Polishing liquid for chemical mechanical polishing of single crystal diamond and preparation method thereof
By combining single crystal diamond powder, H2O2 and Fe2(SO4)3 in the polishing fluid, and adjusting the redox potential and PH value, the problem of single crystal diamond being difficult to oxidize is solved, and efficient ultra-smooth surface processing and high removal rate are achieved.
Patent Information
- Application Number
- CN202210623307.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-01
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-06-01
AI Technical Summary
Existing polishing fluids are difficult to effectively oxidize single crystal diamond, resulting in low processing efficiency and poor surface quality, making it difficult to meet the needs of semiconductor materials under high temperature, high pressure, and high power conditions.
Use a polishing solution containing single crystal diamond powder with an average particle size of 0.25~0.5μm, 30% H2O2 solution and 0.1mol/L~1 mol/L Fe2(SO4)3 solution, and ensure dispersion through ultrasonic cleaning and magnetic stirring. Stability, and use the ORP value to adjust the oxidation ability to form a polishing solution with a pH value of 2 to 4.
It achieves an ultra-smooth surface of Sa﹤0.1nm, Sq﹤0.2nm, and Sz﹤5nm and a removal rate of 750~1000nm/h, which significantly improves the oxidation ability and processing efficiency of single crystal diamond.
Smart Images

Figure CN115109520B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polishing liquids, in particular to a polishing liquid used for polishing hard, brittle and difficult-to-oxidize materials, and more particularly to a polishing liquid used for chemical mechanical polishing of single crystal diamonds and a preparation method thereof. Background Art
[0002] As electronic devices develop towards high power, single crystal silicon cannot meet the demand under complex conditions of high temperature, high pressure and high frequency. Therefore, the emergence of a new material that can be used under complex conditions of high temperature, high pressure, high frequency and high power will greatly promote the development of the semiconductor field. Single crystal diamond can be semiconductorized after being doped with an appropriate amount of boron atoms. Its excellent properties of high thermal conductivity, high temperature resistance and ultra-wide bandgap make it a fourth-generation semiconductor material and is also regarded as the most ideal semiconductor material in the future [1-5]. However, no matter how superior the properties of the material are, it needs to have a good surface quality before application, otherwise its excellent performance cannot be brought into play or even cannot be applied. Since single crystal diamond is the hardest material in nature, it is brittle and has extremely stable chemical properties (it hardly reacts with any acid or alkali reagents at room temperature), it is difficult to remove and easy to damage during processing. It is a typical hard and brittle material that is difficult to process, which brings huge challenges to single crystal diamond processing.
[0003] Chemical mechanical polishing (CMP) is an effective polishing method for obtaining ultra-smooth surfaces and can be used for processing low-damage surfaces of wafers. CMP uses the chemical reaction between chemical substances to form a softer oxide layer between the polishing liquid and the substrate. The oxide layer is removed under the mechanical action of abrasive particles, and finally an ultra-smooth surface is obtained. The composition of the chemical polishing liquid directly affects the reaction speed, polishing quality and efficiency during the polishing process. For ultra-hard materials with extremely high chemical inertness, the oxidation effect of the polishing liquid plays a decisive role in the final surface quality. The CMP method is currently a mature polishing method for obtaining ultra-smooth and ultra-low damage surfaces, but the current efficiency of polishing diamonds is extremely low. Relying solely on the mechanical action of abrasive particles cannot meet the needs of diamond processing. The hard and brittle characteristics of single-crystal diamonds make them difficult to process, and their extremely low chemical inertness makes them difficult to oxidize. Therefore, how to increase the oxidation rate of the single-crystal diamond surface is the key to improving surface quality and removal rate.
[0004] At present, domestic and foreign scholars have done a lot of research on the selection and optimization of polishing liquid in the diamond CMP process. 2 FeO 4 , KMnO 4 , Na 2 MoO 4 , K 2 Cr 2 O 7 , CrO3 , KIO 4 , H 2 O 2 , (NH 4 ) 2 S 2 O 8, Fe(NO 3 ) 3 , oxalic acid (C 2 H 2 O 4 ), sodium thiosulfate (Na 2 S 2 O 3 ), molten LiNO 3 and KNO 3 etc. are used as polishing fluids in the diamond CMP process. However, due to the strong chemical inertness of diamond, it is difficult to be oxidized. Under the existing chemical polishing fluids, the diamond removal rate and the surface quality after polishing still have a lot of room for improvement. There is a bottleneck in processing diamonds relying solely on conventional polishing fluids. Summary of the invention
[0005] In view of the above technical problems, a polishing liquid for chemical mechanical polishing of single crystal diamond and a preparation method thereof are provided.
