Nylon fabric
By adding network points to the fine denier multi-filament warp yarn and adjusting the weaving parameters, the problem of difficulty in taking into account both lightness and strength in the prior art is solved, and the industrial production and quality improvement of ultra-light and thin nylon fabrics are achieved.
Patent Information
- Application Number
- CN202210591741.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-08-31
AI Technical Summary
While pursuing lightness and thinness, existing clothing fabrics are difficult to reduce the weight and thickness while ensuring strength, and the production of ultra-fine multi-filament woven fabrics is difficult, resulting in the inability to achieve industrial mass production.
The Karl Mayer network machine is used to add network points to the fine denier multifilament warp yarn to increase the bundling and strength of the fibers. By adjusting the jet angle and tension parameters of the water jet loom, we ensure the normal delivery of the weft yarn and the weaving process. Avoid breaking the yarn.
Ultra-light and thin nylon fabrics have been prepared, with excellent hand feel and quality parameters, can be applied to industrial production, and the softness and strength of the fabric are improved.
Smart Images

Figure BDA0003665530380000081
Abstract
Description
[0001] This application is a divisional application of the invention patent application with application date of August 31, 2020, application number 202010894729.3, and invention name “Nylon fabric and preparation method thereof”. Technical Field
[0002] The invention relates to the technical field of textiles, and in particular to a nylon fabric. Background Art
[0003] The fashion trend of clothing fabrics is closely related to the progress of science and technology. In the early days, people wore clothes to cover their bodies and keep warm. With the continuous advancement of science and technology and the continuous improvement of people's living standards, people have put forward higher requirements for the quality of clothing fabrics, which should not only show visual beauty but also good touch. Most of the original raw materials of existing chemical fiber fabrics come from oil, which is also a non-renewable resource. The thicker our fabrics are, the more oil resources we consume. In recent decades, with the development of industry, the rapid construction of cities, the increase in carbon emissions, and global warming, it has become an inevitable trend to make fabrics lighter and thinner while maintaining the function of clothing.
[0004] Commonly used clothing fabrics, the weight of fabrics has increased from 150g / m 2 ~200g / m 2 Down to 80g / m 2 ~130g / m 2 ; There are also lighter ones up to 35g / m 2 ~40g / m 2 The fabrics are made of 0.1mm-0.7mm thick fabrics, but the tearing strength of the fabrics cannot reach 9N. The thickness of the fabrics is 0.1mm-0.7mm. The way these woven fabrics are made is generally that the warp yarns are finer and the weft yarns are coarser, and the density of the fabrics is not high. There are also lightweight woven fabrics that use the warp yarns of the upper and lower layers to be arranged at intervals according to different densities. It uses the connecting warp yarns to connect the upper and lower layers of woven fabrics into a whole interval woven fabric, forming a loose composite fabric structure. There are also thinly coated and waxed nylon fabrics, and the fabric weight reaches 35g / m 2 ~50g / m 2 However, the strength of the coated fabric is greatly reduced and cannot meet the needs of use.
[0005] There are already 7D-12D fine multifilaments, which can further reduce the weight and thickness of fabrics while ensuring the strength of fabrics after being woven into fabrics. However, it is difficult to produce ultra-fine multifilament woven fabrics, and warps are easily broken during the production process. Most companies only stay at the stage of trial samples, and cannot produce large quantities of goods. There is no output and quality, and there is no mature process for mass production. Summary of the invention
[0006] In view of this, in order to overcome the defects of the prior art, the object of the present invention is to provide an ultra-light nylon fabric of 7D-12D fine denier multifilament.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A nylon fabric is formed by interweaving warp yarns and weft yarns, both of which are fine denier multifilaments. The preparation method of the nylon fabric comprises the steps of warping, warp yarn sizing, weaving beam preparation, and weaving on a machine. In the warping step, the warp yarn is subjected to a network point treatment to increase the number of network points of the warp yarn so that the network on the yarn is more numerous and denser. The network treatment is performed by using a yarn network device such as a Karl Mayer network machine and other equipment for processing.
[0009] By using the Karl Mayer interlacing machine to add interlacing points to the fine-denier multifilament warp yarn during the warping process, the number of interlacing points of the warp yarn is increased, and the fiber bundling, cohesion and strength are increased, thus avoiding the problem of warp breakage during warping and subsequent steps, which results in the inability to produce or the poor quality of the prepared fabric.
