Powder filling device, filling system, molding machine host, unit and production line
By measuring the powder weight and steel strip cross-sectional size in real time, the flux-cored wire filling device accurately controls the powder feeding speed, which solves the problem of low filling rate control accuracy in the existing technology and improves the consistency and safety of welding quality.
Patent Information
- Application Number
- CN202210974717.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-08-15
AI Technical Summary
The filling rate control accuracy in the existing flux-cored wire production process is low, resulting in uneven welding quality, especially in the welding of high-strength steel and low-temperature steel. The powder formulas of different welding wire products cause trouble in equipment operation, and can easily cause filling rate errors and Welding wire quality deteriorates.
A flux-cored wire powder filling device including a powder feeder, feeding mechanism, weighing mechanism, steel belt speed measuring device, and steel belt cross-section online measurement device is used to accurately control powder feeding by measuring powder weight changes and steel belt cross-sectional dimensions in real time. speed to ensure the stability and uniformity of filling rate.
It improves the control accuracy of flux-cored wire filling rate, reduces the fluctuation of filling rate, ensures the consistency and safety of welding quality, and reduces economic losses and safety hazards in production.
Smart Images

Figure CN115121994B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flux-cored welding wire production, and particularly relates to a flux-cored welding wire powder filling device, a flux-cored welding wire forming machine host, a flux-cored welding wire forming machine unit and a flux-cored welding wire production line. Background Art
[0002] The filling rate of flux-cored wire is an important indicator that affects the welding quality of flux-cored wire. Large fluctuations in the filling rate will lead to uneven composition of the deposited metal during welding, and then the strength of each part of the deposited metal filled in the weld will be uneven, which will lead to greater stress between various parts of the deposited metal, thereby affecting the ability of the deposited metal to bear external loads and reducing the impact toughness of the welded parts. These problems are fatal defects for welding quality. Especially in the welding of high-strength steel or low-temperature steel, the impact is particularly obvious.
[0003] In the prior art, during the production process of flux-cored welding wire, powder is added to the rolled U-shaped steel strip by a powder filling device. Usually, the powder filling device generally includes a feeding mechanism and a powder feeder, and the powder feeder can usually be a belt-type powder feeder, a grinding disc-type powder feeder or an auger-type powder feeder.
[0004] Regarding the feeding mechanism, there are two main technical routes on the market: one is the continuous feeding represented by CN201833121U (public date May 18, 2011). In this scheme, it is advocated to set a transition hopper between the large silo and the final feeding device. The powder flows from the large silo to the transition hopper, and then flows to the final feeding device. Even if the powder in the large silo is used up and the silo is replaced, since there is still powder in the transition hopper, the pressure generated by the overall height of the powder will not change much on the powder feeder. In this way, the density of the powder on the powder feeder is kept small and the stability of the filling material is ensured. However, in this route, in addition to direct control and feedback on the running speed of the powder feeder, there is no closed-loop control of the filling rate in the final link.
[0005] Another route is the intermittent feeding represented by CN101537552A (published on September 23, 2009). In this scheme, a transparent feeding pipe is set between the powder hopper (equivalent to the above-mentioned large silo) and the belt powder feeding assembly (equivalent to the above-mentioned powder feeder), and an upper material level photoelectric sensor and a lower material level photoelectric sensor are respectively set at the upper and lower parts of the transparent feeding pipe. When the powder in the transparent feeding pipe is reduced to the lower material level sensor, the air control valve assembly of the transparent feeding pipe is opened to feed the material into the transparent feeding pipe. When the material accumulates in the transparent feeding pipe to the upper material level photoelectric sensor, the air control valve assembly is closed to stop feeding the material into the transparent feeding pipe. In the above process, the belt powder feeding assembly continues to add powder to the U-shaped groove. The volume of the powder fed into the transparent feeding pipe each time is obtained by the internal cross-sectional area of the transparent feeding pipe and the distance between the upper and lower material level photoelectric sensors, and the filling rate is obtained by the time of each input or output of a tube of powder, the speed, width, thickness, etc. of the steel belt. However, when using the above-mentioned filling device, since the bottom of the transparent feeding tube is located on the belt powder feeding assembly, the volume of the material in the transparent feeding tube before and after each feeding is quite different, usually only 20% or less of the volume after feeding, and the different pressures of the powder on the belt lead to different powder densities. Moreover, the height of this tube is usually 5cm~30cm, and the height difference of the powder falling is relatively large. During each powder feeding process, due to the different densities of the components in the powder, stratification occurs when falling, that is, the lighter components are in the upper layer and the heavier components are in the lower layer. Of course, this phenomenon does not completely and thoroughly separate the different components, but only makes the originally evenly mixed powder become uneven again, thereby affecting the uniformity of the powder components filled into the U-shaped steel belt. Moreover, the device uses volume flow to calculate the mass flow. After calculating the analog quantity in advance, the operating parameters of the equipment can only be adjusted according to the calculated analog quantity. Different welding wire products have different powder formulas, and their powder bulk density is also different. Therefore, for different powder formulas, parameters such as bulk density must be input separately, which causes troubles in equipment operation. Moreover, once the formula is changed, if the density is not re-entered due to negligence, the filling rate will be wrong, which will lead to a significant decrease in the quality of the welding wire, and even the welding wire produced will be scrapped, causing serious economic losses. If such welding wire is put into welding, fatigue cracks are very likely to occur, especially in the welding of ship hulls, causing quality problems and safety hazards. Summary of the invention
[0006] In view of the defects in the prior art, the first object of the present invention is to provide a flux-cored welding wire powder filling device to solve the technical problem of low filling rate control accuracy.
[0007] In the first aspect, the present invention provides a flux-cored welding wire powder filling device, comprising a powder feeder, a feeding mechanism, a first bracket, a second bracket and a weighing mechanism, wherein the feeding mechanism is arranged above the powder feeder, the feeding mechanism comprises a feeding valve, a first fixed hopper and a final feeding piece, the final feeding piece is located below the first fixed hopper and is used to directly supply powder to the powder feeder, the feeding valve is located above the first fixed hopper and is relatively movable with the inlet end of the first fixed hopper in the vertical direction, the powder feeder and the first fixed hopper are relatively fixedly arranged with the first bracket, the first bracket and the second bracket are relatively movable in the vertical direction, the first bracket is supported by the weighing end of the weighing mechanism, the mounting end of the weighing mechanism is relatively fixedly arranged with the second bracket, and the weighing mechanism is used to obtain the reduction of the weighing value at different times during the powder feeding process to obtain the changing speed of the powder weight to control the running speed of the powder feeder.