[0006] The technical means adopted by the present invention are as follows:
[0007] A polishing liquid for chemical mechanical polishing of single crystal diamond, the polishing liquid comprising:
[0008] Single crystal diamond powder with an average particle size of w0.25~w0.5μm;
[0009] Mass fraction is 30%H 2 O 2 solution, and
[0010] 0.1mol / L~1 mol / L Fe 2 (SO 4 ) 3 Solution;
[0011] Single crystal diamond powder, H 2 O 2 Solution and Fe 2 (SO 4 ) 3 The mass ratio is 15:5000:1~100:5000:1.
[0012] The pH value of the polishing liquid is 2-4.
[0013] The ORP value of the polishing liquid is 530mv~550mv.
[0014] The present invention also discloses a method for preparing a polishing liquid for chemical mechanical polishing of single crystal diamond, comprising:
[0015] Add 30% H2O by mass into single crystal diamond powder with an average particle size of w0.25 μm~w0.5 μm. 2 O 2 solution to obtain a first mixed solution;
[0016] Using an ultrasonic cleaner to vibrate the first mixed solution to avoid agglomeration of abrasive particles and to evenly disperse the diamond powder in the solution;
[0017] Prepare 0.1 mol / L~1 mol / L Fe 2 (SO4) 3 The solution is added to the first mixed solution to obtain a second mixed solution, and the second mixed solution satisfies the single crystal diamond powder, H 2 O 2 Solution and Fe 2 (SO 4 ) 3 The mass ratio of Fe is 15:5000:1~100:5000:1; when adding Fe 2 (SO4) 3 During the solution process, an oxidation-reduction potentiometer is used to detect the ORP value in real time (ORP is a parameter indicating the oxidation capacity of the solution. The larger the value, the greater the oxidation capacity). 2 (SO 4 ) 3 After adding in the above proportion, the ORP value of the second mixed solution is 530mv~550mv;
[0018] The pH value of the second mixed solution is adjusted to 2-4 using dilute hydrochloric acid to obtain a polishing solution.
[0019] Before polishing, the polishing liquid is stirred by a magnetic stirrer and a rotor to keep good dispersion stability of the polishing liquid, thereby avoiding scratches and pits on the workpiece due to agglomeration of abrasive particles during the polishing process.
[0020] Compared with the prior art, the present invention has the following advantages:
[0021] 1. Using this polishing liquid to polish diamond can obtain an ultra-smooth surface with Sa﹤0.1nm, Sq﹤0.2nm, Sz﹤5nm (measuring range 868μmⅹ868μm) and a removal rate of 750~1000nm / h.
[0022] 2. The ORP value of the polishing liquid is 530mv~550mv, which has a large oxidation capacity.
[0023] 3. Use the ORP redox instrument to detect the oxidizing property of the polishing liquid in real time. The device can regulate the oxidizing capacity of the polishing liquid in real time to prevent the self-oxidation-reduction reaction of the polishing liquid caused by excessive iron ion concentration, thereby losing the oxidizing ability of the diamond workpiece. It also ensures that the polishing liquid has a greater oxidizing ability to the greatest extent.
[0024] Based on the above reasons, the present invention can be widely promoted in the fields of polishing liquid and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 This is a surface diagram of the diamond after polishing with polishing liquid in Example 1 of the present invention.
[0027] Figure 2 This is a surface diagram of the diamond after polishing with polishing liquid in Example 2 of the present invention. DETAILED DESCRIPTION
[0028] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0029] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0031] Unless otherwise specifically stated, the relative arrangement of the parts and steps described in these embodiments, the numerical expressions and numerical values do not limit the scope of the present invention. At the same time, it should be clear that, for ease of description, the sizes of the various parts shown in the drawings are not drawn according to the actual proportional relationship. The technology, methods and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but in appropriate cases, the technology, methods and equipment should be regarded as part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar numbers and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further discussed in subsequent drawings.
[0032] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings. They are only for the convenience of describing the present invention and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of the present invention: the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.
