A high-strength, high-toughness, long-lasting antibacterial polylactic acid blended composite material and its preparation method and application

By designing functional compatibilizers and process control, the compatibility of polylactic acid and biodegradable polyester or elastomer is improved, and the strength, toughness and antibacterial properties of polylactic acid blended composite materials are solved, achieving high strength, High toughness and long-acting antibacterial polylactic acid blend composite material suitable for packaging field.

CN115073900BActive Publication Date: 2024-11-26HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210649002.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-09
Publication Date
2024-11-26
Estimated Expiration
2042-06-09

AI Technical Summary

Technical Problem

The molecular chains of polylactic acid and biodegradable polyesters or elastomers are very different, resulting in poor compatibility. It is difficult to obtain high-strength, high-toughness and long-acting antibacterial degradable products directly melt and blend, and the polymer material is melted. Antibacterial agents are easily volatile or decomposed during processing, affecting the long-term antibacterial properties of the material.

Method used

By designing functional compatibilizing agents, including glycidyl methacrylate, polyadipic acid-butylene terephthalate and organic antibacterial agents, the introduction of compatibilizing and antibacterial components is enhanced by the design of functional compatibilizing agents, including glycidyl methacrylate, polyadipic acid-butylene terephthalate and organic antibacterial agents, through melt grafting reaction, the introduction of compatibilizing and antibacterial components, and the improvement of polylactic acid and The interaction force and compatibility of biodegradable polyester or elastomer can be prepared by using specific process steps such as vacuum drying, melt blending, etc. to prepare high-strength, high-strength, long-acting, antibacterial polylactic acid blend composite materials.

Benefits of technology

It realizes the high strength, high toughness and long-term antibacterial properties of polylactic acid blended composite materials, while retaining biodegradable properties. It is suitable for packaging fields, especially in disposable medical equipment and food packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115073900B_ABST
    Figure CN115073900B_ABST
Patent Text Reader

Abstract

The present invention proposes a high-strength, high-toughness, long-lasting antibacterial polylactic acid blended composite material and a preparation method and application thereof, wherein the composite material comprises at least the following components: 10-90 parts of polylactic acid; 10-90 parts of biodegradable polyester or elastomer; 1-10 parts of functional compatibilizer; 0.5-2 parts of chain extender; 1-30 parts of filler; and 0.1-2 parts of antioxidant; wherein the functional compatibilizer is obtained by melt grafting of glycidyl methacrylate, polybutylene adipate-terephthalate and an organic antibacterial agent. The functional compatibilizer proposed in the present invention improves the compatibility between components of the polylactic acid blended composite material, improves the mechanical properties of the blended composite material, and realizes and improves the long-lasting antibacterial properties of the material. The polylactic acid blended composite material obtained by this preparation method has high strength, high toughness, long-lasting antibacterial properties and complete biodegradability, which meets the requirements of food packaging and disposable medical packaging and other fields that the material has high mechanical properties, long-lasting antibacterial properties and degradation properties at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer material synthesis, and in particular to a high-strength, high-toughness, long-acting antibacterial polylactic acid blended composite material and a preparation method and application thereof. Background Art

[0002] As the problems of "microplastics" and environmental pollution become increasingly serious, environmentally friendly polymers have received widespread attention. The raw materials of polylactic acid (PLA) are mainly derived from starch contained in biological resources. It can be degraded into water and carbon dioxide under natural conditions, and has excellent mechanical properties and processing properties, and has good application prospects.

[0003] However, PLA has the disadvantages of low melt strength, poor toughness, and weak crystallization ability. Melt blending of PLA with biodegradable polyesters or elastomers such as polybutylene adipate-terephthalate (PBAT), polycaprolactone (PCL), polybutylene succinate (PBS), and polypropylene carbonate (PPC) is one of the most economical methods for improving the performance of PLA. Blending PLA with biodegradable polyesters or elastomers can improve the melt strength and toughness of PLA while retaining the biodegradability of PLA, thereby expanding the application range of PLA. However, the molecular chains of PLA and biodegradable polyesters or elastomers are quite different, and the compatibility between the two is poor. It is difficult to obtain degradable products with application value by direct melt blending.

