Preparation method of zinc oxide and copper oxide co-doped photocatalytic material and its application in removing thallium from water

Through the co-doping of zinc oxide and copper oxide, the hydrothermal method is used to prepare composite photocatalytic materials, which solves the problem of low photocatalytic activity of zinc oxide, and achieves the effect of efficient removal of trace thallium from water, meeting the environmental protection and pollution-free standards.

CN115106090BActive Publication Date: 2024-11-29HARBIN INST OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202210932031.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-04
Publication Date
2024-11-29
Estimated Expiration
2042-08-04

AI Technical Summary

Technical Problem

The existing zinc oxide photocatalytic materials have low photocatalytic activity, resulting in low efficiency in removing trace thallium from water.

Method used

By co-doping with copper oxide, zinc oxide and copper oxide composite photocatalytic materials are prepared by hydrothermal method, and their light absorption range and photogenerated electron-hole recombination rate are adjusted to improve photocatalytic performance.

Benefits of technology

It has achieved efficient removal of trace thallium from water, high photoelectric conversion efficiency, meets environmental protection and pollution-free standards, and can be widely used in water treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115106090B_ABST
    Figure CN115106090B_ABST
Patent Text Reader

Abstract

The preparation method of zinc oxide and copper oxide co-doped photocatalytic material and its application in removing thallium from water, the purpose of the present invention is to solve the problem of low catalytic activity of existing zinc oxide photocatalytic materials. Preparation method: 1. Mix hexadecyltrimethylammonium bromide, zinc nitrate hexahydrate, copper nitrate trihydrate and deionized water, add sodium hydroxide solution to obtain a reaction solution; 2. Carry out hydrothermal reaction in an oven at 160-200°C, then wash the precipitate with anhydrous ethanol and deionized water until it is neutral, and obtain the reactant after centrifugation and drying; 3. Put the reactant into a muffle furnace, roast it at 400-600°C, and obtain zinc oxide and copper oxide co-doped photocatalytic material. The composite photocatalytic material prepared by the present invention has high photoelectric conversion efficiency, high photocatalytic activity, is green and pollution-free, has visible light photocatalytic activity, and has high removal efficiency for trace thallium in wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a zinc oxide and copper oxide co-doped photocatalytic material and application thereof in removing trace thallium in water. Background Art

[0002] Thallium is a highly dispersed rare metal element, widely used in chemical, electronic, pharmaceutical, aerospace, high-energy physics and superconducting materials industries. At the same time, thallium is also an element with strong physiological toxicity. Due to the current extensive exploitation and application of thallium resources, the ways in which thallium enters the water environment are expanding. Thallium mainly exists in the form of positive monovalent in nature. Its toxicity is greater than arsenic. It can enter the human body through the digestive tract, skin contact, and inhalation of dust and smoke, leading to thallium poisoning in the human body. Thallium poisoning can cause numbness or pain in the lower limbs, back pain, hair loss, blindness, headache, lack of energy, tremors in the hands and feet, unsteady walking, etc. Severe thallium poisoning can lead to vegetative state. Therefore, it is particularly important to remove thallium in water.

[0003] Semiconductor-based photocatalytic technology has the advantages of high efficiency, energy saving, and environmental protection. The semiconductor photocatalysts that have been studied more are mainly zinc oxide and titanium dioxide. The preparation cost of zinc oxide is 75% lower than that of titanium dioxide, the raw materials are abundant, and the crystal morphology is diverse. It is an excellent semiconductor photocatalyst. However, according to existing studies, the efficiency of zinc oxide photocatalyst in degrading organic pollutants is not high due to its shortcomings such as narrow light absorption range and high recombination rate of photogenerated electrons and holes.

[0004] In order to overcome the above defects of zinc oxide as a photocatalytic material, people have conducted a lot of research. The main research direction is to modify zinc oxide by doping with metal ions, non-metals and semiconductor composites, in order to improve its photocatalytic performance and enable it to be better applied. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of low photocatalytic activity of existing zinc oxide photocatalytic materials, and to provide a method for preparing semiconductor copper oxide and zinc oxide doped photocatalytic materials with a wide light response range and a low bandgap width. The method is simple and easy to implement, and the prepared photocatalytic material can effectively remove trace thallium in water.