[0010] According to some preferred implementation aspects of the present invention, the warp yarn and the weft yarn are both fine denier multifilament 7D-12D nylon filaments. The fabrics prepared from 7D-12D nylon filaments have better properties such as hand feel and gram weight. However, the existing preparation methods cannot prepare long fabrics from them. By using the method of increasing the number of warp network points in this application and matching the specific preparation process, 7D-12D nylon filaments can be prepared into fabrics and applied to industrial production.
[0011] According to some preferred implementation aspects of the present invention, after the warping step is completed, the total number of network points on the warp yarn is 18 to 30 per meter.
[0012] According to some preferred implementation aspects of the present invention, after the warping step, the total number of network points on the warp yarn is 20 to 25 per meter. If the number of network points is too small, the fabric cannot be prepared or the prepared fabric is of poor quality. If the number of network points is too high, the energy consumption and cost are high.
[0013] According to some preferred implementation aspects of the present invention, in the weaving step, the spray angle of the loom nozzle during weft insertion is 105° to 108°, the angle from water to the lower edge of the cloth is 225° to 230°, and the angle from the weft yarn to the lower edge of the cloth is 245° to 250°. In the prior art, the spray angle during weft insertion is 100°. In the present application, the water spraying time of the nozzle is delayed compared to the traditional water spraying time, which can make the opening angle of the upper and lower groups of warp yarns larger, and avoid the water reaching the warp yarn and interrupting the warp yarn. The angle from water to the lower edge of the cloth (discarded edge) and the angle from the weft yarn to the lower edge of the cloth (discarded edge) are both increased, the water is slow (delayed), and the weft yarn of weft insertion is slow, and the softness of the fabric finally prepared is better.
[0014] According to some preferred implementation aspects of the present invention, in the warping step, the unwinding tension of the monofilament on the warping creel is 3-5 g / filament, and the monofilament tension when the warping beam is wound is 4-6 g / filament. A low tension process is used during the warping process to ensure the strength of the fine denier multifilament warp yarn.
[0015] According to some preferred implementation aspects of the present invention, in the warp sizing step, the warp yarn unwinding tension of the warping beam is 6-8 kg, the single yarn tension when entering the drying room is 4-6 g / strand, and the sizing beam winding tension is 4-6 kg.
[0016] According to some preferred embodiments of the present invention, in the weaving shaft preparation step, the unwinding tension of each pulp shaft is 7-9 kg, and the winding tension of the weaving shaft when it becomes a weaving shaft is 70-80 kg.
[0017] According to some preferred embodiments of the present invention, the warp yarn density of the nylon fabric is 95-105 yarns / cm, the weft yarn density is 73-95 yarns / cm, and the mass of the nylon fabric is 20-30 g / m 2 .
[0018] Another object of the present invention is to provide a nylon fabric prepared by the preparation method as described above.
[0019] In some specific embodiments of the present invention, the method for preparing nylon fabric specifically comprises the following steps:
[0020] 1) Warping: used to wind the warp yarn on the warping beam.
[0021] The specific parameters are: the density of the warp yarn is 8-9 yarns / cm, the tension of the monofilament on the warping creel is 3-5g / thread, and the pressure of the pressure roller is 1.5-2kg / cm 2 ; The single yarn tension when the warping beam is taken up is 4 to 6 g / filament.
[0022] 2) Warp sizing: The warp yarn wound on the warping beam is sizing.
[0023] The warping beam in step 1) is transported to the sizing car for sizing, and the sizing concentration of the sizing agent is 13-15%. The warp yarns of the warping beam are unwound, passed through the sizing tank filled with sizing agent, and the sized warp yarns are initially dried in four drying rooms, and then dried by five cylinders, and then wound on the sizing beam.
[0024] The unwinding tension of the warp yarn on the warping beam is 6-8kg, the monofilament tension when entering the drying room is 4-6g / thread, and the winding tension of the sizing beam is 4-6kg. When sizing, the temperature of the sizing material in the sizing tank is 50-55℃, the drying room temperature is 140-145℃, and the cylinder drying temperature is 115-100℃. The sizing rate of the warp yarn is 12-13%. The shrinking time of the sized warp yarn is 30h.
[0025] 3) Weaving beam preparation: combine multiple pulp beams into a weaving beam.
