumina is greater than the reference specific surface area.
[0054] In addition, the porous alumina of the first characteristic is preferably such that the BaO addition rate is within the range of 0.5 mass % to 14 mass %, and the silicon dioxide and the barium oxide are respectively added to the alumina in such a manner that the specific surface area of the porous alumina is greater than the reference specific surface area.
[0055] According to a preferred embodiment of the porous alumina of the above-mentioned first feature, a combination of SiO2 addition rate and BaO addition rate that improves both heat resistance and coking resistance more surely exists within the range of SiO2 addition rate being greater than 0.7 mass % and less than 3 mass %, or within the range of BaO addition rate being greater than 0.5 mass % and less than 14 mass %.
[0056] In addition, in the porous alumina of the first characteristic, when the SiO2 addition rate is Xs (mass %) and the BaO addition rate is Xb (mass %),
[0057] 0.7 mass%≤Xs<1 mass%, and 5 mass%≤Xb≤10 mass%, or 1 mass%≤Xs<2 mass%, and 3 mass%≤Xb≤10 mass%, or 2 mass%≤Xs≤3 mass%, and 1 mass%≤Xb≤14 mass%, and this is taken as the second feature.
[0058] The porous alumina of the present invention is a porous alumina obtained by adding silicon dioxide (SiO2) and barium oxide (BaO) to alumina (Al2O3).
[0059] The SiO2 addition rate (mass %) defined by the ratio of the SiO2 addition amount to the total mass of the alumina and the SiO2 addition amount is set to Xs (mass %), wherein the SiO2 addition amount is the amount obtained by converting the silicon (Si) content in the porous alumina into the SiO2 content,
[0060] The BaO addition rate (mass %) defined by the ratio of the BaO addition amount to the total mass of the alumina and the SiO2 addition amount is denoted as Xb (mass %), wherein the BaO addition amount is the amount obtained by converting the content of barium (Ba) in the porous alumina into the content of BaO,
[0061] 0.7 mass%≤Xs<1 mass%, and 5 mass%≤Xb≤10 mass%, or 1 mass%≤Xs<2 mass%, and 3 mass%≤Xb≤10 mass%, or 2 mass%≤Xs≤3 mass%, and 1 mass%≤Xb≤14 mass%, and this is taken as the third feature.
[0062] The porous alumina according to the second or third characteristics mentioned above can reliably improve both the heat resistance and the anti-coking properties as compared with the benchmark porous alumina (SiO2 addition rate: 3 mass %, BaO addition rate: 0 mass %) within the specified ranges of the SiO2 addition rate Xs and the BaO addition rate Xb.
[0063] In the porous alumina having the second or third characteristic, preferably, 1 mass % ≤ Xs ≤ 3 mass %, and 3 mass % ≤ Xb ≤ 10 mass %.
[0064] According to a preferred embodiment of the porous alumina having the second or third characteristic, both heat resistance and coking resistance can be further improved.
[0065] Furthermore, the catalyst of the present invention is characterized by comprising porous alumina having the first or second characteristic and a catalyst substance supported on the porous alumina.
[0066] The catalyst having the above characteristics can have improved heat resistance and coking resistance compared to a catalyst using conventional porous alumina as a carrier.
[0067] Effects of the Invention
[0068] The porous alumina according to the present invention has high heat resistance that can maintain a large specific surface area even at high temperatures by using barium oxide as a solid basic oxide and appropriately adjusting the addition amounts of silicon dioxide and barium oxide, and suppressing the addition amount of silicon dioxide, thereby suppressing the increase in the amount of solid acid, thereby achieving high coking resistance, thereby providing a high-performance porous alumina having excellent heat resistance and coking resistance. In addition, by using the porous alumina as a catalyst carrier, a catalyst having excellent heat resistance and coking resistance can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1 This is a graph showing the relationship between the SiO2 addition rate and the specific surface area of porous alumina to which only silicon dioxide is added under three different heat treatment conditions.
[0070] Figure 2 This is a graph showing the measurement results of the SiO2 addition rate, the solid acid amount, and the solid alkali amount of porous alumina to which only silicon dioxide is added.
[0071] Figure 3 This is a graph showing the results of measuring the SiO 2 addition rate and the coke amount in a steam reforming catalyst in which Ni—La is supported on porous alumina to which only silicon dioxide is added.
[0072] Figure 4 This is a graph showing the measurement results of the phase transition temperature to the α phase in porous alumina to which only silicon dioxide is added and porous alumina to which silicon dioxide and barium oxide are added.
[0073] Figure 5 This is a process transition diagram showing an outline of a method for producing the porous alumina of the present invention by a kneading method.
[0074] Figure 6 This is a process transition diagram showing an outline of a method for producing the porous alumina of the present invention by the first type of impregnation method.
[0075] Figure 7 This is a process transition diagram showing an outline of a method for producing the porous alumina of the present invention by the second impregnation method.
[0076] Figure 8 This is a graph showing the measurement results of the specific surface areas of evaluation samples and comparative samples prepared by a kneading method under three different heat treatment conditions.
[0077] Fig. 9 The graphs are XRD diffraction patterns showing the crystal structures of performance evaluation samples and comparative samples prepared by a kneading method under three different heat treatment conditions.
[0078] Fig.10 It means performance Fig. 9 The XRD diffraction pattern of the crystal structure of the evaluation sample is shown.
[0079] Fig.11 This is a table showing the measurement results of the specific surface areas of a plurality of evaluation samples and comparative samples prepared by a kneading method and having different SiO2 addition rates and BaO addition rates after heat treatment at 1200°C for 30 hours.
[0080] Fig.12 This is a graph showing the measurement results of the solid acid amount and the solid base amount of the evaluation sample and the comparative sample prepared by the kneading method.
[0081] Fig.13 This is a graph showing the results of measuring the solid acid content of a plurality of evaluation samples and comparative samples having different SiO2 addition rates and BaO addition rates prepared by a kneading method.
[0082] Fig.14This is a table showing the measurement results of the specific surface areas of a plurality of evaluation samples and comparative samples having different SiO2 addition rates and BaO addition rates prepared by the first type of impregnation method after heat treatment at 1200°C for 30 hours.