[0008] The beneficial effects of the flux-cored welding wire powder filling device of the present invention are:
[0009] By fixing the powder feeder and the first fixed hopper of the feeding mechanism to the first bracket, and connecting the first bracket to the weighing end of the weighing mechanism, the weighing mechanism can be used to obtain the total weight of the above parts and the powder therein, and the weight information can be obtained at very small intervals or continuously, and the weight of the flux-cored welding wire powder filling device can be immediately known. Since the weight of the above mechanical structure itself does not change, the weight change at different times is the powder weight change, and then the powder weight reduction speed in the flux-cored welding wire powder filling device is obtained, that is, the powder filling speed measured by weight. After the powder weight reduction speed measured by weight can be obtained, the running speed of the powder feeder can be more accurately controlled in conjunction with the weight-level input speed of the steel belt, thereby improving the stability of the filling rate and reducing the fluctuation of the filling rate.
[0010] Furthermore, the inlet end of the first fixed hopper is softly connected to the feed valve.
[0011] Further, the first bracket includes a powder feeder bracket, the powder feeder is installed on the powder feeder bracket, the powder feeder bracket is installed with a dustproof box, a fixed hopper bracket is installed on the top of the dustproof box, and the fixed hopper bracket is fixedly installed with the first fixed hopper.
[0012] Furthermore, the flux-cored welding wire powder filling device further includes a second bracket, the feeding mechanism further includes a movable hopper, the movable hopper is detachably mounted on the second bracket, and the first bracket and the second bracket are relatively movably arranged in the vertical direction.
[0013] Furthermore, the flux-cored welding wire powder filling device also includes a powder collecting trough, and the powder collecting trough is installed at the bottom of the first bracket.
[0014] The second object of the present invention is to provide a flux-cored welding wire powder filling system to solve the technical problem of low filling rate control accuracy.
[0015] The flux-cored welding wire powder filling system provided by the present invention comprises a steel strip speed measuring device, an online steel strip cross-section measuring device, a control device and any one of the above flux-cored welding wire powder filling devices, wherein the steel strip speed measuring device, the online steel strip cross-section measuring device and the flux-cored welding wire powder filling device are all electrically connected to the control device, the steel strip speed measuring device is used to measure the running speed of the steel strip, the online steel strip cross-section measuring device is used to measure the width and thickness of the steel strip cross-section, and the control device is used to control the powder feeding speed of the powder filling device according to the speed, thickness and width of the steel strip.
[0016] Compared with the prior art, by setting up an online measuring device for the cross section of the steel strip, the thickness and width of the steel strip are measured online during the operation of the steel strip, and the speed of the steel strip is measured in conjunction with a speed measuring device for the steel strip, so as to accurately know the volume flow and mass flow of the steel strip. As long as the mass flow of the steel strip changes, the mass flow of the powder can be adjusted in time to achieve the matching of the two, thereby improving the stability of the filling rate. The present application changes the prior art of estimating the volume flow of the steel strip by simulating the nominal thickness and width of the steel strip, into a digital method of measuring the thickness and width of the steel strip, thereby obtaining a dynamic mass flow of the steel strip, changing the destructive detection of the breakage experiment to an online full-process non-destructive detection, and changing from passively accepting the size change of the steel strip to actively controlling the mass flow of the powder according to the size change of the steel strip, which can significantly improve the control accuracy of the filling rate of the flux-cored welding wire.
[0017] The third object of the present invention is to provide a flux-cored welding wire forming machine main unit to solve the technical problem of low filling rate control accuracy.
[0018] The main machine of the flux-cored welding wire forming machine provided by the present invention comprises the above-mentioned flux-cored welding wire powder filling device.
[0019] The beneficial effects brought by the flux-cored wire forming machine host in this aspect are:
[0020] Since the flux-cored welding wire forming machine main unit provided in the present aspect includes the above-mentioned flux-cored welding wire powder filling device, it has the corresponding technical effects of the above-mentioned flux-cored welding wire powder filling device, which will not be repeated here.
[0021] Furthermore, the molding machine mainframe includes a machine platform, and a positioning rod is fixedly connected to the machine platform, and the positioning rod is adapted to a positioning hole arranged in the flux-cored welding wire powder filling device.
[0022] A fourth object of the present invention is to provide a flux-cored welding wire forming unit to solve the technical problem of low filling rate control accuracy.
[0023] The flux-cored welding wire forming machine unit provided by the present invention comprises a tape unwinding machine and the above-mentioned flux-cored welding wire forming machine host.
[0024] The beneficial effects brought by the flux-cored wire forming unit of this aspect are:
[0025] Since the flux-cored welding wire forming machine unit provided in the present invention includes the above-mentioned flux-cored welding wire forming machine main machine, it has the corresponding technical effects of the above-mentioned flux-cored welding wire forming machine main machine, which will not be repeated here.
[0026] A fifth object of the present invention is to provide a flux-cored welding wire production line to solve the technical problem of low filling rate control accuracy.
[0027] The flux-cored welding wire production line provided by the present invention comprises the above-mentioned flux-cored welding wire forming unit.
[0028] The beneficial effects brought by the flux-cored welding wire production line of this aspect are:
[0029] Since the flux-cored welding wire production line provided by the present invention includes the above-mentioned flux-cored welding wire forming unit, it has the corresponding technical effects of the above-mentioned flux-cored welding wire forming unit, which will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.
[0031] Figure 1 A schematic diagram of the structure of a flux-cored welding wire powder filling device provided in the first embodiment of the present invention applied to a main unit of a flux-cored welding wire forming machine;
[0032] Figure 2 A left view of the flux-cored welding wire powder filling device provided in the first embodiment of the present invention applied to a main machine of a flux-cored welding wire forming machine;
[0033] Figure 3 yes Figure 1 A partial enlarged view of part A;
[0034] Figure 4 yes Figure 2 A partial enlarged view of part B.