[0026] The pulp beams in step 2) are combined into a weaving beam according to the designed warp density of 85 to 95 strands / cm. The unwinding tension of each pulp beam is 7 to 9 kg, and the winding tension of the weaving beam is 70 to 80 kg when the weaving beam is combined into one. Then the heald and reed are drawn in, and the weaving is ready for weaving on the machine.
[0027] 4) Weaving: The weft is inserted through a water jet loom to interweave the warp and weft yarns to form a fabric.
[0028] Place the fine denier multifilament 7D~12D nylon filament of the weft yarn raw material on the weft yarn rack; pull the weft yarn through the wire guide hole and the weft storage device, and lead it out from the nozzle. The upper machine tension of the weaving beam is adjusted to 800~1000N, and the length range of the weft yarn measurement is 188cm~192cm. During weaving, the angle of the weft yarn scissors at the lower edge of the cloth is 10°, and the angle of the weft yarn scissors at the upper edge of the cloth is 20°. The spray angle of the nozzle during weft insertion is 105°~108°, the angle of water to the lower edge of the cloth (discarded edge) is 225°~230°, the angle of the weft yarn to the lower edge of the cloth (discarded edge) is 245°~250°, the angle of the lower weft detection is 315°~320°, and the angle of the comprehensive flattening time is 345°~350°.
[0029] Due to the adoption of the above technical scheme, compared with the prior art, the benefits of the present invention are as follows: the nylon fabric of the present invention performs a network point treatment on the fine denier multifilament warp yarn during the warping process, thereby increasing the number of network points of the warp yarn, increasing the bundling, cohesion and strength of the fibers, and avoiding the problem of warp breakage during warping and subsequent steps, resulting in the inability to produce or the poor quality of the prepared fabric, so that the prepared nylon fabric is ultra-light and thin. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0031] Example 1
[0032] The method for preparing the ultra-light and thin nylon fabric in this embodiment specifically comprises the following steps:
[0033] 1) Warping: used to wind the warp yarn on the warping beam.
[0034] In this embodiment, the total number of network points on the warp yarn is 18.
[0035] The warp yarn in this embodiment is a fine denier multifilament nylon filament of 7D to 12D. A Karl Mayer network machine is used to add network points to the warp yarn to increase the number of network points of the warp yarn so that the total number of network points on the warp yarn is 18 to 30 per meter. Increasing the number of network points of the warp yarn increases the bundling, cohesion and strength of the fiber, and avoids the problem of warp breakage during warping and subsequent steps, which makes it impossible to produce or the quality of the prepared fabrics poor. If the number of network points is too small, the fabric cannot be prepared or the quality of the prepared fabric is poor. If the number of network points is too high, the energy consumption and cost are high. The total number of network points on the warp yarn in this embodiment is 18.
[0036] The specific parameters are: the density of the warp yarn is 8-9 yarns / cm, the tension of the monofilament on the warping creel is 3g / thread, and the pressure of the pressure roller is 1.5kg / cm 2 The tension of the single filament when winding on the warping beam is 4g / filament. The low tension process is adopted in the warping process to ensure the strength of the fine denier multifilament warp yarn.
[0037] 2) Warp sizing: The warp yarn wound on the warping beam is sizing.
[0038] The warping beam in step 1) is transported to the sizing truck for sizing, and the sizing concentration of the sizing agent is 13%. The warp yarns of the warping beam are unwound, passed through the sizing tank filled with sizing agent, and the sizing warp yarns are preliminarily dried in four drying rooms, and then dried by five cylinders, and then wound on the sizing beam.
[0039] The unwinding tension of the warp yarn of the warping beam is 6kg, the monofilament tension when entering the drying room is 4g / thread, and the winding tension of the sizing beam is 4kg. When sizing, the temperature of the sizing material in the sizing tank is 50-55℃, the drying room temperature is 140-145℃, and the cylinder drying temperature is 115℃. The sizing rate of the warp yarn is 12%. The shrinking time of the sized warp yarn is 30h.
[0040] 3) Weaving beam preparation: combine multiple pulp beams into a weaving beam.
[0041] The pulp beams in step 2) are combined into a weaving beam according to the warp density of 85 to 95 strands / cm designed for the weaving machine. The unwinding tension of each pulp beam is 7kg, and the winding tension of the weaving beam is 70kg when it is combined into one weaving beam. Then the heald and reed are drawn in, and the weaving machine is ready for weaving.
[0042] 4) Weaving: The weft is inserted through a water jet loom to interweave the warp and weft yarns to form a fabric.