[0083] Fig.15 This is a graph showing the results of measuring the solid acid content of a plurality of evaluation samples and comparative samples having different SiO2 addition rates and BaO addition rates prepared by the first type impregnation method.
[0084] Fig.16 This is a process transition diagram showing an outline of the method for producing the porous alumina of the present invention by a precipitation method. DETAILED DESCRIPTION
[0085] A preferred embodiment of the porous alumina of the present invention (hereinafter referred to as “the present embodiment” as appropriate) will be described.
[0086] The porous alumina of the present embodiment (hereinafter, appropriately referred to as "the present alumina") is a porous alumina obtained by adding two oxides, silicon dioxide (SiO2) and barium oxide (BaO), to aluminum oxide (aluminum oxide, Al2O3). In the following description, "the present alumina" is aluminum oxide to which silicon dioxide and barium oxide are added, and when simply referred to as "alumina", it is aluminum oxide to which silicon dioxide and barium oxide are not added.
[0087] [1] The preparation method of the aluminum oxide:
[0088] Next, the preparation method of the present aluminum oxide is described. The preparation method of the present aluminum oxide is basically composed of the following steps: a step for adding silicon dioxide to aluminum oxide; a step for adding barium oxide to aluminum oxide. The preparation method may be an impregnation method, a kneading method, a precipitation method, a sol-gel method, etc., depending on the step for adding barium oxide. However, in the present embodiment, the kneading method and the impregnation method are used in the preparation of samples for evaluating the heat resistance and coking resistance of the present aluminum oxide.
[0089] Before explaining the details of the kneading method and the impregnation method, the addition rates of silicon dioxide and barium oxide added to the alumina in this embodiment are defined as follows: The units of the following SiO2 addition rate and BaO addition rate are "mass %".
[0090] SiO2 addition rate = SiO2 addition amount / (mass of alumina + SiO2 addition amount) × 100
[0091] BaO addition rate = BaO addition amount / (mass of alumina + SiO2 addition amount) × 100
[0092] The amount of SiO2 added is the amount of Si content in the present alumina converted into the amount of SiO2 content, and the amount of BaO added is the amount of Ba content in the present alumina converted into the amount of BaO content. The Si content is the total Si content present in the present alumina as a monomer and a compound, and the Ba content is the total Ba content present in the present alumina as a monomer and a compound.
[0093] In the present embodiment, the reference mass used as the calculation standard for the SiO2 addition rate and the BaO addition rate does not include the BaO addition amount because, in the preparation method of the present alumina shown below, it is convenient to unify the setting of the SiO2 addition rate and the BaO addition rate into (mass of alumina + SiO2 addition amount). The above-mentioned SiO2 addition rate and BaO addition rate can be easily converted into addition rates based on the reference mass including the BaO addition amount. In addition, as needed, the unit of each addition rate can also be converted from "mass %" to "mole %".
[0094] [1.1] Preparation of the present aluminum oxide by kneading method:
[0095] like Figure 5 As shown, the method for preparing the present aluminum oxide by a kneading method, if roughly divided, comprises the following steps: a step of mixing an alkoxysilane solution containing an alkoxysilane, a mixed solvent containing water and an alcohol, and an inorganic acid with an aluminum solution containing an aluminum compound and water to prepare a mixed solution in which the aluminum compound and the alkoxysilane are dissolved in the mixed solvent (step #K1); a step of co-precipitating aluminum hydroxide and a silicon compound in the mixed solvent to form a precipitate (step #K2); a step of adding an aqueous solution of a barium compound to the precipitate and kneading the precipitate (step #K3); a step of drying and calcining the precipitate kneaded with the barium compound to form a porous aluminum oxide (the present aluminum oxide) containing aluminum oxide, silicon dioxide and barium oxide (step #K4).
[0096] The alkoxysilane contained in the alkoxysilane solution of step #K1 is preferably tetraethoxysilane (hereinafter referred to as "TEOS"), the alcohol is preferably ethanol, and the inorganic acid is preferably hydrochloric acid or nitric acid, but is not limited to these.
[0097] The aluminum solution in step #K1 is preferably prepared by dissolving aluminum nitrate in water or aluminum hydroxide in an aqueous nitric acid solution from the viewpoint of improving heat resistance.
[0098] The mixing ratio of the alkoxysilane and the aluminum compound in the mixed solution prepared in step #K1 is adjusted so that the addition rate of silicon dioxide (SiO2 addition rate) in the porous alumina formed in step #K3 becomes a desired value.
[0099] The alkoxysilane and the aluminum compound in the mixed solution prepared in step #K1 are uniformly dissolved in the mixed solvent composed of water and alcohol. In other words, the mixed solution does not undergo phase separation but forms a single liquid phase.
[0100] In step #K2, the acidic mixed solution is preferably heated to 40°C to 100°C (for example, heated to 100°C while refluxed) while adding a precipitant containing an alkaline compound. By adding the alkaline compound until the pH value of the mixed solution reaches about 8 (for example, 8 to 8.5), aluminum hydroxide and the silicon compound are co-precipitated. The silicon compound contained in the precipitate generated by the co-precipitation may be an alkoxysilane or a hydrolysis condensate thereof.
[0101] The precipitating agent contains, for example, at least one basic compound selected from the group consisting of aqueous ammonia, sodium hydroxide, potassium hydroxide and urea, of which aqueous ammonia is preferred.
[0102] In step #K3, for example, the precipitate is preferably taken out from the mixed solution by a common method such as filtration, and washed with water (distilled water) at room temperature. An aqueous solution of a barium compound is added to the washed precipitate and kneaded. In addition, the aqueous solution of the barium compound is preferably prepared by dissolving barium nitrate in water to prepare a barium nitrate aqueous solution, or by dissolving barium hydroxide in water to prepare a barium hydroxide aqueous solution.