[0035] Description of Reference Numerals
[0036] 10-feeding mechanism; 11-first fixed hopper; 12-second fixed hopper; 13-feeding valve; 14-hose; 15-movable hopper; 21-powder feeder; 22-powder collecting trough; 23-dustproof box; 24-observation window; 30-weighing mechanism; 41-first bracket; 42-second bracket; 43-sensor mounting plate; 50-U-shaped steel belt; 61-machine platform; 62-steel belt roller; 63-positioning rod. DETAILED DESCRIPTION
[0037] The following embodiments of the technical solution of the present invention are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and cannot be used to limit the protection scope of the present invention.
[0038] It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should have the common meanings understood by those skilled in the art to which the present invention belongs.
[0039] Embodiment 1: Figure 1 A schematic diagram of the structure of a flux-cored welding wire powder filling device provided in the first embodiment of the present invention applied to a main unit of a flux-cored welding wire forming machine; Figure 2 This is a left view of the flux-cored welding wire powder filling device provided in the first embodiment of the present invention applied to the main machine of the flux-cored welding wire forming machine. Figure 1 and Figure 2 As shown, the flux-cored welding wire powder filling device provided in the first embodiment includes a powder feeder 21, a feeding mechanism 10, a first bracket 41, a second bracket 42 and a weighing mechanism 30. The feeding mechanism 10 is arranged above the powder feeder 21. The feeding mechanism 10 includes a feeding valve 13, a first fixed hopper 11 and a final feeding piece. The final feeding piece is located below the first fixed hopper 11 and is used to directly supply powder to the powder feeder 21. The feeding valve 13 is located above the first fixed hopper 11 and is relatively movable with the inlet end of the first fixed hopper 11 in the vertical direction. The first bracket 41 and the second bracket 42 are relatively movable in the vertical direction. The first bracket 41 is supported by the weighing end of the weighing mechanism 30. The mounting end of the weighing mechanism 30 is relatively fixedly arranged with the second bracket 42. The weighing mechanism 30 is used to obtain the reduction of the weighing value at different times in the powder feeding process to obtain the change speed of the powder weight to control the running speed of the powder feeder 21.
[0040] It should be noted that the first fixed hopper 11 does not mean that after the fixed hopper is installed on the first bracket 41, it must be removed in a destructive manner to be separated from the first bracket 41. Rather, it means that during the normal production process, the fixed hopper is inactive relative to the first bracket 41. For example, the first fixed hopper 11 can be a glass hopper or a metal hopper, which is directly placed on the first bracket 41, or placed on other brackets fixed relative to the first bracket 41, so as to achieve a relatively fixed setting relative to the first bracket 41.
[0041] Among them, in this embodiment, the first fixed hopper 11 is a metal hopper, and the top of the metal hopper has a hopper cover, and the middle of the hopper cover is opened, and the feeding powder enters the first fixed hopper 11. In addition, the final feeding piece can cooperate with a commonly used belt-type powder feeder. The final feeding piece can be a movable hopper, such as the final feeding device of the wire rolling mill powder feeder mentioned in CN201559029U (published on August 25, 2010); or it can also be a fixed second fixed hopper 12, and the height of the side panel body of the second fixed hopper 12 facing the U-shaped steel belt 50 can be adjusted. In short, the weight of the final feeding piece and the powder therein can be borne by the first bracket 41. For example, the frame of CN201559029U can also be installed on the first bracket. As for the weight of the final feeding device and the powder therein, it is mainly borne by the powder feeder, and the weight of the powder feeder can also fall on the first bracket 41. As for how to fix the second fixed hopper 12 to the powder feeder bracket, it is a technology known to those skilled in the art, and is not the main content discussed in this application, and will not be described here.
[0042] In this embodiment, the weighing mechanism 30 may include three weighing sensors, and the three weighing sensors are distributed in a triangular shape when viewed from a top view. Usually, the weighing end of the weighing sensor is located at the top of each weighing sensor, and the mounting end of the weighing sensor is located at the bottom. The bottoms of the three weighing sensors are mounted on a sensor mounting plate 43 extending from the middle of the second bracket 42, that is, the mounting end of the weighing mechanism 30 is relatively fixedly arranged with the second bracket 42. Since the first fixed hopper 11 and the powder feeder 21 are provided in this embodiment, the three weighing sensors are mounted on the lower surface of the first bracket 41, so that the weight of the first bracket 41, the first fixed hopper 11, the powder feeder 21 and the powder therein can be weighed.
[0043] The feed valve 13 may be an electric or pneumatic gate valve or butterfly valve, the inlet end of the feed valve 13 is located at the upper part of the feed valve 13, and the outlet end of the feed valve 13 is located at the lower part of the feed valve 13. The feed valve 13 may be controlled to open or close by electric or pneumatic means, so that the powder flows into the fixed hopper through the feed valve 13.
[0044] By setting the feeding valve 13, it can be opened when it is necessary to replenish the first fixed hopper 11 with powder, and closed when it is not necessary to replenish the powder. In the closing stage, the weighing mechanism 30 weighs the part of the feeding mechanism 10 below the first fixed hopper 11, such as the powder feeder 21, the first bracket 41, and the total weight of the powder therein. The speed of feeding the powder into the U-shaped steel belt 50 can be known according to the change amount and change speed of the total, so as to accurately control the filling rate. By fixing the powder feeder 21 and the first fixed hopper 11 of the feeding mechanism 10 to the first bracket 41, and connecting the first bracket 41 to the weighing end of the weighing mechanism 30, the weighing mechanism 30 can be used to obtain the total weight of the above parts and the powder therein, and the weight information can be obtained at very small intervals or continuously, and the weight of the flux-cored welding wire powder filling device can be immediately known. Since the weight of the above-mentioned mechanical structure itself does not change, the weight change at different times is the powder weight change, and then the powder reduction speed in the flux-cored welding wire powder filling device is obtained, that is, the powder filling speed measured by weight. After the powder weight reduction speed measured by weight can be obtained, the running speed of the powder feeder 21 can be more accurately controlled in conjunction with the input speed of the steel belt measured by weight, so as to improve the stability of the filling rate and reduce the fluctuation of the filling rate.