[0004] Antimicrobial materials are widely used in biomedicine, food packaging, and health prevention and control because they can reduce bacteria and microbial infections caused by contact between people and products, and between products. Traditional inorganic antimicrobial additives have the defects of difficult dispersion, easy migration, and low efficiency. Organic antimicrobial additives, especially halamine antimicrobial agents and guanidine antimicrobial agents, have broad-spectrum and high-efficiency antimicrobial activity, low mammalian cell toxicity, and good stability. They can be added to polymer materials by melt blending to improve the antimicrobial properties of the materials. However, the high temperature during the melt processing of polymer materials may cause the volatilization or decomposition and inactivation of the antimicrobial agent. At the same time, the migration of small molecules of organic antimicrobial agents affects the long-term antimicrobial properties of polymer materials.

[0005] The core of the present invention is to avoid the volatilization, decomposition and inactivation of organic antibacterial agents during the preparation of PLA blended composite materials and the migration during use, which will affect their antibacterial properties, and to achieve their long-term antibacterial properties while maintaining or even improving the basic properties of PLA blended composite materials. How to obtain a macromolecular compatibilizer with antibacterial function through molecular design, while maintaining the basic properties of PLA blended composite materials, improve the compatibility between the components of the blended composite materials, and obtain a high-strength, high-toughness and long-term antibacterial PLA blended composite material is the technical problem to be solved by the present invention. Summary of the invention

[0006] The present invention proposes a high-strength, high-toughness, long-acting antibacterial polylactic acid blend composite material and a preparation method and application thereof. The compatibilizing and antibacterial components are introduced by molecular design and process control of a functional compatibilizer, and the compatibilizing and antibacterial components are introduced into a polylactic acid / biodegradable polyester or elastomer blend. While retaining the degradation performance of the polylactic acid / biodegradable polyester or elastomer blend, the interaction force and compatibility between the polylactic acid and biodegradable polyester or elastomer phases are improved, so as to obtain a high-strength, high-toughness, long-acting antibacterial degradable polylactic acid blend composite material.

[0007] To solve the above technical problems, the present invention is achieved through the following technical solutions:

[0008] The present invention provides a high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material, characterized in that it comprises at least the following components:

[0009]

[0010]

[0011] The functional compatibilizer is obtained by melt grafting reaction of glycidyl methacrylate, polybutylene adipate-terephthalate and an organic antibacterial agent.

[0012] In one embodiment of the present invention, the functional compatibilizer has the general structural formula:

[0013]

[0014] Wherein R is an organic halogenamine antibacterial agent or an organic guanidine salt antibacterial agent containing a primary amine or a secondary amine in the molecular structure, and the structural formula of R is selected from any one of the following structural formulas:

[0015]

[0016]

[0017] Wherein, X=Cl, Br or I, R1 is H, hydroxyl, alkyl chain of 1-16 C atoms or organic ring, R2 is H or alkyl chain of 1-6 C atoms, R3 is H or alkyl chain of 1-6 C atoms, n=1~20, m=2~400, Y is Cl - Br - 、NO3 - 、HCO3 - or H2PO4 - One of them.

[0018] In one embodiment of the present invention, the biodegradable polyester or elastomer is one or more polymers selected from the group consisting of polybutylene adipate-terephthalate, polycaprolactone, polypropylene carbonate, and polybutylene succinate.

[0019] In one embodiment of the present invention, the chain extender is a mixture of one or more of styrene-methacrylate glycidyl copolymer, styrene-acrylate-methacrylate glycidyl copolymer, styrene-acrylate-maleic anhydride copolymer, styrene-acrylonitrile-methacrylate glycidyl copolymer, 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, glycerol triglycidyl ether and triphenyl phosphite.

[0020] In one embodiment of the present invention, the filler is a mixture of one or more of starch, light calcium carbonate, silicon dioxide, montmorillonite and talc.

[0021] In one embodiment of the present invention, the antioxidant is a mixture of one or more of antioxidant 168, antioxidant 300, antioxidant 618, antioxidant 626, antioxidant 1010, antioxidant 1076, antioxidant TBHQ, antioxidant AT-10, and antioxidant BHT.