[0103] In step #K4, for example, the precipitate kneaded with the barium compound is dried for a predetermined time in a drier at 150°C, and then the dried precipitate is pulverized in a mortar or the like to be powdered. The dried and powdered precipitate is fired in air at 1000°C for 5 hours, for example, to form porous alumina (present alumina) containing alumina, silica and barium oxide. In the formed porous alumina, the alumina is mainly composed of intermediate aluminas such as γ-alumina and θ-alumina.
[0104] [1.2] Preparation of the present alumina by impregnation method:
[0105] There are two types of preparation methods for the present alumina by impregnation method: a first impregnation method in which silica and barium oxide are added to existing porous alumina by impregnation method to prepare the present alumina; and a second impregnation method in which silica-added porous alumina is prepared by adding silica to alumina, and barium oxide is added to the silica-added porous alumina by impregnation method to prepare the present alumina.
[0106] [1.2.1] Type I immersion method:
[0107] like Figure 6As shown, the first type of impregnation method, if roughly divided, is composed of the following steps: a step of impregnating an existing porous alumina (Al2O3 powder) with an alkoxysilane solution and an aqueous solution of a barium compound (step #I11); a step of drying and calcining the porous alumina impregnated with the alkoxysilane solution and the aqueous solution of a barium compound to form a porous alumina (primary alumina) containing aluminum oxide, silicon dioxide and barium oxide (step #I12).
[0108] The ready-made porous alumina used in step #I11 is a porous alumina mainly composed of intermediate aluminas such as γ-alumina and θ-alumina. For example, in the examples of the present embodiment, as the ready-made porous alumina, C20 manufactured by Nippon Light Metal is used, but it is not limited to the porous alumina manufactured by Nippon Light Metal, and it may be independently prepared. In addition, the alkoxysilane contained in the alkoxysilane solution of step #I11 is preferably TEOS, as in step #K1 of the kneading method. In addition, the aqueous solution of the barium compound in step #I11 is preferably prepared by dissolving barium nitrate in water as a barium nitrate aqueous solution, or by dissolving barium hydroxide in water as a barium hydroxide aqueous solution, as in step #K3 of the kneading method.
[0109] In step #I12, the porous alumina impregnated with an alkoxysilane solution and an aqueous solution of a barium compound is dried, for example, at 150°C in air or using a rotary evaporator, and then calcined, for example, at 1000°C in air for 5 hours to obtain a porous alumina (present alumina) containing aluminum oxide, silicon dioxide and barium oxide.
[0110] [1.2.2] Second type of immersion method:
[0111] like Figure 7 As shown, the second type of impregnation method, if roughly divided, is composed of the following steps: a step of mixing an alkoxysilane solution containing alkoxysilane, a mixed solvent containing water and alcohol, and an inorganic acid with an aluminum solution containing an aluminum compound and water to prepare a mixed solution in which the aluminum compound and the alkoxysilane are dissolved in the mixed solvent (step #I21); a step of co-precipitating aluminum hydroxide and a silicon compound in the mixed solvent to form a precipitate (step #I22); a step of drying and calcining the precipitate to form a porous alumina containing aluminum oxide and silicon dioxide (silicon dioxide added porous alumina) (step #I23); a step of impregnating the silica added porous alumina with an aqueous solution of a barium compound (step #I24); a step of drying and calcining the silica added porous alumina impregnated with an aqueous solution of a barium compound to form a porous alumina containing aluminum oxide, silicon dioxide and barium oxide (primary alumina) (step #I25).
[0112] Step #I21 and step #I22 of the second type of impregnation method are basically the same as step #K1 and step #K2 of the kneading method described above, and repeated description is omitted. In addition, the preparation method of silica-added porous alumina in steps #I21 to #I23 is the same as the preparation method of the comparative sample with a BaO addition rate of 0 mass% based on the kneading method described later, except that the sintering temperature of step #K4 is different from that of step #I23.
[0113] Furthermore, in the second type of impregnation method, the silica-added porous alumina used in step #I24 may be replaced by readily available silica-added porous alumina instead of the porous alumina prepared in steps #I21 to #I23.
[0114] In step #I23, the precipitate is preferably taken out from the mixed solution by a common method such as filtration, and washed with room temperature water (distilled water). The precipitate is dried to remove most of the solvent, and then pulverized in a mortar or the like to powder.
[0115] The dried and powdered precipitate is fired to form silica-added porous alumina. Alumina constituting the silica-added porous alumina is mainly composed of intermediate alumina such as γ-alumina and θ-alumina.
[0116] The calcination temperature is preferably 400 to 1000° C. If the calcination temperature is too high, the aluminum oxide will undergo a transformation into the α phase, and the specific surface area may decrease. The calcination time is preferably about 1 hour to several tens of hours.
[0117] In step #I24, similarly to step #K3 of the kneading method, the aqueous solution of the barium compound is preferably prepared by dissolving barium nitrate in water to form a barium nitrate aqueous solution, or by dissolving barium hydroxide in water to form a barium hydroxide aqueous solution.
[0118] In step #I25, similarly to step #I12 of the first type of impregnation method, the silica-added porous alumina impregnated with an aqueous solution of a barium compound is dried, for example, at 150°C in air or using a rotary evaporator, and then calcined, for example, at 1000°C in air for 5 hours to obtain a porous alumina (present alumina) containing alumina, silica and barium oxide.
[0119] The alumina prepared by the kneading method, the first or second type impregnation method is mainly composed of intermediate alumina such as γ-alumina and θ-alumina. In addition, the alumina is, as an example, a powder obtained by crushing secondary particles of needle-shaped or fibrous primary particles and sieving them to a predetermined particle size range (for example, 100 μm to 500 μm). In addition, the alumina can be in various shapes such as granular, disc-shaped, honeycomb, etc. in addition to powder.
[0120] In the kneading method, the first or second type of impregnation method, the amount of silicon and barium added to alumina is determined by the amount of each solution added. In other words, the total amount of silicon and barium in the solution is added to alumina after the added solution is evaporated to dryness, so the above-mentioned SiO2 addition rate and BaO addition rate are uniquely determined by the mass of a given alumina or the amount of alkoxysilane solution used and the amount of each solution added.