[0006] The preparation method of the zinc oxide and copper oxide co-doped photocatalytic material of the present invention is achieved by the following steps:

[0007] 1. Weigh hexadecyltrimethylammonium bromide, zinc nitrate hexahydrate and copper nitrate trihydrate, add deionized water to obtain a precursor reaction solution, and dropwise add 0.5-0.8 mol / L sodium hydroxide solution to the precursor reaction solution (slowly and uniformly) under magnetic stirring conditions to obtain a reaction solution after reaction;

[0008] 2. The reaction solution obtained in step 1 is placed in a reaction kettle and subjected to a hydrothermal reaction in an oven at 160-200° C., the solid precipitate is collected, and then the precipitate is washed with anhydrous ethanol and deionized water until it becomes neutral, and the reactant is obtained after centrifugation and drying;

[0009] 3. placing the reactants in a muffle furnace and calcining them at 400-600° C. to obtain a zinc oxide and copper oxide co-doped photocatalytic material;

[0010] The molar ratio of zinc to copper in the zinc nitrate hexahydrate, the zinc nitrate trihydrate and the copper nitrate in step 1 is 100:(2-8).

[0011] The application of the zinc oxide and copper oxide co-doped photocatalytic material of the present invention is to use the zinc oxide and copper oxide co-doped photocatalytic material as a water treatment agent to remove (trace) thallium in water.

[0012] The preparation method of the zinc oxide and copper oxide co-doped photocatalytic material of the present invention and its application include the following beneficial effects:

[0013] The present invention utilizes a simple and easy-to-operate hydrothermal method to prepare a zinc oxide-copper oxide composite photocatalytic material, and improves the shortcomings of zinc oxide alone as a photocatalytic material, such as a narrow light absorption range and a high photogenerated electron-hole recombination rate, by doping with copper oxide. Finally, the optimal doping ratio, reaction temperature, optimal concentration of sodium hydroxide and other reaction conditions of the composite photocatalytic material are determined through experiments. Finally, the composite photocatalytic material prepared by the present invention has high photoelectric conversion efficiency, high photocatalytic activity, is green and pollution-free, and has visible light photocatalytic activity, so that the photocatalytic material can be more widely used.

[0014] The zinc oxide and copper oxide co-doped photocatalytic material prepared by the present invention can oxidize monovalent thallium to trivalent thallium, promote the precipitation of trivalent thallium ions, and simultaneously utilize the adsorption performance of the surface of the photocatalyst to achieve the effect of removing thallium. After the wastewater containing 0.01 mg / L of thallium is treated, the metal thallium content in the wastewater is lower than 0.002 mg / L, which meets the national standard of "Inorganic Chemical Industry Pollutant Emission Standard" that the thallium content is lower than 0.005 mg / L. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is an X-ray diffraction pattern of the zinc oxide and copper oxide co-doped photocatalytic material prepared in Example, wherein 1 represents a zinc oxide and copper oxide molar ratio of 100:2, 2 represents a zinc oxide and copper oxide molar ratio of 100:7, and 3 represents a zinc oxide and copper oxide molar ratio of 100:8;

[0016] Figure 21 is a comparison chart of the effects of zinc oxide and copper oxide co-doped photocatalytic materials prepared in the embodiment and the comparative example on removing thallium under the same reaction time and dosage conditions, wherein ◆ represents the embodiment and ■ represents the comparative example. DETAILED DESCRIPTION

[0017] Specific implementation method 1: The preparation method of the zinc oxide and copper oxide co-doped photocatalytic material in this implementation method is implemented according to the following steps:

[0018] 1. Weigh hexadecyltrimethylammonium bromide, zinc nitrate hexahydrate and copper nitrate trihydrate, add deionized water to obtain a precursor reaction solution, and dropwise add 0.5-0.8 mol / L sodium hydroxide solution to the precursor reaction solution (slowly and uniformly) under magnetic stirring conditions to obtain a reaction solution after reaction;

[0019] 2. The reaction solution obtained in step 1 is placed in a reaction kettle and subjected to a hydrothermal reaction in an oven at 160-200° C., the solid precipitate is collected, and then the precipitate is washed with anhydrous ethanol and deionized water until it becomes neutral, and the reactant is obtained after centrifugation and drying;

[0020] 3. placing the reactants in a muffle furnace and calcining them at 400-600° C. to obtain a zinc oxide and copper oxide co-doped photocatalytic material;

[0021] The molar ratio of zinc to copper in the zinc nitrate hexahydrate, the zinc nitrate trihydrate and the copper nitrate in step 1 is 100:(2-8).

[0022] In step 1 of this embodiment, the hexadecyltrimethylammonium bromide is used as a surfactant, which can effectively control the structure, morphology and performance of the synthesized product.