[0045] The existing intermittent feeding technology route feeds the transparent feeding tube once every 30 seconds to several minutes. For example, the interval disclosed in CN101537552A is 35 seconds for one measurement cycle. In fact, it can only measure the average filling rate within this time period, and the average filling rate is still based on the weight of the powder calculated by multiplying the volume of the powder by the density of the powder. Moreover, due to the different heights of the powder itself, the density of the powder drawn away by the belt powder feeding assembly at the bottom of the transparent feeding tube is different. The filling rate within this time period is bound to be obviously unstable, and a more accurate instant filling rate cannot be obtained.
[0046] The present application measures the total weight of the powder feeder 21 and the feeding mechanism 10 and the powder thereon by using the weight loss method, which can significantly shorten the measurement interval. For example, the measurement can be performed every 1 second or 0.1 second, and in practice it may even be measured 20 times or more than 30 times per second, and the total weight can even be considered to be measured continuously, so that the instant filling rate can be obtained according to the weight difference and the interval time of the two measurements, in combination with the corresponding parameters of the steel belt; accordingly, parameters such as the running speed of the powder feeder can be adjusted 20 times or more than 30 times per second, which can meet the adverse effects caused by different powder densities.
[0047] Moreover, taking the scheme disclosed in CN101537552A as an example, a glass tube with good light transmittance is selected as a transparent material delivery tube 4, and the inner diameter of the transparent material delivery tube 4 is 3.4 cm. Two material level photoelectric sensors 5 and 6 are fixed thereon, and the distance between the two is 16 cm. The distance between the upper and lower material level photoelectric sensors has reached 16 cm, so the distance from the outlet of the upstream pore valve assembly 11 to the lower material level photoelectric sensor 6 should be greater than 16 cm, for example, at least 20 cm according to the estimation of the size in the figure. Under this route, the smaller the diameter of the transparent tube is, the more conducive to improving the detection accuracy, because the powder is accumulated by falling, and roughly, the powder will form a conical upper surface after falling, and it is completely impossible to ensure that the shape and size of each accumulation are absolutely the same, so the larger the diameter, the greater the shape difference caused by its accumulation link, and the more unfavorable it is to ensure the volume stability during each measurement. However, as described in the background technology of this application, increasing the height of the transparent tube, that is, increasing the height difference when the powder falls, will cause increased non-uniformity in the powder density and even increase the non-uniformity in the powder composition, thereby affecting the product quality of the flux-cored welding wire.
[0048] Since the scheme of this embodiment is to measure mass, it is no longer affected by the scheme of the above-mentioned photoelectric sensor, and the cross-sectional area of the first fixed hopper 11 can be increased. Each time the powder is replenished in the first fixed hopper 11, it is not necessary to wait until the powder is used each time with a fixed large height difference. The powder can be replenished when the height of the powder does not change much, so as to avoid excessive changes in the pressure difference of the powder acting on the bottom, which leads to excessive changes in density and ultimately affects the stability of the weight of the filled powder, and excessive falling speed of the powder, which leads to light powder splashing and uneven composition. Specifically, it can be considered that the powder can be replenished in the first fixed hopper 11 once every time the upper surface of the powder drops two or three centimeters in the first fixed hopper 11. Of course, in the process of replenishing the powder in the first fixed hopper 11, although the weighing mechanism 30 is still weighing, the weighing is only used to control the weight of the powder added to the first fixed hopper 11, and does not participate in the measurement of the filling rate. Therefore, when the flux-cored wire forming machine is running, the time for replenishing powder to the first fixed hopper 11 should not be too long, or the proportion of the time the first fixed hopper 11 is in replenishing powder to the total time should not be too large. Alternatively, when each roll of steel strip is replaced, enough powder can be added to the first fixed hopper 11 to match the production of a roll of steel strip, and when a roll of steel strip is running, powder is no longer added to the first fixed hopper 11. Of course, this method will cause the weight of the powder in the first fixed hopper 11 to be too much, and the weight weighed by the weighing mechanism 30 is large, so a weighing mechanism 30 with a larger range is required, which will correspondingly reduce the weighing sensitivity and accuracy. The specific size of the first fixed hopper 11 and the timing of replenishing powder can be set by technicians in the relevant technical field according to their needs.
[0049] Specifically, in this embodiment, the total weight of the first bracket 41, the powder feeder 21, the first fixed hopper 11 and the final feeding member and other parts can be 40kg, and the maximum capacity of the powder contained in the first fixed hopper can be 40kg. The total weight of the two is about 80kg. Specifically, when the weight of the powder in the first fixed hopper 11 is 10% of the capacity, the first fixed hopper 11 can be replenished with powder. In this embodiment, the powder is replenished when the weight is 4kg. When the weight of the powder in the first fixed hopper 11 is 90% of the capacity, the powder is replenished, that is, the powder is stopped when the weight increases to 36kg. Of course, if the powder capacity of the first fixed hopper 11 is 20kg, the powder can be replenished when the weight is reduced to 2kg, and the powder is stopped when the weight is added to 90% of the powder capacity, that is, 18kg.
[0050] In this case, a weighing sensor with a resolution of 1 / 60000 can be selected, that is, the resolution value of the weighing mechanism is 1g. For flux-cored welding wire, the total mass flow rate of the steel strip and powder at the outlet of the flux-cored welding wire powder filling device is about 170g / s, and the filling rate is 15%, so the mass flow rate of the powder is about 25g / s. The weighing mechanism with the above accuracy can fully meet the requirements. If it is necessary to weigh the weight change in a shorter time interval, a weighing sensor with a higher weighing resolution can be selected.
[0051] Moreover, the present application can supply powder to the first fixed hopper 11 in a manner that the height of the accumulated powder changes little, and the powder density will not change significantly, so the continuity of powder feeding can be well guaranteed, so that the uniformity of the powder in the welding wire product is well guaranteed. Therefore, the above-mentioned flux-cored welding wire powder filling device is applied in the actual process of flux-cored welding wire, which can well guarantee the welding processability and welding quality of the welding wire.