[0022] The present invention also provides a method for preparing a high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material, which comprises at least the following steps:

[0023] adding a free radical initiator to glycidyl methacrylate to prepare a mixed solution;

[0024] Drying polybutylene adipate-terephthalate in a vacuum oven at 40-60° C. for 12-24 hours, then adding the dried polybutylene adipate-terephthalate into an internal mixer set at 120-150° C. to melt for 5-20 minutes; adding the mixed solution into the internal mixer, and continuing to melt-mix with the polybutylene adipate-terephthalate for 5-20 minutes to obtain a blend;

[0025] Adding an organic antibacterial agent to the blend for further melt blending, the melt blending temperature is 150-170° C., the melt blending time is 5-20 min, and the rotation speed is 50-100 rpm to obtain a compatibilizer;

[0026] The compatibilizer is melt-blended with polylactic acid, biodegradable polyester or elastomer, chain extender, filler and antioxidant in an internal mixer at a melt-blending temperature of 140-220° C., a melt-blending time of 5-20 min, and a rotation speed of 50-100 rpm to obtain the high-strength, high-toughness, long-acting antibacterial polylactic acid blended composite material.

[0027] In one embodiment of the present invention, the free radical initiator is a mixture of one or more of dicumyl peroxide, benzoyl peroxide, and tert-butyl hydroperoxide, and the amount of the free radical initiator is 0.01%-0.5% of the amount of the glycidyl methacrylate.

[0028] In one embodiment of the present invention, the amount of the glycidyl methacrylate is 5-15% of the amount of the polybutylene adipate-terephthalate, and the amount of the organic antibacterial agent is 30-70% of the amount of the glycidyl methacrylate.

[0029] The present invention also provides a package, comprising the above-mentioned high-strength, high-toughness, long-acting antibacterial polylactic acid blended composite material.

[0030] The present invention proposes a high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material, a preparation method and an application thereof. The preparation process is simple to operate, and the compatibilizer effectively improves the compatibility of the heterogeneous components of the blend in the polylactic acid / biodegradable polyester or elastomer blend composite system through an in-situ reaction during the melt blending process, wherein the grafted organic antibacterial component imparts the polylactic acid blend composite material with long-lasting antibacterial properties. The prepared polylactic acid blend composite material has high strength, high toughness, long-lasting antibacterial properties and biodegradability, and can be applied to the packaging field to alleviate environmental pressure. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The present invention is a flow chart of a method for preparing a high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material.

[0032] Figure 2 This is a process diagram for preparing the functional compatibilizer of the present invention.

[0033] Figure 3 Schematic diagram of the structure of the polyhexamethyleneguanidine hydrochloride compatibilizer in Example 1.

[0034] Figure 4 This is the NMR spectrum of the polyhexamethyleneguanidine hydrochloride compatibilizer in Example 1. DETAILED DESCRIPTION

[0035] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0036] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner. Therefore, the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0037] The technical solution of the present invention is further described in detail below in conjunction with several embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] Polylactic acid and its products have stable physical properties under normal temperature and humidity conditions, and polylactic acid waste can be degraded into carbon dioxide and water by microorganisms in soil or seawater, and then can enter the natural cycle infinitely through plant photosynthesis. Therefore, polylactic acid is an ideal green polymer material. Polylactic acid has many applications, such as in the automotive field, disposable products field, and electronic field. For example, in the field of disposable products, due to the fact that polylactic acid is absolutely harmless to the human body, polylactic acid has unique advantages in disposable tableware, food packaging materials, etc.

[0039] See also Figure 1 As shown, the present invention proposes a method for preparing a high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material, including but not limited to the following steps S1-S4.

[0040] S1. adding a free radical initiator to glycidyl methacrylate to prepare a mixed solution;

[0041] S2, drying the polybutylene adipate-terephthalate in a vacuum oven at 40-60° C. for 12-24 h, then adding the dried polybutylene adipate-terephthalate to an internal mixer set at a temperature of 120-150° C. to melt for 5-20 min; adding the mixed solution to the internal mixer, and continuing to melt-mix with the polybutylene adipate-terephthalate for 5-20 min to obtain a blend;

[0042] S3, adding an organic antibacterial agent to the blend for further melt blending, the melt blending temperature is 150-170° C., the melt blending time is 5-20 min, and the rotation speed is 50-100 rpm to obtain a compatibilizer;

[0043] S4. Melt-blending the compatibilizer with polylactic acid, biodegradable polyester or elastomer, chain extender, filler and antioxidant in an internal mixer at a melt-blending temperature of 140-220° C., a melt-blending time of 5-20 min, and a rotation speed of 50-100 rpm to obtain the high-strength, high-toughness, long-acting antibacterial polylactic acid blended composite material.