[0121] [2] Evaluation of heat resistance and anti-coking properties of the alumina prepared by the kneading method:
[0122] [2.1] Preparation of evaluation samples and comparative samples:
[0123] Evaluation samples, through Figure 5 The kneading method shown is prepared according to the following instructions.
[0124] As the alkoxysilane solution of step #K1, 7.52 g of ethanol was added to 5.00 g of TEOS, and the mixture was stirred at room temperature for 5 minutes. Then, 1.25 g of hydrochloric acid (37% by mass) was added, and the mixture was stirred at room temperature for another 5 minutes. 71.23 g of water was added to the mixed solution to obtain a transparent and uniform 5.88% by mass TEOS solution.
[0125] In step #K1, the TEOS solution obtained according to the above method is added to a specified amount of 20 mass % aluminum nitrate aqueous solution to obtain a uniform mixed solution. Use the required amount of TEOS solution and aluminum nitrate aqueous solution as the target SiO2 addition rate. Heat this mixed solution to reflux, drip 28 mass % ammonia water and stir until the pH value reaches 8.5. As the ammonia water is dripped, aluminum hydroxide and silicon compounds co-precipitate to form a precipitate in the solution. For this precipitate, use No.1 filter paper to filter out the precipitate by suction filtration. Wash this precipitate with distilled water. Add a specified amount of barium nitrate aqueous solution to the washed precipitate and mix it. Then dry it in a dryer at 150°C for 20 hours. Crush the dried precipitate with a mortar and sinter it at 1000°C in air for 5 hours to obtain a sample for evaluation of this alumina.
[0126] As samples for comparison, three types of comparative samples were prepared, namely, only SiO2 addition rate was 0 mass%, only BaO addition rate was 0 mass%, and both SiO2 addition rate and BaO addition rate were 0 mass%. The evaluation samples and comparative samples were represented by symbols SK (Xs, Xb). Xs represents the SiO2 addition rate (mass %), and Xb represents the BaO addition rate (mass %).
[0127] The comparative sample with Xs=0 mass % was prepared in step #K1 by using a blank solution not containing TEOS (a solution containing ethanol and hydrochloric acid whose concentration was adjusted with water) instead of the TEOS solution. The comparative sample with Xb=0 mass % was prepared in step #K3 by omitting the step of adding an aqueous solution of a barium compound to the precipitate after suction filtration and water washing and kneading.
[0128] [2.2] Sample evaluation method:
[0129] The specific surface area of each sample was measured by the nitrogen adsorption BET method under the following three heat treatment conditions using a fully automatic gas adsorption measuring device (BELSORP-max manufactured by MicrotracBEL). The first heat treatment condition is the state before the other two heat treatments are implemented (before heat treatment). The second heat treatment condition is to increase the temperature from room temperature to 1200°C at 10°C / min, stop heating, and maintain the temperature at 1200°C for 5 hours (5 hours at 1200°C). The third heat treatment condition is to increase the temperature from room temperature to 1200°C at 10°C / min, stop heating, and maintain the temperature at 1200°C for 30 hours (30 hours at 1200°C).
[0130] The crystal structure of each sample was measured by irradiating Cukα with an X-ray diffraction device (ULTIMA III manufactured by Rigaku) and using a two-dimensional high-speed detector. The amount of Al, Si and Ba in each sample was analyzed by the glass bead method using an X-ray fluorescence analyzer (Superrmini manufactured by Rigaku). The amount of solid acid and base in each sample was measured by the temperature rise desorption method (TPD, base probe molecule: NH3, acid probe molecule: CO2) using a catalyst evaluation device (BELCAT manufactured by MicrotracBEL).
[0131] The evaluation method of the sample is the same as that in the evaluation of the heat resistance and coking resistance of the present alumina prepared by the first type of impregnation method described later.
[0132] [2.3] Evaluation results of heat resistance:
[0133] Figure 8 The graph shows the results of measuring the specific surface area of one evaluation sample and five comparative samples prepared by the kneading method before heat treatment, at 1200°C for 5 hours, and at 1200°C for 30 hours. The evaluation sample and comparative sample used were SK(1,7), SK(0,0), SK(1,0), SK(3,0), SK(5,0), and SK(0,7).
[0134] exist Fig. 9Shown in the figure are XRD diffraction patterns showing the crystal structure of one evaluation sample and three comparative samples prepared by the kneading method before heat treatment, at 1200°C for 5 hours, and at 1200°C for 30 hours. The evaluation sample and comparative sample used were SK(1,7), SK(0,0), SK(1,0), and SK(0,7). Fig.10 In Fig. 9 The XRD diffraction patterns of the evaluation sample SK(1,7) under three heat treatment conditions are shown in one figure.
[0135] Fig.11 The results are shown in Figure 1, which show the results of measuring the specific surface area after heat treatment at 1200°C for 30 hours for evaluation samples and comparative samples prepared by the kneading method with increasing the number of samples. The number of samples is 90 for evaluation and 24 for comparative samples, and the ranges of SiO2 addition rate and BaO addition rate cover a wide range of 0≤Xs≤30 and 0≤Xb≤100.
[0136] according to Figure 8 In the comparative sample SK(0,7) to which only barium oxide was added, no significant increase in specific surface area due to the addition of barium oxide was observed compared with the sample to which silicon dioxide was added, regardless of the heat treatment conditions. However, after heat treatment at 1200°C for 5 hours, the specific surface area of the evaluation sample SK(1,7) was improved compared with the comparative samples SK(1,0) and SK(0,7). In addition, after heat treatment at 1200°C for 30 hours, the evaluation sample SK(1,7) was able to maintain a larger specific surface area than the comparative samples SK(1,0) and SK(0,7), confirming that the mixed addition of silicon dioxide and barium oxide was effective in improving heat resistance. In addition, after heat treatment at 1200°C for 5 hours and at 1200°C for 30 hours, it was confirmed that the specific surface area of the evaluation sample SK(1,7) was improved compared with the comparison sample SK(3,0). Even if the SiO2 addition rate was reduced from 3 mass % to 1 mass %, by adding an appropriate amount of barium oxide, a specific surface area greater than the specific surface area of the comparison sample (equivalent to the comparison benchmark porous alumina) to which only 3 mass % silica was added (equivalent to the benchmark specific surface area) could be obtained.