[0052] like Figure 1-Figure 4 As shown, further, the inlet end of the first fixed hopper 11 is softly connected to the feed valve 13 .
[0053] Specifically, the inlet end of the first fixed hopper 11 is softly connected to the feeding valve 13, and a section of hose 14 can be fixedly connected to the outlet end of the feeding valve 13 to introduce the powder into the feeding port of the first fixed hopper 11. The hose can be a mesh hose made of steel wire that does not leak powder, or a rubber hose. Alternatively, the soft connection can also be achieved in the following way: a vertical rigid tube is respectively provided at the inlet end of the first fixed hopper 11 and the outlet end of the feeding valve 13, and the two vertical rigid tubes can be one inside and one outside without contact, and the tube connected to the feeding valve 13 is preferably located inside the other tube.
[0054] By softly connecting the inlet end of the first fixed hopper 11 with the feeding valve 13, it is possible to avoid the weight of the feeding valve 13 and the structure above it being transferred to the first fixed hopper 11, thereby preventing the weight of the weighing mechanism 30 from increasing, and avoiding the use of a weighing mechanism 30 with an excessively large range, thereby reducing the sensitivity and precision of the weighing mechanism 30 and affecting the accuracy of the weighing mechanism 30 results.
[0055] like Figure 1-Figure 4 As shown, further, the first bracket 41 includes a powder feeder bracket, the powder feeder bracket is installed with the powder feeder 21, the powder feeder bracket is installed with a dustproof box 23, the top of the dustproof box 23 is installed with a fixed hopper bracket, and the fixed hopper bracket is fixedly installed with the first fixed hopper 11.
[0056] The dustproof box 23 is a rectangular box, and the top of the front door of the dustproof box 23 is pivotally connected to the top of the dustproof box 23 and can be opened upward. At least one of the upstream side and the downstream side of the dustproof box 23 can be provided with an observation hole, and a transparent observation window 24 is provided in the observation hole to facilitate observation of the operation of the powder feeder 21. The transparent observation window 24 can be formed by organic glass embedded in the dustproof box 23 through a sealing strip. Of course, the upstream side wall and the downstream side wall of the dustproof box 23 are also provided with a wire hole (not shown in the figure) to allow the U-shaped steel belt 50 to pass through while minimizing the possibility of powder overflowing into the environment, so that the change in weight is as close as possible to the actual amount of powder injected into the U-shaped steel belt 50.
[0057] By providing a dustproof box 23, the pollution to the environment caused by the splashing of powder when the powder feeder 21 feeds the powder into the U-shaped steel belt 50 can be reduced. Moreover, the splashing powder can be bound inside the dustproof box 23 as much as possible. The weight of this part will also be weighed by the weighing mechanism 30 together with the dustproof box 23 and the powder feeder bracket, so that the reduction in the weight weighed by the weighing mechanism 30 is as close as possible to the weight of the powder entering the steel belt, thereby improving the accuracy of control.
[0058] like Figure 1-Figure 4 As shown, further, the flux-cored welding wire powder filling device also includes a second bracket 42, and the feeding mechanism 10 also includes a movable hopper 15, which is detachably mounted on the second bracket 42, and the first bracket 41 and the second bracket 42 are relatively movably arranged along the vertical direction.
[0059] Since in this embodiment, the weight of the first fixed hopper 11 is borne by the dustproof box 23, and the dustproof box 23 is fixedly connected to the powder feeder bracket, three weighing sensors are installed on the lower surface of the powder feeder bracket to weigh the weight of the first bracket 41, the first fixed hopper 11, the powder feeder 21 and the powder therein.
[0060] The weight of the powder contained in the movable hopper 15 can match a roll of steel belt, and a new movable hopper 15 containing powder can be replaced each time a roll of steel belt is replaced; the weight of the powder contained in the movable hopper 15 can also match multiple rolls of steel belt, and each movable hopper 15 can be used for one or two shifts or even one or two days of production. After the movable hopper 15 is placed on the second bracket 42, the opening at the bottom can be opened manually or automatically, for example, a lifting portion is provided on the second bracket 42 to lift the bottom cover of the movable hopper 15.
[0061] By providing a second bracket 42 to detachably mount the movable hopper 15, and the second bracket 42 is independently mounted on the ground instead of being mounted on the table 61 of the molding machine main body, it is possible to reduce the vibration of the molding machine main body during operation from being transmitted to the second bracket 42, thereby reducing the stratification of the powder due to long-term vibration and causing inaccurate weighing of the weighing mechanism 30.
[0062] like Figure 1-Figure 4 As shown, further, the flux-cored welding wire powder filling device also includes a powder collecting tank 22 , and the powder collecting tank 22 is installed at the bottom of the first bracket 41 .
[0063] The powder collecting trough 22 is provided to collect at least most of the powder that has escaped from the powder feeder 21 but has not fallen into the U-shaped steel belt 50, and the powder collecting trough 22 is installed at the bottom of the first bracket 41, so that the powder collecting trough 22 and the powder therein can be weighed together, so that the weight change obtained by the weighing mechanism 30 is very close to the weight of the powder that has fallen into the U-shaped steel belt 50. The influence of a small amount of powder that has not fallen into the U-shaped steel belt 50 on the weighing accuracy is reduced, and the accuracy of the measurement is improved.
[0064] Embodiment 2: The flux-cored welding wire powder filling system provided in this embodiment includes a steel strip speed measuring device, an online steel strip cross-section measuring device, a control device and the above-mentioned flux-cored welding wire powder filling device. The steel strip speed measuring device, the online steel strip cross-section measuring device and the flux-cored welding wire powder filling device are all electrically connected to the control device. The steel strip speed measuring device is used to measure the running speed of the steel strip, the online steel strip cross-section measuring device is used to measure the width and thickness of the steel strip cross-section, and the control device is used to control the powder feeding speed of the powder filling device according to the speed, thickness and width of the steel strip.
[0065] In flux-cored wire production, inconsistent thickness and width of the steel strip are important factors that lead to changes in fill rate.