[0043] Place the fine denier multifilament 7D-12D nylon filament of the weft yarn raw material on the weft yarn rack; pull the weft yarn through the wire guide hole and the weft storage device, and lead it out from the nozzle. The upper machine tension of the weaving beam is adjusted to 800N, and the length range of the weft yarn measurement is 188cm. During weaving, the angle of the weft yarn scissors at the lower edge of the cloth is 10°, the angle of the weft yarn scissors at the upper edge of the cloth is 20°, the spray angle of the nozzle water during weft insertion is 105°, the angle of water to the lower edge of the cloth (discarded edge) is 225°, the angle of the weft yarn to the lower edge of the cloth (discarded edge) is 245°, the angle of the lower weft detection is 315°, and the angle of the comprehensive flattening time is 345°.
[0044] In the prior art, the spray angle during weft insertion is 100°. In the present application, the spray time of the nozzle is delayed compared to the traditional spray time, which can make the opening angle of the upper and lower warp yarns larger, and avoid the water reaching the warp yarns and interrupting the warp yarns. The angles of water to the lower edge of the cloth (discarded edge) and the angles of the weft yarn to the lower edge of the cloth (discarded edge) are increased, the water is slow (delayed), and the weft yarn is slow to be inserted, and the nylon fabric finally prepared has better softness.
[0045] The warp yarns and weft yarns in this embodiment are both fine-denier multifilament nylon filaments of 7D to 12D. The nylon fabric prepared from 7D to 12D nylon filaments has better properties in terms of hand feel, gram weight and other parameters. However, the existing preparation methods cannot prepare long fabrics. By adopting the method of increasing the number of warp yarn network points in this embodiment and matching the specific preparation process, 7D to 12D nylon filaments can be prepared into ultra-light and thin fabrics and applied to industrial production. The warp yarn density of the prepared nylon fabric is 95 to 105 strands / cm, the weft yarn density is 73 to 95 strands / cm, and the mass is 20 to 30g / m 2 .
[0046] Example 2
[0047] The method for preparing the ultra-light and thin nylon fabric in this embodiment specifically comprises the following steps:
[0048] 1) Warping: used to wind the warp yarn on the warping beam.
[0049] In this embodiment, the total number of network points on the warp yarn is 20.
[0050] The specific parameters are: the density of the warp yarn is 8-9 yarns / cm, the tension of the monofilament on the warping creel is 5g / thread, and the pressure of the pressure roller is 2kg / cm 2 ; The single yarn tension when the warping beam is taken up is 6g / filament.
[0051] 2) Warp sizing: The warp yarn wound on the warping beam is sizing.
[0052] The warping beam in step 1) is transported to the sizing truck for sizing, and the sizing concentration of the sizing agent is 15%. The warp yarns of the warping beam are unwound, passed through the sizing tank filled with sizing agent, and the sizing warp yarns are initially dried in four drying rooms, and then dried by five cylinders, and then wound on the sizing beam.
[0053] The unwinding tension of the warp yarn on the warping beam is 8kg, the monofilament tension when entering the drying room is 6g / thread, and the winding tension of the sizing beam is 6kg. When sizing, the temperature of the sizing material in the sizing tank is 50-55℃, the drying room temperature is 140-145℃, and the cylinder drying temperature is 100℃. The sizing rate of the warp yarn is 13%. The shrinking time of the sized warp yarn is 30h.
[0054] 3) Weaving beam preparation: combine multiple pulp beams into a weaving beam.
[0055] The pulp beams in step 2) are combined into a weaving beam according to the warp density of 85 to 95 strands / cm designed for the weaving machine. The unwinding tension of each pulp beam is 9 kg, and the winding tension of the weaving beam is 80 kg when it is combined into one weaving beam. Then the heald and reed are drawn in, and the weaving machine is ready for weaving.
[0056] 4) Weaving: The weft is inserted through a water jet loom to interweave the warp and weft yarns to form a fabric.
[0057] Place the fine denier multifilament 7D-12D nylon filament of the weft yarn raw material on the weft yarn rack; pull the weft yarn through the wire guide hole and the weft storage device, and lead it out from the nozzle. The upper machine tension of the weaving beam is adjusted to 1000N, and the length range of the weft yarn measurement is 192cm. During weaving, the angle of the weft yarn scissors at the lower edge of the cloth is 10°, the angle of the weft yarn scissors at the upper edge of the cloth is 20°, the spray angle of the nozzle water during weft insertion is 108°, the angle of water to the lower edge of the cloth (discarded edge) is 230°, the angle of the weft yarn to the lower edge of the cloth (discarded edge) is 245°, the angle of the lower weft detection is 320°, and the angle of the comprehensive flattening time is 350°.