[0044] See also Figure 1-2 As shown, in step S1, in one embodiment of the present invention, glycidyl methacrylate can be selected from glycidyl methacrylate (GMA) solution or monodisperse glycidyl methacrylate (GMA) microspheres. In this embodiment, glycidyl methacrylate is selected from glycidyl methacrylate (GMA) solution, and the content of glycidyl methacrylate is 97%. Glycidyl methacrylate (GMA) solution is added with a stabilizer to prevent glycidyl methacrylate from coagulation and ensure that glycidyl methacrylate is uniformly dispersed in the solution. The present invention does not limit the type and content of the stabilizer. In this embodiment, the stabilizer is selected from p-hydroxyanisole (MEHQ), and the content of p-hydroxyanisole is 100ppm. In one embodiment of the present invention, the amount of glycidyl methacrylate is, for example, 5%-15% of the amount of polybutylene adipate-terephthalate, and further, the amount of glycidyl methacrylate is, for example, 10% of the amount of polybutylene adipate-terephthalate. In this embodiment, the amount of glycidyl methacrylate used is, for example, 10 g.

[0045] See also Figure 1-2 As shown, in step S1, a free radical initiator is added to glycidyl methacrylate to prepare a glyceride mixed solution containing the free radical initiator. In one embodiment of the present invention, the free radical initiator can be a peroxide initiator with a higher decomposition temperature, for example, one or more free radical initiators such as diisopropyl peroxide, benzoyl peroxide, and tert-butyl hydroperoxide. Further, in this embodiment, the free radical initiator is, for example, diisopropyl peroxide (DCP). And the amount of the free radical initiator is, for example, 0.01%-0.5% of the amount of glyceride, and further, the amount of the free radical initiator is, for example, 0.1% of the amount of glyceride. In this embodiment, the amount of the free radical initiator is, for example, 0.01g.

[0046] See also Figure 1-2As shown, in step S2, before melting polybutylene adipate-terephthalate, polybutylene adipate-terephthalate needs to be vacuum dried to remove residual moisture in the raw material. In one embodiment of the present invention, polybutylene adipate-terephthalate can be placed in a vacuum oven for drying, and the drying temperature is set to, for example, 40-60°C, and the drying time is set to, for example, 12-24h. Further, the drying temperature is 60°C and the drying temperature is 12h. In one embodiment of the present invention, polybutylene adipate-terephthalate is used as the main chain, and the amount of polybutylene adipate-terephthalate (PBAT) is, for example, 30-60g, and further, the amount of polybutylene adipate-terephthalate (PBAT) is, for example, 50g.

[0047] See also Figure 1-2 As shown, in step S2, in one embodiment of the present invention, an internal mixer can be used to melt the polybutylene adipate-terephthalate so that the polybutylene adipate-terephthalate is melted into a liquid state at a high temperature. In one embodiment of the present invention, the temperature of the melt treatment of the polybutylene adipate-terephthalate is, for example, 120-150° C., and the melt treatment time is 5-20 minutes. Further, the melt treatment temperature is, for example, 140° C., and the melt treatment time is 5-20 minutes.

[0048] See also Figure 1-2 As shown, in step S2, in one embodiment of the present invention, in order to obtain the compatibilizer, the mixed solution formed in step 2 needs to be added to an internal mixer and melt blended with polybutylene adipate-terephthalate at high temperature. In one embodiment of the present invention, the melt blending time is set to, for example, 5-20 minutes, and the speed of the internal mixer is set to, for example, 50-100 rpm.

[0049] See also Figure 1-3 As shown, in step S3, in one embodiment of the present invention, in order to obtain a compatibilizer with antibacterial properties, an organic antibacterial agent can be added to the internal mixer for melt blending. In this embodiment, the antibacterial agent is, for example, an organic antibacterial agent, and further, optionally, the antibacterial agent is, for example, polyhexamethyleneguanidine hydrochloride (PHMG). In one embodiment of the present invention, the amount of the antibacterial agent is, for example, 30-70% of the amount of glycidyl methacrylate, and further, the amount of the antibacterial agent is, for example, 30% of the amount of glycidyl methacrylate. In this embodiment, the amount of the antibacterial agent is, for example, 3g.