[0066] According to the existing production process, taking the case where the nominal cross-sectional size of the steel strip is 1.0mm*14mm and the filling rate is 15% as an example, the density of the steel strip is 7.8g / cm 3, the weight per unit length of the steel strip = ρsteel * dsteel * wsteel, substituting the above values, theoretically, the weight per unit length of the steel strip = 7.8g / cm 3 *0.1cm*1.4cm*100cm / m, the weight of the steel strip per meter is 109.2g. If the running speed of the steel strip at the powder adding point is 100m / min, substitute the mass flow rate of the steel strip = ρsteel*dsteel*wsteel*vsteel; theoretically, the mass flow rate of the steel strip can be obtained as 10.92kg / min.
[0067] According to this steel belt flow, according to the calculation formula of filling rate:
[0068] Filling rate = mass flow rate of medicine powder / (mass flow rate of medicine powder + mass flow rate of steel belt). Conversely, the mass flow rate of medicine powder = mass flow rate of steel belt / (1-filling rate)*filling rate.
[0069] Substituting the filling rate as 15%, the mass flow rate of the powder = 10.92 / (1-15%)*15%=1.927kg / min.
[0070] Therefore, this value is set and put into production. However, in the actual production process, since the actual cross-sectional dimensions of the steel strip cannot maintain a value, there will be tolerances. Therefore, the actual filling rate obtained by the above method cannot meet the 15% standard, and even has a large deviation. This seriously affects the quality of the flux-cored welding wire and will cause unpredictable hidden dangers during use. An example is as follows:
[0071] The thickness of SPCC steel strip, which is the raw material of flux-cored welding wire steel strip, is within the qualified range of 1.0mm±0.06mm. If the thickness deviation reaches the upper tolerance limit of 0.06mm, it means that 6% of the weight of the steel strip is less or more than that per unit time. In addition, in terms of width, a steel strip with a nominal width of 14mm may also have a width of 13.5mm or 14.5mm.
[0072] If the width and thickness of the steel strip at a certain point or section are both the above minimum values, that is, 0.94mm thick and 13.5mm wide, substitute the unit length weight of the steel strip = ρsteel * dsteel * wsteel, and you get the unit length weight of the steel strip = 7.8g / cm 3 *0.094cm*1.35cm*100cm / m, the weight of the steel belt per meter is 98.982g, calculated based on the above steel belt running speed, substituting the above values into the mass flow rate of the steel belt = ρsteel*dsteel*wsteel*vsteel, then the mass flow rate of the steel belt is:
[0073] 7.8g / cm 3*0.094cm*1.35cm*100cm / m*100m / min=9.8982kg / min. According to the traditional process, the filling is still carried out according to the preset powder weight flow rate of 1.927kg / min, so the filling rate is 1.927 / (9.8982+1.927)=0.163=16.3%.
[0074] If the thickness and width of this steel strip are both at their maximum values, that is, the thickness of a certain place or a certain section of the steel strip is 1.06mm and the width is 14.5mm, substitute the unit length weight of the steel strip = ρsteel*dsteel*wsteel,
[0075] The weight per unit length of the steel strip is 7.8 g / cm 3 *0.106cm*1.45cm*100cm / m, the weight of the steel belt per meter is 119.886g, still calculated based on the above steel belt running speed, substitute this value into:
[0076] The mass flow rate of steel belt = ρsteel*dsteel*wsteel*vsteel, then:
[0077] Mass flow rate of steel belt = 7.8g / cm 3 *0.106cm*1.45cm*100cm / m*100m / min =11988.6g / min=11.9886kg / min. At this time, the weight flow rate of the powder still uses the preset 1.927kg / min. At this time, the actual filling rate of the flux-cored wire is 1.927 / (1.927+11.9886)=13.8%, which is 2.5 percentage points different from the maximum filling rate of 16.3%, and the absolute filling rate is 1 / 6. Such a filling rate fluctuation range can completely affect the welding performance.
[0078] Even if the influence of the width of the steel strip is not considered, assuming that the width of the steel strip is stable and only the thickness of the steel strip is considered, the weight flow rate of the powder calculated according to the filling rate of 15% corresponding to the thickness of the steel strip is still 1.927kg / min. Then, when the thickness of the steel strip is the maximum value of 1.06mm, the unit length weight of the steel strip = ρsteel * dsteel * wsteel is substituted, and the unit length weight of the steel strip = 7.8g / cm 3 *0.94cm*1.4cm*100cm / m, the weight of the steel belt per meter is 102.648g, still calculated based on the above steel belt running speed, substitute:
[0079] The mass flow rate of steel strip = ρsteel*dsteel*wsteel*vsteel, we get:
[0080] Mass flow rate of steel belt = 7.8g / cm 3*0.094cm*1.4cm*100cm / m*100m / min =10264.8g / min=10.2648kg / min, correspondingly, at this time,
[0081] Actual filling rate = 1.927 / (1.927+10.2648) = 0.158 = 15.8%.
[0082] Then when the thickness of the steel strip is the maximum value of 1.06mm, substitute the weight per unit length of the steel strip = ρsteel * dsteel * wsteel, and you get the weight per unit length of the steel strip = 7.8g / cm 3 *0.106cm*1.4cm*100cm / m, the weight of the steel belt per meter is 115.752g, still calculated based on the above steel belt running speed, substitute:
[0083] The mass flow rate of steel strip = ρsteel*dsteel*wsteel*vsteel, we get:
[0084] Mass flow rate of steel belt = 7.8g / cm 3 *0.106cm*1.4cm*100cm / m*100m / min =11575.2g / min=11.5752kg / min, correspondingly, at this time,
[0085] Actual filling rate = 1.927 / (1.927+11.5752) = 0.143 = 14.3%.
[0086] The difference between the maximum fill rate and the minimum fill rate can reach 1.5 percentage points, accounting for 10% of the absolute value of the fill rate.
[0087] However, in the prior art, there is no precedent for setting up an online measurement device for the steel strip cross section in a flux-cored wire forming machine. Generally speaking, the powder feeding amount of the powder feeder is adjusted only according to the change in the steel strip speed. The filling rate fluctuation caused by the thickness and width of the steel strip can only be ignored. Therefore, even though the industry has made efforts for a long time to solve the filling rate fluctuation, it still cannot reach a satisfactory level.