[0137] according to Fig. 9 (A) Before heat treatment, the peaks of θ-Al2O3 and γ-Al2O3 can be confirmed in SK(0,0) and SK(1,0), and the peaks of γ-Al2O3 and barium aluminate (BaO·Al2O3) can be confirmed in SK(0,7) and SK(1,7). Fig. 9(B) After heat treatment at 1200°C for 5 hours, complete transformation to α-Al2O3 can be confirmed in SK(0,0) and SK(1,0), and in addition to the peak of α-Al2O3, peaks of monobarium aluminate and barium hexaaluminate (BaO·6Al2O3) can be confirmed in SK(0,7) and SK(1,7). Fig. 9 (C) After heat treatment at 1200℃ for 30 hours, the same product as that after heat treatment at 1200℃ for 5 hours can be seen. However, the peak intensity of α-Al2O3 of SK(1,7) is lower than that of other comparative samples. Figure 8 As shown, even after heat treatment at 1200°C for 30 hours, the coexistence of silicon dioxide and barium oxide can suppress the generation of α-Al2O3 due to the high specific surface area, which is known to contribute to heat resistance.
[0138] Depend on Fig.11 It can be seen that within the range of SiO2 addition rate Xs being 0.7 mass % or more and 3 mass % or less and BaO addition rate Xb being 0.5 mass % or more and 14 mass % or less, even after heat treatment at 1200°C for 30 hours, the first effective range of SiO2 addition rate Xs and BaO addition rate Xb having a specific surface area greater than the specific surface area (equivalent to the reference specific surface area) of the comparative sample SK (3,0) equivalent to the reference porous alumina exists in a wide range ( Fig.11 In addition, at the same SiO2 addition rate Xs, if the BaO addition rate Xb increases from 0.5 mass%, the specific surface area exceeds the reference specific surface area and reaches a maximum value, and then decreases to below the reference specific surface area. Here, it can be seen that the range of BaO addition rate Xb where the specific surface area is above the reference specific surface area becomes wider as the SiO2 addition rate Xs increases.
[0139] Depend on Fig.11It can be seen that, according to the SiO2 addition rate Xs, by setting the BaO addition rate Xb as shown below, the specific surface area after heat treatment at 1200°C for 30 hours can be maintained or increased within the range of 1 to 1.724 times relative to the reference porous alumina. Even if the SiO2 addition rate Xs is reduced from 3 mass% to 0.7 mass%, and the BaO addition rate Xb is in the range of 5 mass% ≤ Xb ≤ 10 mass%, the specific surface area is still 1 to 1.034 times the reference specific surface area, and the heat resistance substantially equivalent to that of the reference porous alumina can be achieved. In addition, even if the SiO2 addition rate Xs is reduced from 3 mass% to 1 mass%, and the BaO addition rate Xb is in the range of 3 mass% ≤ Xb ≤ 10 mass%, the specific surface area is still 1 to 1.414 times the reference specific surface area, and the heat resistance substantially equivalent to or higher than that of the reference porous alumina can be achieved. In addition, even if the SiO2 addition rate Xs is reduced from 3 mass% to 2 mass%, and the BaO addition rate Xb is in the range of 1 mass% ≤ Xb ≤ 14 mass%, the year-on-year surface area is still 1 to 1.655 times the reference specific surface area, and the heat resistance substantially equal to or higher than that of the reference porous alumina can be achieved. In addition, when the SiO2 addition rate Xs is 3 mass%, and the BaO addition rate Xb is in the range of 0.5 mass% ≤ Xb ≤ 14 mass%, the year-on-year surface area is 1.207 to 1.724 times the reference specific surface area, and the heat resistance higher than that of the reference porous alumina by more than 20% can be achieved. In particular, when the SiO2 addition rate Xs is in the range of 1 to 3 mass%, and the BaO addition rate Xb is close to 5 mass%, the improvement of the specific surface area of about 1.4 to 1.7 times the reference specific surface area can be achieved, and the heat resistance can be further improved.
[0140] Based on the above, the first effective range of the SiO2 addition rate Xs and the BaO addition rate Xb in which the specific surface area after heat treatment at 1200°C for 30 hours is greater than the reference specific surface area is approximately as follows.
[0141] 0.7 mass%≤Xs<1 mass%, and 5 mass%≤Xb≤10 mass%, or
[0142] 1 mass%≤Xs<2 mass%, and, 3 mass%≤Xb≤10 mass%, or,
[0143] 2 mass %≤Xs≤3 mass %, and 1 mass %≤Xb≤14 mass %.
[0144] However, even outside the first effective range, for example, the specific surface area of the evaluation sample SK(3,0.5) with a SiO2 addition rate Xs of 3 mass% and a BaO addition rate Xb of 0.5 mass% is larger than the reference specific surface area. Fig.11In the vicinity of the thick line frame, the specific surface area after heat treatment at 1200°C for 30 hours may reach or exceed the reference specific surface area.
[0145] [2.4] Evaluation results of anti-coking properties:
[0146] Fig.12 The following table shows the results of measuring the solid acid and solid base content of one evaluation sample and five comparative samples prepared by the kneading method. The evaluation sample and comparative sample used were SK(1,7), SK(0,0), SK(1,0), SK(3,0), SK(5,0), and SK(0,7).
[0147] Fig.13 The results of increasing the number of samples and measuring the solid acid content of the evaluation samples and comparative samples prepared by the kneading method are shown in FIG. 1. The number of samples is 15 for the evaluation samples and 9 for the comparative samples, and the range of the SiO2 addition rate and the BaO addition rate is widely involved in 0≤Xs≤5 and 0≤Xb≤14.