[0050] See also Figure 1-3As shown, in step S3, in one embodiment of the present invention, the temperature of melt blending is set to, for example, 140-160°C, and the melt blending time is set to, for example, 5-20min. Further, in this embodiment, the temperature of melt blending is set to, for example, 140°C, and the melt blending time is set to, for example, 8min. In an embodiment of the present invention, when the antibacterial agent is added to further melt blend the blend, the speed of the internal mixer is set to, for example, 50-100rpm to obtain the desired functional compatibilizer. The epoxy functional group contained in the functional compatibilizer can effectively react with the terminal hydroxyl or terminal carboxyl of polylactic acid, biodegradable polyester or elastomer to extend the chain, so that the polylactic acid macromolecular segment grafted with biodegradable polyester or elastomer is obtained in the blending system, and the physical entanglement formed between the macromolecular segment and the biodegradable polyester or elastomer matrix is ​​used to effectively improve the compatibility of the polylactic acid / biodegradable polyester or elastomer blend, and improve the mechanical properties of the prepared polylactic acid blended composite material, while retaining the biodegradability of the material. At the same time, the organic antibacterial molecules contained in the functional compatibilizer can enable the prepared antibacterial and degradable polylactic acid blended composite materials to obtain efficient and lasting antibacterial properties.

[0051] See also Figure 1-4 As shown, in step S4, in one embodiment of the present invention, before the functional compatibilizer is melt-blended with polylactic acid and the like to obtain the high-strength, high-toughness, long-lasting antibacterial polylactic acid blended composite material, the polylactic acid, biodegradable polyester or elastomer, and the functional compatibilizer must be dried. In one embodiment of the present invention, polylactic acid, biodegradable polyester or elastomer, and the functional compatibilizer can be placed in a vacuum oven for vacuum drying, and the drying temperature is set to 40°C-60°C, for example, and the drying time is set to 12-24h, for example. Furthermore, the drying temperature is set to 60°C, for example, and the drying time is set to 12h, for example. In one embodiment of the present invention, polylactic acid, biodegradable polyester or elastomer, functional compatibilizer, chain extender, filler, and antioxidant are uniformly mixed in a specific mass ratio and melt-blended in an internal mixer. The melt-blending temperature is, for example, set to 140-220°C, the rotation speed is, for example, set to 50-100rpm, and the melt-blending time is, for example, set to 5-20min. After blending, the high-strength, high-toughness, long-lasting antibacterial polylactic acid blended composite material is obtained.

[0052] See also Figure 1-4As shown, in one embodiment of the present invention, the high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material is obtained by melt blending the required functional compatibilizer with polylactic acid, biodegradable polyester or elastomer, chain extender, filler and antioxidant. The mass fraction of polylactic acid is, for example, 10-90 parts, the mass fraction of biodegradable polyester or elastomer is, for example, 90-10 parts, the mass fraction of the required functional compatibilizer is, for example, 1-10 parts, the mass fraction of the chain extender is, for example, 0.5-2 parts, the mass fraction of the filler is, for example, 1-30 parts, and the mass fraction of the antioxidant is, for example, 0.1-2 parts. In one embodiment of the present invention, the chain extender is a mixture of styrene-methacrylate glycidyl copolymer, styrene-acrylate-methacrylate glycidyl copolymer, styrene-acrylate-maleic anhydride copolymer, styrene-acrylonitrile-methacrylate glycidyl copolymer, 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, glycerol triglycidyl ether, triphenylphosphite, etc. Further, the chain extender is BASF polyurethane chain extender ADR-4300. In one embodiment of the present invention, the filler is a mixture of starch, light calcium carbonate, silicon dioxide, montmorillonite, talc, etc. The added filler can reduce the production cost without affecting the properties of other materials such as mechanical properties, degradation properties, etc. Further, the filler is light calcium carbonate. In one embodiment of the present invention, the antioxidant is a mixture of one or more of antioxidant 168, antioxidant 300, antioxidant 618, antioxidant 626, antioxidant 1010, antioxidant 1076, antioxidant TBHQ, antioxidant AT-10, antioxidant BHT, etc. Further, the antioxidant is a compound antioxidant, which is compounded from antioxidant 1010 and antioxidant 168.