[0033] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below their position devices or structures". Thus, the exemplary term "above" may include both "above" and "below". The device may also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0034] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0035] A polishing liquid for chemical mechanical polishing of single crystal diamond, comprising:
[0036] Single crystal diamond powder with an average particle size of w0.25μm~w0.5μm;
[0037] Mass fraction is 30%H 2 O 2 solution, and
[0038] 0.1mol / L~1 mol / L Fe 2 (SO 4 ) 3 Solution;
[0039] The mass ratio of single crystal diamond powder, H2O2 solution and Fe2 (SO4)3 is 15:5000:1 to 100:5000:1.
[0040] The pH value of the polishing liquid is 2-4.
[0041] The ORP value of the polishing liquid is 530mv to 550mv.
[0042] The present invention also discloses a method for preparing a polishing liquid for chemical mechanical polishing of single crystal diamond, comprising:
[0043] Add 30% H2O by mass into single crystal diamond powder with an average particle size of w0.25 μm~w0.5 μm. 2 O 2solution to obtain a first mixed solution;
[0044] Using an ultrasonic cleaner to vibrate the first mixed solution to avoid agglomeration of abrasive particles and to evenly disperse the diamond powder in the solution;
[0045] Prepare 0.1 mol / L~1 mol / L Fe 2 (SO4) 3 The solution is added to the first mixed solution to obtain a second mixed solution, and the second mixed solution satisfies the single crystal diamond powder, H 2 O 2 Solution and Fe 2 (SO 4 ) 3 The mass ratio of Fe is 15:5000:1~100:5000:1; when adding Fe 2 (SO 4 ) 3 During the solution process, an oxidation-reduction potentiometer is used to detect the ORP value in real time (ORP is a parameter indicating the oxidation capacity of the solution. The larger the value, the greater the oxidation capacity). 2 (SO 4 ) 3 After adding in the above proportion, the ORP value of the second mixed solution is 530mv~550mv;
[0046] The pH value of the second mixed solution is adjusted to 2-4 using dilute hydrochloric acid to obtain a polishing solution.
[0047] Before polishing, the polishing liquid is stirred by a magnetic stirrer and a rotor to keep good dispersion stability of the polishing liquid, thereby avoiding scratches and pits on the workpiece due to agglomeration of abrasive particles during the polishing process.
[0048] Example 1
[0049] like Figure 1 As shown in the figure, a method for preparing a polishing liquid for chemical mechanical polishing of single crystal diamond is as follows: weigh 30% H 2 O 2 500g of solution and 25g of single crystal diamond powder with an average particle size of w0.25μm; weigh 4g of ferric sulfate solute and place it in a beaker, add 50mL of water, stir to dissolve, transfer to a 100mL volumetric flask, and prepare 0.1mol / L Fe 2 (SO 4 ) 3 Solution 100mL.
[0050] Add 25g of the weighed single crystal diamond powder to the 500g of 30% H 2 O2 The solution was stirred evenly and cleaned with an ultrasonic cleaner for 5 minutes. 2 (SO 4 ) 3 0.1 g of the solution was added to the aforementioned solution, and the pH value of the polishing solution was adjusted to 3 with dilute hydrochloric acid to prepare the required polishing solution.
[0051] The prepared polishing liquid is delivered to the surface of the diamond wafer through a peristaltic pump, and the oxidizing property of the polishing liquid is detected in real time by an ORP redox instrument. The oxidizing capacity of the polishing liquid is regulated in real time by the device to prevent the self-oxidation-reduction reaction of the polishing liquid caused by excessive iron ion concentration, thereby losing the oxidizing capacity of the diamond workpiece, and also ensuring that the polishing liquid has a large oxidizing capacity to the greatest extent. Secondly, the relative rotation between the polishing disk and the workpiece surface is used to bring the polishing liquid to the bottom of the workpiece. The polishing liquid can react with the diamond wafer. Under the action of the catalyst iron salt, hydrogen peroxide can generate a large number of hydroxyl radicals (·OH). The hydroxyl radical has a higher oxidation electrode potential (E=2.8eV) than other oxidants, so that the carbon atoms on the surface of the diamond workpiece combine with ·OH to generate CO or CO 2 is removed (see formula (1) (2)), or a snowflake-like oxide layer is formed on the surface of the diamond, Fe 3+ Requires H 2 O 2 Fe 2+ (See formula (3)), then Fe 2+ Consumption of H 2 O 2 In order to generate •OH (see formula (4)), this allows diamond to be continuously oxidized for a long time.