[0088] Even if the steel strip is measured, since the steel strip is usually transported and stored in coils, the existing technology can only use sampling to determine whether the steel strip is qualified. For example, the surface of the coiled steel strip is selected, cut off, and the width and thickness of the cross section are measured. This experiment is a destructive test, and it is impossible to conduct a comprehensive test on the entire coil of steel strip along its length - because doing so is completely unacceptable from the perspective of cost and efficiency, and it can be said that it is basically of no substantial help in controlling the filling rate of the welding wire.
[0089] In this embodiment, the steel strip speed measuring device can be set at the entrance of the forming roller of the flux-cored welding wire forming machine. For example, the steel strip can be bent into an S shape. Specifically, the steel strip speed measuring device in CN101537552A can be used. The steel strip speed measuring device is not the object of the invention of this application and will not be described in detail here. The online measuring device for the steel strip cross section can measure the thickness and width of the steel strip cross section in real time, so as to obtain the cross-sectional size of the steel strip. In conjunction with the steel strip speed measuring device, the volume flow rate of the steel strip can be known. Since the density of the steel strip is relatively stable, the mass flow rate of the steel strip can be obtained. The mass flow rate of the steel strip = ρsteel*dsteel*wsteel*vsteel. Among them, ρsteel is the density of the steel strip, dsteel is the thickness of the steel strip measured by the steel strip measuring device, wsteel is the width of the steel strip, and vsteel is the instantaneous speed of the steel strip measured by the steel strip speed measuring device.
[0090] Assuming the filling rate is 15%, it can be calculated that the corresponding mass flow rate of the powder is the mass flow rate of the steel belt / (1-0.15)*0.15. Taking the belt-type powder feeder as an example, the mass flow rate of the powder is ρ powder*d powder*w powder*v powder. Among them, ρ powder is the bulk density of the powder, d powder is the thickness of the powder on the powder feeding belt, w powder is the width of the powder on the powder feeding belt, and v powder is the speed of the powder feeding belt in the powder feeder. In this embodiment, ρ powder, d powder, and w powder are all relatively stable. Therefore, the control device can control the size of v powder according to the result of d steel*w steel*v steel, that is: v powder=ρ steel*d steel*w steel*v steel / (1-0.15)*0.15 / (ρ powder*d powder*w powder), so that the mass flow rate of the powder can match the mass flow rate of the steel belt, and the filling rate can remain stable.
[0091] For example, for the above-mentioned steel belt thickness deviation, if the steel belt thickness changes from 1.0mm to 0.94mm, and the width and running speed of the steel belt remain unchanged, the running speed of the powder feeding belt can be reduced by 6%. Correspondingly, the mass flow rate of the powder is reduced by 6%, and the mass flow rate of the powder is reduced from 1.927kg / min to 1.927*0.94=1.81138kg / min, thereby matching the mass flow rates of the powder and the steel belt and still ensuring a filling rate of 15%.
[0092] The online measuring device for the cross section of the steel strip can use ultrasonic, laser or reflective photoelectric sensors to measure the size of the steel strip from the online measuring device for the cross section of the steel strip. More specifically, it can measure from both the upper and lower sides and the left and right sides of the steel strip at the same time. Even if the height or left and right position of the steel strip changes, the stability of the cross-sectional size measurement of the steel strip can still be guaranteed. For example, at a certain moment, the overall thickness of the steel strip suddenly decreases by 0.05mm compared to the previous moment, the size measured from the top of the steel strip changes from 2mm to 2.05mm, and the size measured from the bottom of the steel strip changes from 2mm to 1.95mm, which means that the thickness of the steel strip has not changed, and there is no need to adjust the powder feeding speed due to the thickness.
[0093] Compared with the prior art, in this embodiment, by setting an online measuring device for the cross section of the steel strip, the thickness and width of the steel strip are measured online during the operation of the steel strip, and the speed of the steel strip is measured in conjunction with the steel strip speed measuring device, so as to accurately know the volume flow rate and mass flow rate of the steel strip. As long as the mass flow rate of the steel strip changes, the mass flow rate of the powder can be adjusted in time to achieve the matching of the two, thereby accurately improving the stability of the filling rate. The present application changes the prior art of estimating the volume flow rate of the steel strip by simulating the nominal thickness and width of the steel strip, and changes it to measuring the thickness and width of the steel strip in a digital way, thereby obtaining a dynamic mass flow rate of the steel strip, and changes from the sampling destructive detection of the breakage experiment to the online full-process non-destructive detection, and from passively accepting the size change of the steel strip to actively controlling the mass flow rate of the powder according to the size change of the steel strip, which can significantly improve the control accuracy of the filling rate of the flux-cored welding wire.
[0094] Embodiment 3: The main body of the flux-cored welding wire forming machine provided in this embodiment includes the above-mentioned flux-cored welding wire powder filling device.
[0095] Since the flux-cored welding wire forming machine main unit provided in this embodiment includes the above-mentioned flux-cored welding wire powder filling device, it has the corresponding technical effects of the above-mentioned flux-cored welding wire powder filling device, which will not be repeated here.
[0096] like Figure 2 and Figure 4 As shown, further, the main machine of the forming machine includes a machine table 61, and a positioning rod 63 is fixedly connected to the machine table 61, and the positioning rod 63 is adapted to the positioning hole set in the flux-cored welding wire powder filling device.
[0097] Steel belt rollers 62 are usually installed on the machine table 61 of the main machine of the forming machine, which are respectively arranged upstream and downstream of the position where the U-shaped steel belt 50 is injected with powder by the flux-cored welding wire powder filling device, and are usually as close to the flux-cored welding wire powder filling device as possible. The steel belt rollers 62 are used to stabilize the steel belt to reduce the shaking of the steel belt when the powder is injected. A positioning rod 63 is arranged on the machine table 61, and the positioning rod 63 is adapted to the positioning hole of the flux-cored welding wire powder filling device, so that the powder can fall into the U-shaped steel belt 50 as much as possible after leaving the powder feeder 21, so as to avoid more powder falling outside the U-shaped steel belt 50 due to inaccurate assembly.