[0053] The present invention also provides an application of a high-strength, high-toughness, long-acting antibacterial polylactic acid blended composite material. The high-toughness, long-acting antibacterial polylactic acid blended composite material obtained by the above preparation method is used as a raw material to prepare a degradable polyester film. The preparation is carried out according to the following steps:

[0054] 1) Add the dried polylactic acid, polybutylene adipate-terephthalate, compatibilizer and chain extender, CaCO3, and compound antioxidant into a high-speed mixer at a mass ratio of 15:75:10:0.5:5:0.01 to form a uniform mixture. In an embodiment of the present invention, the mixing speed is, for example, set to 800-1000 r / min, and the mixing time is, for example, set to 5-20 min.

[0055] 2) The mixture obtained in step 1) is then melted, blended, and extruded through a twin-screw extruder. In an embodiment of the present invention, the aspect ratio of the twin-screw extruder is, for example, 32:1, the processing temperature of the twin-screw extruder can be set to 140-220°C, and the speed of the twin-screw extruder can be set to 100-300r / min. After melting, blending, and extrusion, and then through water-cooled drawing, air drying, and pelletizing processes, a polylactic acid blended composite material with excellent comprehensive performance, high strength, high toughness, and long-lasting antibacterial properties is obtained.

[0056] 3) Adding the polylactic acid composite material obtained in step 2) into a single screw extruder blown film machine to blow a film to prepare a degradable polyester film. In an embodiment of the present invention, the temperature of each section of the film blowing machine can be controlled within the range of 140-170° C., the main screw speed is, for example, 50-250 r / min, and the blow-up ratio (BUR) is, for example, 3-5.

[0057] After testing, the biodegradable polyester film had a tensile strength of 25.5 MPa, an elongation at break of 350%, and antibacterial rates against Escherichia coli and Staphylococcus aureus of 99.7% and 99.8%, respectively.

[0058] Hereinafter, the present invention will be explained in more detail by citing examples, which should not be construed as limiting. Appropriate modifications may be made within the scope consistent with the gist of the present invention, all of which fall within the technical scope of the present invention.

[0059] Example 1

[0060] The preparation method of the required functional compatibilizer comprises the following specific steps:

[0061] 1) Dissolve 0.05 g of dicumyl peroxide (DCP) in 10 g of glycidyl methacrylate (GMA) solution to prepare a GMA solution containing a free radical initiator DCP.

[0062] 2) 50 g of polybutylene adipate terephthalate (PBAT) was vacuum dried at 60° C. for 12-24 h to remove residual moisture in the raw material.

[0063] 3) The dried PBAT was added to an internal mixer and melted at 140° C. for 5 min, and then the GMA solution containing the free radical initiator was added and melt-mixed for 6-8 min.

[0064] 4) Add 5 g of polyhexamethyleneguanidine hydrochloride (PHMG) to the blend for further melt blending at a melt blending temperature of 160° C., a blending time of 6-10 min, and a rotation speed of 50-100 rpm to obtain the desired compatibilizer.

[0065] The raw materials and their mass fraction ratios used in the following examples and comparative examples for preparing the required high-strength, high-toughness, long-acting antibacterial polylactic acid blended composite materials are shown in Table 1:

[0066] Table 1. Raw materials and amounts of composite materials required for preparing the examples and comparative examples (proportion by mass)

[0067] Components Comparative Example 1 Example 2 Example 3 Example 4 PLA 70 70 70 70 PBAT 30 30 30 30 Compatibilizer \ 1 5 10 ADR-4300 0.5 0.5 0.5 0.5 <![CDATA[CaCO3]]> 5 5 5 5 Compound antioxidant 0.1 0.1 0.1 0.1

[0068] Comparative Example 1

[0069] Referring to Table 1, the preparation of the required polylactic acid blended composite material in this comparative example is carried out according to the following steps:

[0070] 1) First, polylactic acid and polybutylene adipate-terephthalate are vacuum dried at 60° C. for 12-24 h.

[0071] 2) According to the mass proportion in Table 1, 70 parts of polylactic acid, 30 parts of polybutylene adipate terephthalate, 0.5 parts of ADR-4300, 5 parts of CaCO3 and 0.1 parts of compound antioxidant were mixed evenly, added into an internal mixer with a speed of 50-100 rpm, and melt-blended at 180-190 ° C for 8-10 min to obtain the desired polylactic acid blended composite material.

[0072] Example 2

[0073] Referring to Table 1, the steps for preparing the required high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material in this embodiment are as follows:

[0074] 1) First, polylactic acid, polybutylene adipate-terephthalate and compatibilizer are vacuum dried at 60° C. for 12-24 h.