[0148] according to Fig.12 In the comparative sample with BaO addition rate Xb of 0 mass %, Figure 2 The measurement results shown also show that the amount of solid acid increases and the amount of solid alkali decreases as the SiO2 addition rate Xs increases. In contrast, in the evaluation sample SK(1,7) and the comparative sample SK(0,7) added with barium and having a BaO addition rate Xb of 7 mass%, the amount of solid acid decreases and the amount of solid alkali increases compared to the comparative samples SK(1,0) and SK(0,0) having the same SiO2 addition rate Xs. The amount of solid acid in the evaluation sample SK(1,7) decreases to the same level as the amount of solid acid in the comparative sample SK(0,0) having a SiO2 addition rate Xs and a BaO addition rate Xb of 0 mass%.
[0149] Depend on Fig.13 It can be confirmed that, when SiO2 addition rate Xs is in the range of 0 mass % to 5 mass %, when SiO2 addition rate Xs is the same, as BaO addition rate Xb increases from 0 mass % to 14 mass %, the solid acid amount monotonically decreases. It can also be confirmed that, when BaO addition rate Xb is in the range of 0 mass % to 14 mass %, when BaO addition rate Xb is the same, as SiO2 addition rate Xs increases from 0 mass % to 5 mass %, the solid acid amount monotonically increases.
[0150] In addition, by Fig.13It can be seen that when the SiO2 addition rate Xs is below 3 mass% and the BaO addition rate Xb is below 14 mass%, the solid acid amount of the present alumina is lower than the solid acid amount of the comparative sample SK(3,0) corresponding to the benchmark porous alumina, and the anti-coking property is improved relative to the benchmark porous alumina.
[0151] [2.5] Summary of evaluation results:
[0152] Depend on Figure 8 and Fig.12 It was confirmed that the evaluation sample SK(1,7) had an increased specific surface area and a decreased amount of solid acid after heat treatment at 1200°C for 5 hours and 1200°C for 30 hours, respectively, compared with the comparison sample SK(3,0) corresponding to the benchmark porous alumina. It was also confirmed that the mixed addition of silica and barium oxide was effective in improving both heat resistance and anti-coking properties.
[0153] In addition, by Fig.11 and Fig.13 It can be seen that within the range of SiO2 addition rate Xs being below 3% by mass and BaO addition rate Xb being below 14% by mass, the specific surface area of the present alumina after heat treatment at 1200°C for 30 hours is greater than the specific surface area (reference specific surface area) of the comparative sample SK(3,0), and the effective range of SiO2 addition rate Xs and BaO addition rate Xb exists in a wide range where the solid acid amount of the present alumina is less than the solid acid amount of the comparative sample SK(3,0), and it can be confirmed that the mixed addition of silicon dioxide and barium oxide within this effective range is effective for both improving heat resistance and improving anti-coking properties. In addition, this effective range is the first effective range of SiO2 addition rate Xs and BaO addition rate Xb where the specific surface area of the present alumina after heat treatment at 1200°C for 30 hours is greater than the reference specific surface area.
[0154] In addition, by Fig.11 It shows that by narrowing the range of SiO2 addition rate Xs and BaO addition rate Xb to 1 mass % ≤ Xs ≤ 3 mass % and 3 mass % ≤ Xb ≤ 10 mass % relative to the above-mentioned effective range, the specific surface area of the alumina after heat treatment at 1200°C for 30 hours is further increased, and the heat resistance can be further improved while maintaining the anti-coking property.
[0155] [3] Evaluation of heat resistance and anti-coking properties of the present alumina prepared by the first type of impregnation method:
[0156] [3.1] Preparation of evaluation samples and comparative samples:
[0157] As a ready-made porous alumina, C20 manufactured by Nippon Light Metal was used, and as an alkoxysilane solution and an aqueous solution of a barium compound, a TEOS solution and an aqueous solution of barium nitrate in amounts corresponding to the target SiO2 addition rate and BaO addition rate were used, and the above-mentioned treatments of step #I11 and step #I12 were carried out to obtain a sample for evaluation of the present alumina.
[0158] As comparative samples, three types of comparative samples were prepared, one in which only SiO2 addition rate was 0 mass%, one in which only BaO addition rate was 0 mass%, and both SiO2 addition rate and BaO addition rate were 0 mass%. In the above-mentioned step #I11, the comparative sample with SiO2 addition rate of 0 mass% was impregnated without using TEOS solution, and the comparative sample with BaO addition rate of 0 mass% was impregnated without using barium nitrate aqueous solution. The evaluation sample and the comparative sample are represented by the symbol SI (Xs, Xb). Xs represents the SiO2 addition rate (mass%), and Xb represents the BaO addition rate (mass%).
[0159] [3.2] Evaluation results of heat resistance:
[0160] Fig.14 The results shown in FIG. 1 are the results of measuring the specific surface area of the evaluation samples and the comparative samples prepared by the first type of impregnation method after heat treatment at 1200°C for 30 hours. The number of samples is 20 for evaluation and 3 for comparative, and the ranges of the SiO2 addition rate and the BaO addition rate are 0≤Xs≤3 and 0≤Xb≤14.
[0161] Depend on Fig.14 It can be seen that within the range of SiO2 addition rate Xs being 0.7 mass % or more and 3 mass % or less and BaO addition rate Xb being 1 mass % or more and 14 mass % or less, the second effective range of SiO2 addition rate Xs and BaO addition rate Xb, in which the specific surface area is equal to or greater than the specific surface area (equivalent to the reference specific surface area) of the comparative sample SI (3,0) of the reference porous alumina even after heat treatment at 1200°C for 30 hours, exists in a wide range ( Fig.14 The second effective range is the area surrounded by the thick line frame. Fig.11 The first effective range of the evaluation sample prepared by the kneading method is consistent with that shown in FIG. Fig.11 The measurement results shown are consistent: at the same SiO2 addition rate Xs, if the BaO addition rate Xb increases from 1 mass%, the year-on-year surface area exceeds the benchmark specific surface area and reaches a maximum value, and then decreases to a point below the benchmark specific surface area; the range of the BaO addition rate Xb where the year-on-year surface area is above the benchmark specific surface area becomes wider as the SiO2 addition rate Xs increases.
[0162] therefore, Fig.11 The heat resistance of the test samples prepared by the kneading method shown in the figure is as follows: Fig.14 The same is true for the evaluation samples prepared by the first type of immersion method shown.