[0023] The principle of synthesizing zinc oxide and copper oxide co-doped photocatalytic materials in this embodiment is as follows:

[0024] Zn(NO 3 ) 2 6H 2 O+NaOH→Zn(OH) 2 (hydrothermal reaction);

[0025] Cu(NO 3 ) 2 ·3H 2 O+NaOH→Cu(OH) 2 (hydrothermal reaction);

[0026] Zn(OH) 2 +Cu(OH) 2 →ZnO / CuO (drying and calcining to form the final material).

[0027] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the molar ratio of zinc to copper in zinc nitrate hexahydrate, trihydrate and copper nitrate in step 1 is 100:(5-8).

[0028] Specific implementation method three: This implementation method is different from specific implementation method two in that the molar ratio of zinc to copper in zinc nitrate hexahydrate, trihydrate and copper nitrate in step one is 100:7.

[0029] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that in step 1, 0.4 to 0.6 g of hexadecyltrimethylammonium bromide, 4.2 to 4.5 g of zinc nitrate hexahydrate and 0.18 to 0.29 g of copper nitrate trihydrate are weighed, and 80 to 120 mL of deionized water are added.

[0030] Specific implementation mode five: This implementation mode is different from specific implementation mode four in that in step one, 100 mL of a sodium hydroxide solution having a concentration of 0.4 to 0.8 mol / L is added dropwise to the precursor reaction solution under magnetic stirring conditions at 20° C. and 200 r / min, and the reaction time is 30 min.

[0031] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that in step 2, the hydrothermal reaction is carried out in an oven at 180° C. for 3.5 h to 4.5 h.

[0032] Specific implementation method 7: The difference between this implementation method and any one of specific implementation methods 1 to 6 is that the centrifugation treatment in step 2 is performed in a centrifuge at a speed of 4000 r / min for 15 minutes.

[0033] Specific implementation eight: This implementation differs from specific implementations one to seven in that the drying process described in step two is performed in an oven at 80° C. for 12 hours.

[0034] Specific embodiment 9: This embodiment is different from any one of specific embodiments 1 to 6 in that the calcination treatment is performed at 500° C. for 30 minutes in step 3.

[0035] Specific implementation method 10: In this implementation method, the application of the zinc oxide and copper oxide co-doped photocatalytic material is to use the zinc oxide and copper oxide co-doped photocatalytic material as a water treatment agent to remove (trace) thallium in water.

[0036] Embodiment: The preparation method of the zinc oxide and copper oxide co-doped photocatalytic material of this embodiment is implemented according to the following steps:

[0037] 1. Weigh 0.5 g of hexadecyltrimethylammonium bromide, 4.455 g of zinc nitrate hexahydrate and copper nitrate trihydrate, add 100 mL of deionized water to obtain a precursor reaction solution, and use a constant temperature magnetic stirrer to slowly drop 100 mL of a 0.6 mol / L sodium hydroxide solution into the precursor reaction solution at 20°C and 200 r / min, and react for 30 minutes to obtain a reaction solution;

[0038] 2. The reaction solution obtained in step 1 is placed in a reactor and subjected to hydrothermal reaction in an oven at 180°C for 4 hours. The supernatant of the reaction solution is poured off, the solid precipitate is collected, and the precipitate is washed with anhydrous ethanol and deionized water until it is neutral. The precipitate is then placed in a centrifuge and centrifuged at 4000 r / min for 15 minutes. The precipitate is placed in an oven at 80°C and dried for 12 hours to obtain a reactant.

[0039] 3. The reactants were placed in a muffle furnace and calcined at 500° C. for 30 min to obtain a zinc oxide and copper oxide co-doped photocatalytic material.

[0040] In step 1 of this embodiment, the molar ratios of zinc to copper are 100:1, 100:2, 100:5, 100:7, 100:8 and 100:10 for zinc oxide and copper oxide respectively, and the sample number groups are ranked 1-6 in terms of molar ratio.

[0041] Comparative Example: This example is different from Example 1 in that 100 mL of 0.3 mol / L sodium hydroxide solution is slowly and uniformly added to the precursor reaction solution at 20°C and 200 r / min using a constant temperature magnetic stirrer.

[0042] In this embodiment, the monovalent thallium is oxidized to trivalent thallium by co-doping the photocatalytic material with zinc oxide and copper oxide to precipitate it, and then further adsorbed by the adsorption effect on the surface of the photocatalyst, so as to better remove trace thallium in water.

[0043] pass Figure 1 It can be seen that the zinc oxide and copper oxide co-doped photocatalytic material was prepared in this embodiment, and the higher the copper oxide doping ratio, the more obvious its characteristic diffraction peak. The copper oxide semiconductor band gap is narrow and can absorb visible light. In addition, the positions of the energy levels of zinc oxide and copper oxide match each other. When illuminated, the two can form a heterojunction, and the photogenerated carriers can also be effectively separated. This is an effective method to broaden the latter's light absorption range and promote charge separation.