[0075] 2) According to the mass proportions in Table 1, 70 parts of polylactic acid, 30 parts of polybutylene adipate-terephthalate, 1 part of a compatibilizer, 0.5 parts of ADR-4300, 5 parts of CaCO3 and 0.1 parts of a compound antioxidant were mixed evenly, added into an internal mixer at a speed of 50-100 rpm, and melt-blended at 180-190 ° C for 8-10 minutes to obtain the desired high-strength, high-toughness and long-lasting antibacterial polylactic acid blended composite material.

[0076] Example 3

[0077] Referring to Table 1, the steps for preparing the required high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material in this embodiment are as follows:

[0078] 1) First, polylactic acid, polybutylene adipate-terephthalate and compatibilizer are vacuum dried at 60° C. for 12-24 h.

[0079] 2) According to the mass proportions in Table 1, 70 parts of polylactic acid, 30 parts of polybutylene adipate terephthalate, 5 parts of compatibilizer, 0.5 parts of ADR-4300, 5 parts of CaCO3 and 0.1 parts of compound antioxidant were mixed evenly, added into an internal mixer with a speed of 50-100 rpm, and melt-blended at 180-190 ° C for 8-10 minutes to obtain the desired high-strength, high-toughness and long-lasting antibacterial polylactic acid blended composite material.

[0080] Example 4

[0081] Referring to Table 1, the steps for preparing the required high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material in this embodiment are as follows:

[0082] 1) First, polylactic acid, polybutylene adipate-terephthalate and compatibilizer are vacuum dried at 60° C. for 12-24 h.

[0083] 2) According to the mass proportion in Table 1, 70 parts of polylactic acid, 30 parts of polybutylene adipate-terephthalate, 10 parts of compatibilizer, 0.5 parts of ADR-4300, 5 parts of CaCO3 and 0.1 parts of compound antioxidant were mixed evenly, added into an internal mixer with a speed of 50-100 rpm, and melt-blended at 180-190 ° C for 8-10 minutes to obtain the desired high-strength, high-toughness and long-lasting antibacterial polylactic acid blended composite material.

[0084] The high-strength, high-toughness, long-acting antibacterial polylactic acid blended composite materials prepared in the above comparative examples and embodiments were hot-pressed to prepare test specimens, wherein the test standard is;

[0085] Tensile strength, tested according to ISO 527 standard, speed is 50mm / min.

[0086] Bending strength, tested according to ISO 178 standard, speed is 2mm / min.

[0087] Izod notched impact strength, tested according to ISO 180 standard.

[0088] The antibacterial rate is tested according to GB / T 31402-2015 standard.

[0089] Table 2. Test results of composite material properties in various embodiments and comparative examples

[0090]

[0091] The test results are shown in Table 2. Comparing Comparative Example 1 with Examples 2-4, the prepared macromolecular compatibilizer grafted with epoxy functional groups and antibacterial guanidine salts can effectively improve the compatibility, antibacterial properties and mechanical properties of polylactic acid (PLA) / polybutylene adipate-terephthalate (PBAT) blends. At the same time, the higher the content of the compatibilizer, the better the compatibilization effect on the polylactic acid (PLA) / polybutylene adipate-terephthalate (PBAT) blend, the higher the tensile strength, elongation at break and impact strength of the prepared antibacterial polylactic acid composite material, and the better the antibacterial effect on Escherichia coli and Staphylococcus aureus. The above results show that the compatibilizer synthesized by the present invention can effectively improve the compatibility and interfacial bonding force of polylactic acid (PLA) and biodegradable polyester or elastomer, significantly improve the strength and toughness of the antibacterial polylactic acid composite material, and give the material antibacterial properties. In addition, the compatibilizer itself is degradable, and can fully retain its degradable properties while improving the comprehensive performance of the high-strength, high-toughness and long-lasting antibacterial polylactic acid blended composite material, and has high application value in the packaging field, especially in disposable medical device packaging and food packaging.

[0092] In summary, the present invention proposes a high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material, a preparation method and an application thereof, and introduces antibacterial components through molecular design and process control to obtain a functional macromolecular compatibilizer grafted with epoxy functional groups and antibacterial guanidine salts. This functional compatibilizer can effectively improve the compatibility, antibacterial properties and mechanical properties of polylactic acid / polybutylene adipate-terephthalate blends, thereby obtaining a modified polylactic acid blend composite material with high strength, high toughness and excellent antibacterial properties, which has high application value in the packaging field, especially in disposable medical device packaging and food packaging.