[0163] [3.3] Evaluation results of anti-coking properties:
[0164] Fig.15 The figure shows the measurement results of the solid acid content of the evaluation samples and the comparative samples prepared by the first type of impregnation method. Regarding the number of samples, there are 12 evaluation samples and 8 comparative samples, and the ranges of SiO2 addition rate and BaO addition rate are 0≤Xs≤5 and 0≤Xb≤20.
[0165] Depend on Fig.15 It can be confirmed that when the SiO2 addition rate Xs is in the range of 0 mass % to 5 mass %, if the SiO2 addition rate Xs is the same, the solid acid amount of the comparative sample with a BaO addition rate Xb of 0 mass % decreases monotonically as the BaO addition rate Xb increases from 0 mass % to 20 mass %. Fig.13 This is consistent with the situation of the evaluation samples prepared by the kneading method shown.
[0166] In addition, by Fig.15 It can be seen that when the SiO2 addition rate Xs is less than 3 mass % and the BaO addition rate Xb is less than 14 mass %, Fig.13 As shown in the evaluation sample prepared by the kneading method, in the present alumina prepared by the first type of impregnation method, the amount of solid acid is also lower than the solid acid amount of the comparative sample SI (3,0) corresponding to the benchmark porous alumina, and the anti-coking property is improved compared with the benchmark porous alumina.
[0167] [3.4] Summary of evaluation results:
[0168] Depend on Fig.14 and Fig.15 It can be seen that Fig.11 and Fig.13Similarly, in the present alumina prepared by the first type of impregnation method, within the range of SiO2 addition rate Xs being 3% by mass or less and BaO addition rate Xb being 14% by mass or less, the specific surface area of the present alumina after heat treatment at 1200°C for 30 hours is greater than the specific surface area (reference specific surface area) of the comparative sample SI (3,0), and the effective range of the SiO2 addition rate Xs and the BaO addition rate Xb in which the solid acid amount of the present alumina is less than the solid acid amount of the comparative sample SI (3,0) exists in a wide range. As a result, it can be confirmed that the mixed addition of silicon dioxide and barium oxide within this effective range is effective for both improving heat resistance and improving anti-coking properties. In addition, this effective range is the second effective range of the SiO2 addition rate Xs and the BaO addition rate Xb in which the specific surface area of the present alumina after heat treatment at 1200°C for 30 hours is greater than the reference specific surface area.
[0169] As described above, regardless of the preparation method, in the same effective range of SiO2 addition rate Xs and BaO addition rate Xb (the same as the first effective range and the second effective range), it is possible to achieve both improved heat resistance and improved anti-coking properties by mixed addition of silica and barium oxide. This helps that the components contained in the sample fired at 1000°C are the same regardless of whether the preparation method is a kneading method or an impregnation method. Moreover, if the sample is fired at 1200°C for a long time, the solid phase reaction of silica and alumina, and barium oxide and alumina begins. As described above, when barium is added alone, the alphaization of γ-alumina will be faster than the formation of barium hexaaluminate, which is the key to inhibiting sintering, because the specific surface area is reduced due to high-temperature heat treatment. In addition, although the addition of silica can delay the alphaization to some extent in the initial stage of sintering, it is a long-term firing at 1200°C after all, and the alphaization cannot be prevented. On the other hand, by adding silica and barium oxide together, silica delays the initial alpha transformation, and then the formation of barium hexaaluminate inhibits the formation of α-alumina, resulting in the maintenance of a high specific surface area. These tendencies can be explained by Figure 8 , Fig. 9 and Fig.10 illustrate.
[0170] [4] Other embodiments of the method for preparing aluminum oxide:
[0171] In the above embodiment, the kneading method, the first and second types of impregnation methods are described as the preparation method of the present aluminum oxide, but the preparation method of the present aluminum oxide is not limited to a specific preparation method as long as it is a preparation method that can accurately control the SiO2 addition rate and the BaO addition rate. As other preparation methods of the present aluminum oxide, preparation methods based on precipitation methods, sol-gel methods, etc. are envisioned. Below, the preparation method using the precipitation method is briefly described.
[0172] [4.1] Preparation of the present aluminum oxide by precipitation method:
[0173] like Fig.16 As shown, the preparation method of the present alumina by precipitation method, if roughly divided, comprises the following steps: a step of mixing an alkoxysilane containing an alkoxysilane, a mixed solvent containing water and an alcohol, an alkoxysilane solution of an inorganic acid and an aqueous solution of a barium compound with an aluminum solution containing an aluminum compound and water to prepare a mixed solution in which the aluminum compound, alkoxysilane, and the barium compound are dissolved in the mixed solvent (step #P1); a step of co-precipitating aluminum hydroxide and a silicon compound in the mixed solvent to form a first precipitate (step #P2); a step of first cooling the solution containing the precipitate to below 60°C, and then adding ammonium carbonate to precipitate barium as a carbonate to form a second precipitate (step #P3); a step of filtering out the precipitate containing the barium compound by suction filtration and washing it, and drying and calcining the filtered and washed precipitate to form a porous alumina (the present alumina) containing aluminum oxide, silicon dioxide and barium oxide (step #P4).
[0174] The alkoxysilane solution, aluminum solution, and aqueous solution of the barium compound used in step #P1 are the same as the alkoxysilane solution, aluminum solution, and aqueous solution of the barium compound used in step #K1 and step #K3 of the kneading method described above, and their repeated description is omitted. Fig.16 In the above, the alkoxysilane solution is exemplified by a TEOS solution, and the aqueous solution of the barium compound is exemplified by a barium nitrate aqueous solution. In addition, step #P2 is basically the same as step #K2 of the above-mentioned kneading method, and repeated description is omitted. However, in step #P2, since the barium compound cannot be co-precipitated with aluminum hydroxide and the silicon compound as barium hydroxide, step #P3 is required.
[0175] In step #P3, the solution containing the precipitate is cooled to below 60°C because ammonium carbonate will decompose into carbon dioxide, ammonia and water when the temperature is above 60°C, so cooling is to avoid the decomposition.