[0058] Example 3
[0059] The method for preparing the ultra-light and thin nylon fabric in this embodiment specifically comprises the following steps:
[0060] In this embodiment, the total number of network points on the warp yarn is 25.
[0061] 1) Warping: used to wind the warp yarn on the warping beam.
[0062] The specific parameters are: the density of the warp yarn is 8-9 yarns / cm, the tension of the monofilament on the warping creel is 4g / thread, and the pressure of the pressure roller is 2kg / cm 2 ; The single yarn tension when the warping beam is taken up is 5g / filament.
[0063] 2) Warp sizing: The warp yarn wound on the warping beam is sizing.
[0064] The warping beam in step 1) is transported to the sizing truck for sizing, and the sizing concentration of the sizing agent is 14%. The warp yarns of the warping beam are unwound, passed through the sizing tank filled with sizing agent, and the sizing warp yarns are initially dried in four drying rooms, and then dried by five cylinders, and then wound on the sizing beam.
[0065] The unwinding tension of the warp yarn of the warping beam is 7kg, the monofilament tension when entering the drying room is 5g / thread, and the winding tension of the sizing beam is 5kg. When sizing, the temperature of the sizing material in the sizing tank is 50-55℃, the drying room temperature is 140-145℃, and the cylinder drying temperature is 110℃. The sizing rate of the warp yarn is 13%. The shrinking time of the sized warp yarn is 30h.
[0066] 3) Weaving beam preparation: combine multiple pulp beams into a weaving beam.
[0067] The pulp beams in step 2) are combined into a weaving beam according to the warp density of 85-95 strands / cm designed for the weaving machine. The unwinding tension of each pulp beam is 8kg, and the winding tension of the weaving beam is 75kg when it is combined into one weaving beam. Then the heald and reed are drawn in, and the weaving machine is ready for weaving.
[0068] 4) Weaving: The weft is inserted through a water jet loom to interweave the warp and weft yarns to form a fabric.
[0069] Place the fine denier multifilament 7D-12D nylon filament of the weft yarn raw material on the weft yarn rack; pull the weft yarn through the wire guide hole and the weft storage device, and lead it out from the nozzle. The upper machine tension of the weaving beam is adjusted to 900N, and the length range of the weft yarn measurement is 190cm. During weaving, the angle of the weft yarn scissors at the lower edge of the cloth is 10°, the angle of the weft yarn scissors at the upper edge of the cloth is 20°, the spray angle of the nozzle water during weft insertion is 108°, the angle of water to the lower edge of the cloth (discarded edge) is 230°, the angle of the weft yarn to the lower edge of the cloth (discarded edge) is 250°, the angle of the lower weft detection is 320°, and the angle of the comprehensive flattening time is 350°.
[0070] Comparative Examples 1 to 3
[0071] The warp yarn used in Comparative Example 1 is the original warp yarn, which is not subjected to point interlacing treatment, and the number of interlacing points in the original warp yarn is 10 to 12 per meter.
[0072] The warp yarn used in Comparative Example 2 was subjected to a point network treatment, and the total number of network points of the warp yarn after the treatment was 15 / m.
[0073] The warp yarn used in Comparative Example 3 was subjected to a point network treatment, and the total number of network points of the warp yarn after the treatment was 17 / m.
[0074] After the machine experiment, the network points of the warp yarns obtained in Comparative Examples 1 to 3 were insufficient, and the warps were easily broken during the warping step, and subsequent operations could not be continued.
[0075] Comparative Example 4
[0076] The method for preparing the ultra-light and thin nylon fabric in this embodiment specifically comprises the following steps:
[0077] 1) Warping: used to wind the warp yarn on the warping beam.
[0078] The total number of network points on the warp yarn in this comparative example is 18.
[0079] The specific parameters are: the density of the warp yarn is 8-9 yarns / cm, the tension of the monofilament on the warping creel is 3g / thread, and the pressure of the pressure roller is 1.5kg / cm 2 ; The single yarn tension when the warping beam is taken up is 4g / filament.
[0080] 2) Warp sizing: The warp yarn wound on the warping beam is sizing.