[0093] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.

[0094] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.

Claims

1. A high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material, characterized in that: It is composed of the following components: Polylactic acid 10-90 parts; 10-90 parts of biodegradable polyester or elastomer; 1-10 parts of functional expander; Chain extender 0.5-2 parts; 1-30 parts of filler; Antioxidant 0.1-2 parts; Wherein, the functional compatibilizer is obtained by melt grafting glycidyl methacrylate, polybutylene adipate-terephthalate and an organic antibacterial agent; The functional compatibilizer has the general structural formula: ; R is an organic halogenamine antibacterial agent or an organic guanidine salt antibacterial agent containing a primary amine or a secondary amine in the molecular structure; The biodegradable polyester or elastomer is one or more polymers selected from polybutylene adipate-terephthalate, polycaprolactone, polypropylene carbonate, and polybutylene succinate; The structural formula R is selected from any one of the following structural formulas: ; ; ; Wherein, X = Cl, Br or I, R1 is H, hydroxyl, alkyl chain of 1-16 C atoms or organic ring, R2 is H or alkyl chain of 1-6 C atoms, R3 is H or alkyl chain of 1-6 C atoms, n = 1-20, m = 2-400, Y is Cl - Br - 、NO3 - 、HCO3 - or H2PO4 - One of; The chain extender is one or more mixtures of styrene-glycidyl methacrylate copolymer, styrene-acrylate-glycidyl methacrylate copolymer, styrene-acrylate-maleic anhydride copolymer, styrene-acrylonitrile-glycidyl methacrylate copolymer, 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, glycerol triglycidyl ether and triphenyl phosphite.

2. The high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material according to claim 1, characterized in that: The filler is one or more mixtures of starch, light calcium carbonate, silicon dioxide, montmorillonite and talc.

3. The high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material according to claim 1, characterized in that: The antioxidant is a mixture of one or more of antioxidant 168, antioxidant 300, antioxidant 618, antioxidant 626, antioxidant 1010, antioxidant 1076, antioxidant TBHQ, antioxidant AT-10, and antioxidant BHT.

4. A method for preparing a high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material, characterized in that: At least the following steps are included: adding a free radical initiator to glycidyl methacrylate to prepare a mixed solution; Drying polybutylene adipate-terephthalate in a vacuum oven at 40-60° C. for 12-24 hours, then adding the dried polybutylene adipate-terephthalate into an internal mixer set at a temperature of 120-150° C. to melt for 5-20 minutes, then adding the mixed solution into the internal mixer, and continuing to melt-mix with the polybutylene adipate-terephthalate for 5-20 minutes to obtain a blend; Adding an organic antibacterial agent to the blend, and obtaining a functional compatibilizer containing an antibacterial structure through a melt grafting reaction at a temperature of 150-170° C., a melt blending time of 5-20 min, and a rotation speed of 50-100 rpm; The functional compatibilizer is melt-blended with polylactic acid, biodegradable polyester or elastomer, chain extender, filler and antioxidant in an internal mixer at a melt-blending temperature of 140-220° C., a melt-blending time of 5-20 min, and a rotation speed of 50-100 rpm to obtain the high-strength, high-toughness, long-acting antibacterial polylactic acid blended composite material; Wherein, the organic antibacterial agent is an organic halogen amine antibacterial agent or an organic guanidine salt antibacterial agent containing primary amine or secondary amine.

5. The method for preparing a high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material according to claim 4, characterized in that: The free radical initiator is a mixture of one or more of dicumyl peroxide, benzoyl peroxide, and tert-butyl hydroperoxide, and the amount of the free radical initiator used is 0.01%-0.5% of the amount of the glycidyl methacrylate used.

6. The method for preparing a high-strength, high-toughness, long-lasting antibacterial polylactic acid blend composite material according to claim 4, characterized in that: The amount of the glycidyl methacrylate is 5-15% of the amount of the polybutylene adipate-terephthalate, and the amount of the organic antibacterial agent is 30-70% of the amount of the glycidyl methacrylate.

7. A packaging, characterized in that: It includes the high-strength, high-toughness, long-lasting antibacterial polylactic acid blended composite material as described in claims 1-3.