[0044] By comparing the effects of the embodiment and the comparative embodiment on degrading trace thallium in wastewater, it can be seen that the zinc oxide and copper oxide co-doped photocatalytic material prepared in the embodiment has stable performance and can efficiently remove thallium in wastewater. In wastewater containing thallium at a concentration of 0.01 mg / L, 1 g / L of photocatalytic material is added, a xenon lamp is used as the light source and magnetic stirring is performed, and the irradiation time is 2 hours. The removal rate of the zinc oxide and copper oxide co-doped photocatalytic material with a zinc-copper molar ratio of 100:7 in the embodiment can reach up to 89.6%, while the removal rate of the photocatalytic material in the comparative embodiment is 60.8%.

[0045] The above descriptions are merely embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any use of the contents of the present invention's specification and drawings, or direct or indirect use in other related technical fields, is also included in the patent protection scope of the present invention.

Claims

1. Application of zinc oxide and copper oxide co-doped photocatalytic materials, characterized in that The zinc oxide and copper oxide co-doped photocatalytic material is used as a water treatment agent to remove thallium from water; The preparation method of the zinc oxide and copper oxide co-doped photocatalytic material is achieved by the following steps:

1. Weigh hexadecyltrimethylammonium bromide, zinc nitrate hexahydrate and copper nitrate trihydrate, add deionized water to obtain a precursor reaction solution, and dropwise add 0.5-0.8 mol / L sodium hydroxide solution to the precursor reaction solution under magnetic stirring to obtain a reaction solution after reaction; 2. Put the reaction solution obtained in step 1 into a reactor and perform hydrothermal reaction in an oven at 160-200° C., collect the solid precipitate, and then wash the precipitate with anhydrous ethanol and deionized water until it is neutral, and obtain the reactant after centrifugation and drying; 3. placing the reactants in a muffle furnace and calcining them at 400-600° C. to obtain a zinc oxide and copper oxide co-doped photocatalytic material; The molar ratio of zinc to copper in the zinc nitrate hexahydrate and copper nitrate trihydrate described in step 1 is 100:(5-8).

2. The use of zinc oxide and copper oxide co-doped photocatalytic material according to claim 1, characterized in that In step 1, the molar ratio of zinc to copper in zinc nitrate hexahydrate, trihydrate and copper nitrate is 100:

7.

3. The use of zinc oxide and copper oxide co-doped photocatalytic material according to claim 1, characterized in that In step 1, weigh 0.4-0.6 g of hexadecyltrimethylammonium bromide, 4.2-4.5 g of zinc nitrate hexahydrate, and 0.18-0.29 g of copper nitrate trihydrate, and add 80-120 mL of deionized water.

4. The use of zinc oxide and copper oxide co-doped photocatalytic material according to claim 3, characterized in that In step 1, 100 mL of a 0.4-0.8 mol / L sodium hydroxide solution was added dropwise to the precursor reaction solution at 20° C. and 200 r / min of magnetic stirring, and the reaction time was 30 min.

5. The use of zinc oxide and copper oxide co-doped photocatalytic material according to claim 1, characterized in that In step 2, the hydrothermal reaction is carried out in an oven at 180° C. for 3.5 h to 4.5 h.

6. The use of zinc oxide and copper oxide co-doped photocatalytic material according to claim 1, characterized in that The centrifugation in step 2 is carried out in a centrifuge at a speed of 4000 r / min for 15 min.

7. The use of zinc oxide and copper oxide co-doped photocatalytic material according to claim 1, characterized in that The drying process described in step 2 is drying in an oven at 80° C. for 12 h.

8. The use of zinc oxide and copper oxide co-doped photocatalytic material according to claim 1, characterized in that In step 3, the sintered product is calcined at 500° C. for 30 min.

Citation Information

Patent Citations

  • CuO / ZnO composite nano-catalyst, and preparation method and application thereof

    CN106622253A

  • Solid catalyst for dimethyl carbonate and oxamide co-production process and preparation method of solid catalyst

    CN106669684A

  • 3D flower cluster-like nanometer zinc oxide composite silver material, and preparation method and application thereof

    CN110090646A

  • Copper tungstate@zinc oxide composite photocatalyst, preparation method and application thereof

    CN110252326A

  • Mesoporous nanorod-like catalyst as well as preparation method and application thereof

    CN111871417A