[0081] The warping beam in step 1) is transported to the sizing truck for sizing, and the sizing concentration of the sizing agent is 13%. The warp yarns of the warping beam are unwound, passed through the sizing tank filled with sizing agent, and the sizing warp yarns are preliminarily dried in four drying rooms, and then dried by five cylinders, and then wound on the sizing beam.
[0082] The unwinding tension of the warp yarn of the warping beam is 6kg, the monofilament tension when entering the drying room is 4g / thread, and the winding tension of the sizing beam is 4kg. When sizing, the temperature of the sizing material in the sizing tank is 50-55℃, the drying room temperature is 140-145℃, and the cylinder drying temperature is 115℃. The sizing rate of the warp yarn is 12%. The shrinking time of the sized warp yarn is 30h.
[0083] 3) Weaving beam preparation: combine multiple pulp beams into a weaving beam.
[0084] The pulp beams in step 2) are combined into a weaving beam according to the warp density of 85 to 95 strands / cm designed for the weaving machine. The unwinding tension of each pulp beam is 7kg, and the winding tension of the weaving beam is 70kg when it is combined into one weaving beam. Then the heald and reed are drawn in, and the weaving machine is ready for weaving.
[0085] 4) Weaving on the loom: The weft is inserted through a water jet loom to interweave the warp and weft yarns to form a fabric. The weft raw material, fine denier multifilament 7D~12D nylon filament, is placed on the weft rack; the weft yarn is pulled through the wire guide hole and the weft storage device and led out from the nozzle. The machine tension of the weaving shaft is adjusted to 800~1000N, and the length range of the weft yarn measurement is 188cm~192cm. During weaving, the angle of the weft yarn scissors at the lower edge of the cloth is 10°, and the angle of the weft yarn scissors at the upper edge of the cloth is 20°. The spray angle of the nozzle water during weft insertion is 100°, the angle of water to the lower edge of the cloth (discarded edge) is 220°, the angle of the weft yarn to the lower edge of the cloth (discarded edge) is 240°, the angle of the lower weft detection is 315°, and the angle of the comprehensive flattening time is 345°.
[0086] Results and Discussion:
[0087] The following table is a table of process parameters and effects of the above embodiments and comparative examples.
[0088] Table 1 Process parameters and effects
[0089]
[0090] In Comparative Examples 1 to 3, due to the insufficient number of network points of the warp yarn, during the warping process, the hairiness is high when passing through the wire guide, the yarn is easily broken, and it cannot be opened, and subsequent operations cannot be performed. In Comparative Example 4, the number of network points reaches 18 / m, and warping and subsequent operations can be performed. However, during the weaving process, the jet angle is set to 100° forward, causing the warp yarn on the first cloth edge of the loom to be occasionally broken by water; 220° water to discarded edge and 240° yarn to discarded edge cause the weft yarn to be pulled; production is difficult, and the weft marks on the cloth are serious, and mass production cannot be performed.
[0091] In Example 1, the number of network points reaches 18 / m, and warping and subsequent operations can be performed. In the weaving process, compared with Comparative Example 4, the jet angle in Example 1 is 5° later, and the warp yarn at the upper edge of the loom does not touch the water; the 225° water to the discarded edge and the 245° yarn to the discarded edge are relatively delayed, and the weft yarn is sent to the lower edge of the cloth under normal tension; trial production can be carried out, and the production efficiency is increased to 70%; the genuine rate is about 60%, and the quality is improved.
[0092] In Example 2, the number of network points reaches 20 / m. During the weaving process, the jet angle is 8° backward, which is 108°, the angle from water to discarded edge is 230°, and the angle from yarn to discarded edge is 245°, and the production efficiency is further improved to 80-85%. The genuine rate reaches 70-75%, the quality is significantly improved, and batch production is possible.
[0093] In Example 3, the number of network points reaches 25 / m. During the weaving process, the jet angle is 8° backward, which is 108°, the angle from water to the discarded edge is 230°, and the angle from yarn to the discarded edge is 250°, and the production efficiency is further improved to 85-90%. The genuine rate reaches 80%, the quality is improved, and it can be mass-produced. In addition, the angle from yarn to discarded edge in Example 3 is larger, and the prepared fabric product feels better and softer than the fabric product in Example 2. The trapezoidal tear strength of the fabric prepared in Example 3 reaches 11-50N; the tensile breaking strength reaches 150N-260N; and the tensile elongation reaches 25-45%.