[0052] (1) Diamond + 2•OH → CO↑ + H 2 O
[0053] (2) Diamond + 4•OH→ CO 2 ↑ + 2H 2 O
[0054] (3) Fe 3+ + H 2 O 2 → Fe 2+ + H + + OOH•
[0055] (4) Fe 2+ + H 2 O 2 → Fe 3+ + OH- + OH•
[0056] Furthermore, in this embodiment, the free abrasive diamond powder is contacted with the surface of the diamond wafer for processing. The mechanical action of the diamond powder can destroy the lattice structure of the diamond, reduce the activation energy of the diamond chemical reaction, indirectly accelerate the oxidation of the diamond wafer, and improve the polishing efficiency. After 1 hour of polishing, an ultra-smooth surface with Sa=0.079nm, Sq=0.100nm, Sz=2.744 nm (measuring range 868μmx 868μm) and a removal rate of 881nm / h can be obtained (as shown in the attached Figure 1 As shown in Figure 2), the experiment verifies that the polishing liquid has a large oxidation capacity and can achieve efficient and ultra-low damage processing of single crystal diamond.
[0057] Example 2
[0058] like Figure 2 As shown in the figure, a method for preparing a polishing liquid for chemical mechanical polishing of single crystal diamond is as follows: weigh 30% H 2 O 2 500g of solution and 7.5g of single crystal diamond powder with an average particle size of w0.25μm; weigh 4g of ferric sulfate solute and place it in a beaker, add 50mL of water, stir to dissolve, transfer to a 100mL volumetric flask, and prepare 0.1mol / L Fe 2 (SO 4 ) 3 Solution 100mL.
[0059] Add 7.5 g of the weighed single crystal diamond powder to the 500 g of 30% H 2 O 2 The solution was stirred evenly and cleaned with an ultrasonic cleaner for 5 minutes. 2 (SO 4 ) 3 Add 0.1 g of the solution into the above solution, adjust the pH value of the polishing solution to 3 with dilute hydrochloric acid to prepare the required polishing solution.
[0060] The prepared polishing liquid is delivered to the surface of the diamond wafer through a peristaltic pump, and the oxidizing property of the polishing liquid is detected in real time by an ORP redox instrument. The oxidizing capacity of the polishing liquid is regulated in real time by the device to prevent the self-oxidation-reduction reaction of the polishing liquid caused by excessive iron ion concentration, thereby losing the oxidizing capacity of the diamond workpiece, and also ensuring that the polishing liquid has a large oxidizing capacity to the greatest extent. Secondly, the relative rotation between the polishing disc and the workpiece surface is used to bring the polishing liquid to the bottom of the workpiece, where the polishing liquid can react with the diamond wafer. Under the action of the catalyst iron salt, hydrogen peroxide can generate a large number of hydroxyl radicals (·OH).
[0061] Furthermore, in this embodiment, the free abrasive diamond powder is contacted with the surface of the diamond wafer for processing. The mechanical action of the diamond powder can destroy the lattice structure of the diamond, reduce the activation energy of the diamond chemical reaction, indirectly accelerate the oxidation of the diamond wafer, and improve the polishing efficiency. After 1 hour of polishing, an ultra-smooth surface with Sa=0.076nm, Sq=0.096nm, Sz=2.357 nm (measuring range 868μmx 868μm) and a removal rate of 751nm / h can be obtained (as shown in the attached Figure 2 As shown in Figure 2), the experiment verifies that the polishing liquid has a large oxidation capacity and can achieve efficient and ultra-low damage processing of single crystal diamond.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a polishing liquid for chemical mechanical polishing of single crystal diamond, characterized in that: It is composed of the following substances: Single crystal diamond powder with an average particle size of w0.25μm; The mass fraction is 30% H2O2 solution; 0.1 mol / L Fe2(SO4)3 solution; Add 7.5 g of single crystal diamond powder to 500 g of 30% H2O2 solution, stir evenly, and use an ultrasonic cleaner to shake and clean for 5 minutes. Add 0.1 g of 0.1 mol / LFe2(SO4)3 solution to solution I, and adjust the pH value of the polishing solution to 3 with dilute hydrochloric acid.
2. The polishing liquid prepared by the method for preparing a polishing liquid for chemical mechanical polishing of single crystal diamond as claimed in claim 1.