[0176] [5] Modifications of the present alumina:
[0177] The present alumina is, for example, a porous alumina obtained by mixing two oxides, silicon dioxide and barium oxide, with alumina prepared by the kneading method, impregnation method, precipitation method, etc., so that the SiO2 addition rate and the BaO addition rate are within the above-mentioned effective range. Therefore, the SiO2 addition rate and the BaO addition rate are within the above-mentioned effective range on average with respect to the total amount of the present alumina prepared.
[0178] However, when a heterogeneous porous alumina (alumina monomer, porous alumina with only silica added to alumina, porous alumina with only barium oxide added to alumina, porous alumina with silica and barium oxide added to alumina, porous alumina with oxides other than silica and barium oxide added to alumina, etc.) whose SiO2 addition rate and BaO addition rate are not within the above-mentioned effective range is mixed with the present alumina and thus partially or locally exists, assuming that the SiO2 addition rate and the BaO addition rate are outside the above-mentioned effective range on average relative to the total amount of the present alumina and the heterogeneous porous alumina, if the present alumina exists separately from the heterogeneous porous alumina and has the desired properties (specific surface area after heat treatment at 1200°C for 30 hours, solid acid amount), then the part where the present alumina exists can of course achieve the expected effect, namely, provide a porous alumina with excellent heat resistance and coking resistance. Therefore, as one embodiment of the present alumina, the present alumina can take a form in which the above-mentioned heterogeneous porous alumina is partially or locally present.
[0179] In addition, as long as the SiO2 addition rate and the BaO addition rate are within the above-mentioned effective range and the present alumina has the desired properties (specific surface area and solid acid content after heat treatment at 1200°C for 30 hours), a small amount of components other than silica and barium oxide (oxides, etc.) may be added to the alumina compared to silica and barium oxide.
[0180] [6] Application examples of this alumina:
[0181] The present alumina has excellent heat resistance as described above, so it is useful as a catalyst carrier for supporting catalyst active components, a filter, etc. In addition, the present alumina has excellent coking resistance in addition to excellent heat resistance as described above, so it is suitable as a catalyst carrier used in reactions using hydrocarbons such as steam reforming reactions.
[0182] Industrial Applicability
[0183] The present invention is suitable for porous alumina obtained by adding silicon dioxide and barium oxide to alumina, and for a catalyst using the porous alumina as a carrier.
Claims
1. A porous alumina, The characteristic is that In alumina Al 2 O 3 Adding silicon dioxide SiO 2 A porous alumina made of silicon dioxide and barium oxide BaO, wherein the silicon dioxide and the barium oxide are added to the alumina in the following manner: The barium oxide is barium aluminate BaO·Al 2 O 3 Exists either as barium aluminate BaO·Al 2 O 3 and barium hexaaluminate BaO·6Al 2 O 3 exist, Assume that the SiO 2 The amount of addition is relative to the alumina and SiO 2 The total mass ratio of the added amount is SiO 2 Addition rate, unit is mass % Assume that the amount of BaO added is relative to the amount of aluminum oxide and the amount of SiO 2 The total mass ratio of the added amount is the BaO addition rate, and the unit is mass %. The SiO 2 The amount of addition is the amount of silicon Si in the porous alumina converted into SiO 2 The amount of content, The BaO addition amount is the amount obtained by converting the content of barium Ba in the porous alumina into the content of BaO. In the SiO 2 The addition rate is within the range of 0.7 mass % to 3 mass %, and the BaO addition rate is within the range of 0.5 mass % to 14 mass %, The specific surface area of the porous alumina measured by a predetermined measurement method after heat treatment at 1200°C for 30 hours is greater than or equal to the reference specific surface area, which is the specific surface area obtained by converting the SiO 2 The addition rate was set to 3 mass %, and the BaO addition rate was set to 0 mass % to prepare a reference porous alumina for comparison, and the specific surface area of the reference porous alumina was measured in the same manner.
2. The porous alumina according to claim 1, It is characterized in that Assume that the SiO 2 The addition rate is expressed as Xs in mass %, and the BaO addition rate is expressed as Xb in mass %, 0.7 mass%≤Xs<1 mass%, and 5 mass%≤Xb≤10 mass%, or 1 mass%≤Xs<2 mass%, and 3 mass%≤Xb≤10 mass%, or 2 mass %≤Xs≤3 mass %, and 1 mass %≤Xb≤14 mass %.
3. The porous alumina according to claim 2, It is characterized in that It is formed so that 1 mass % ≤ Xs ≤ 3 mass %, and 3 mass % ≤ Xb ≤ 10 mass %.
4. A porous alumina, The characteristic is that In alumina Al 2 O 3 Adding silicon dioxide SiO 2 and barium oxide BaO, wherein: The barium oxide is barium aluminate BaO·Al 2 O 3 Exists either as barium aluminate BaO·Al 2 O 3 and barium hexaaluminate BaO·6Al 2 O 3 exist, The SiO 2 The amount of addition is relative to the alumina and SiO 2 The SiO in mass % is specified by the total mass ratio of the added amount. 2 The addition rate is set to Xs, wherein the SiO 2 The amount of addition is the amount of silicon Si in the porous alumina converted into SiO 2 The unit of Xs is mass %. The amount of BaO added relative to the amount of alumina and SiO 2 When the BaO addition rate in mass % specified by the total mass ratio of the added amount is Xb, wherein the BaO addition amount is the amount obtained by converting the content of barium Ba in the porous alumina into the content of BaO, and the unit of Xb is mass %. Formed as: 0.7 mass%≤Xs<1 mass%, and 5 mass%≤Xb≤10 mass%, or 1 mass%≤Xs<2 mass%, and 3 mass%≤Xb≤10 mass%, or 2 mass %≤Xs≤3 mass %, and 1 mass %≤Xb≤14 mass %.
5. The porous alumina according to claim 4, It is characterized in that It is formed so that 1 mass % ≤ Xs ≤ 3 mass %, and 3 mass % ≤ Xb ≤ 10 mass %.
6. A catalyst, It is characterized in that The porous alumina according to any one of claims 1 to 5 and a catalyst substance supported on the porous alumina.