[0094] The woven fabrics of Examples 1 to 3 are breathable and comfortable to wear after dyeing; they are suitable for light skin clothing and light windbreakers, and are convenient to store when traveling; and they can be made into cold-proof down clothing fabrics after bonding.
[0095] The purpose of the present invention is to provide an ultra-light and thin nylon fabric using fine denier multifilament 7D-12D nylon filaments in both warp and weft as the main raw material. This is mainly achieved by combining the following schemes:
[0096] 1) Use a yarn interlacing device such as the Karl Mayer interlacing machine to add interlacing points to the warp yarn to increase the number of interlacing points on the warp yarn so that the total number of interlacing points on the warp yarn is 18 to 30 per meter. Increasing the number of interlacing points in the warp yarn increases the bundling, cohesion and strength of the fibers, and avoids the problem of warp breakage during warping and subsequent steps, which results in the inability to produce or the poor quality of the prepared fabric. If the number of interlacing points is too small, the fabric cannot be produced or the quality of the prepared fabric is poor. If the number of interlacing points is too high, the energy consumption and cost are high.
[0097] 2) Low tension technology is used in the warping process and subsequent processes to ensure the strength of fine denier multifilament.
[0098] 3) In the prior art, the spray angle during weft insertion is 100°. In the present application, the spray time of the nozzle is delayed compared to the traditional spray time, which can make the opening angle of the upper and lower warp yarns larger, avoiding the water reaching the warp yarns and interrupting the warp yarns. The angles of water to the lower edge of the cloth (discarded edge) and the angles of the weft yarn to the lower edge of the cloth (discarded edge) are increased, the water is slow (delayed), and the weft yarn is slow to be inserted, and the softness of the fabric finally prepared is better.
[0099] By adopting the preparation process combined with the above schemes, 7D-12D nylon filaments can be prepared into ultra-light and thin fabrics and applied to industrial production. The prepared fabric has a warp density of 95-105 strands / cm, a weft density of 73-95 strands / cm, and a mass of 20-30g / m 2 , to achieve true high density and light weight.
[0100] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A nylon fabric, which is formed by interweaving warp yarns and weft yarns, characterized in that: The raw material of the warp yarn is fine denier multifilament 7D-12D nylon filament, the warp yarn includes mesh points, and the mesh points are located on the nylon filament. During the preparation of the nylon fabric, the warp yarn is subjected to a mesh point treatment to increase the number of the mesh points of the warp yarn, and the total number of the mesh points on the warp yarn is 18-30 / m; The raw material of the weft yarn is fine denier multifilament 7D-12D nylon filament; the density of the warp yarn is 95-105 strands / cm, the density of the weft yarn is 73-95 strands / cm, and the mass of the nylon fabric is 20-30g / m 2 ; The nylon fabric is prepared by the following preparation method: the steps of warping, warp sizing, weaving beam preparation, and weaving are sequentially included, in which the warp yarn is subjected to the network point treatment to increase the number of network points of the warp yarn; the debonding tension of the monofilament on the warping creel is 3 to 5 g / thread, and the monofilament tension when the warping beam is wound is 4 to 6 g / thread; In the warp sizing step, the warp yarn unwinding tension of the warp beam is 6-8 kg, the single yarn tension when entering the drying room is 4-6 g / thread, and the winding tension of the sizing beam is 4-6 kg; In the weaving step, the water jetting angle of the loom nozzle during weft insertion is 105° to 108°, the angle from the water to the lower edge of the cloth is 225° to 230°, and the angle from the weft yarn to the lower edge of the cloth is 245° to 250°; In the weaving shaft preparation step, the unwinding tension of each pulp shaft is 7-9 kg, and the winding tension of the weaving shaft when it is formed into a weaving shaft is 70-80 kg.
2. The nylon fabric according to claim 1, characterized in that: In the warping and warp yarn sizing steps, the density of the nylon filaments used as the raw material of the warp yarn is 8 to 9 filaments / cm.
3. The nylon fabric according to claim 1, characterized in that: In the warp yarn sizing step, the sizing concentration of the slurry is 13-15%.
4. The nylon fabric according to claim 3, characterized in that: The sizing rate of the warp yarn obtained after the warp yarn sizing step is 12-13%.
5. The nylon fabric according to claim 1, characterized in that: In the weaving step, the weaving tension of the loom beam is 800-1000N, and the length of the weft yarn is measured in the range of 188cm-192cm.