[0098] Specifically, the positioning hole is located on the sensor mounting plate 43, and the positioning rod 63 is only inserted into the positioning hole and adapted to the positioning hole, and is not fixed by bolts or studs and nuts. Therefore, the positioning rod 63 only prevents the position of the flux-cored wire powder filling device from being fixed on the horizontal plane, and does not transmit the vibration of the machine table 61 in the vertical direction to the first bracket 41. The feeding mechanism 10 generates additional load on the weighing mechanism 30 due to vibration, which affects the weighing accuracy of the weighing mechanism 30. Specifically, the positioning rod 63 may include a positioning seat, a threaded hole is provided on the positioning seat, and a through hole is provided on the machine table 61. The through hole accommodates bolts or screws that pass through the bottom of the table of the machine table 61 and are threadedly connected to the threaded hole on the positioning seat to fix the positioning rod 63.
[0099] In addition, a forming machine roll stand is installed on the machine table 61, and the forming machine roll stand includes a forming roll stand and a reducing roll stand. The forming roll stand is arranged at the upstream and downstream sides of the flux-cored wire powder filling device, and is responsible for rolling the steel strip into a U shape, and closing the U-shaped steel strip 50 filled with powder to form a ring. The reducing roll stand is arranged at the downstream side of the flux-cored wire powder filling device, and is located at the downstream side of all the forming roll stands.
[0100] Embodiment 4: The flux-cored welding wire forming machine unit provided in this embodiment includes a tape unwinding machine and the above-mentioned flux-cored welding wire forming machine main unit.
[0101] Since the flux-cored welding wire forming machine unit provided in this embodiment includes the above-mentioned flux-cored welding wire forming machine main unit, it has the corresponding technical effects of the above-mentioned flux-cored welding wire forming machine main unit, which will not be repeated here.
[0102] In addition to the unwinding machine and the flux-cored wire forming machine main unit, the flux-cored wire forming unit may also include a steel strip cleaning machine, which may be arranged between the forming machine main unit and the unwinding machine. Among them, the unwinding machine may be an active unwinding machine or a passive unwinding machine, which is not limited in this embodiment. In addition, if the flux-cored wire forming unit is a rolling and drawing integrated flux-cored wire forming unit, it may also include a rough drawing unit and a wire take-up machine. If the semi-finished product size is processed by rolling, the powder in the flux-cored wire is densely filled, and there will be no movement of powder in the length direction of the wire due to the wire being in a state or being transported, causing uneven filling rate. In this case, a wire take-up machine may be directly arranged behind the forming machine main unit to take up the semi-finished wire.
[0103] Of course, if the welding wire is directly processed to the finished size by connecting a wire drawing unit to the main forming machine, or if the full rolling method or rolling plus wire drawing method is continued after the main forming machine, the welding wire can also be processed to the finished size, which can also be regarded as the flux-cored welding wire forming unit of this application.
[0104] Embodiment 5: This embodiment provides a flux-cored welding wire production line, including the above-mentioned flux-cored welding wire forming unit.
[0105] For example, if the flux-cored welding wire forming unit is a flux-cored welding wire forming unit that only processes semi-finished welding wire, the flux-cored welding wire production line may also include a fine drawing unit to process the flux-cored welding wire to a finished product size. In addition, it may also include at least one of a common welding wire layer winding unit, a steel strip layer winding unit, and a slitting unit.
[0106] In the description of the present application, it should be understood that the terms "upper", "lower", "front", "back", "left", "right", "horizontal", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0107] In addition, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. In the description of the present invention, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.
[0108] In the description of the present invention, a large number of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.
[0109] In the description of this specification, specific features, structures, materials or characteristics can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples without contradiction.
[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents, and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A flux-cored welding wire powder filling device, characterized in that: The invention comprises a powder feeder (21), a feeding mechanism (10), a first bracket (41), a second bracket (42) and a weighing mechanism (30), wherein the feeding mechanism (10) is arranged above the powder feeder (21), the feeding mechanism (10) comprises a feeding valve (13), a first fixed hopper (11) and a final feeding member, the final feeding member is located below the first fixed hopper (11) and is used to directly supply powder to the powder feeder (21), the feeding valve (13) is located above the first fixed hopper (11) and is vertically connected to the inlet end of the first fixed hopper (11). The powder feeder (21) and the first fixed hopper (11) are relatively fixedly arranged with respect to the first bracket (41), the first bracket (41) and the second bracket (42) are relatively movably arranged in the vertical direction, the first bracket (41) is supported by the weighing end of the weighing mechanism (30), the mounting end of the weighing mechanism (30) and the second bracket (42) are relatively fixedly arranged, and the weighing mechanism (30) is used to obtain the reduction of the weighing value at different times during the powder feeding process to obtain the change speed of the powder weight so as to control the running speed of the powder feeder (21); The inlet end of the first fixed hopper (11) is softly connected to the feeding valve (13); the feeding mechanism (10) further comprises a movable hopper (15), the movable hopper (15) is detachably mounted on the second bracket (42), and the movable hopper (15) is located above the feeding valve (13); the first bracket (41) comprises a powder feeder bracket, the powder feeder bracket is mounted with the powder feeder (21), the powder feeder bracket is mounted with a dustproof box (23), the powder feeder bracket is relatively fixedly arranged with the fixed hopper bracket, and the fixed hopper bracket is fixedly mounted with the first fixed hopper (11).
2. A flux-cored welding wire powder filling device according to claim 1, characterized in that: The flux-cored welding wire powder filling device further comprises a powder collecting trough (22), wherein the powder collecting trough (22) is mounted on the bottom of the first bracket (41).
3. A flux-cored welding wire powder filling system, characterized in that: It comprises a steel strip speed measuring device, an online steel strip cross-section measuring device, a control device and a flux-cored welding wire powder filling device according to any one of claims 1 to 2, wherein the steel strip speed measuring device, the online steel strip cross-section measuring device and the flux-cored welding wire powder filling device are all electrically connected to the control device, the steel strip speed measuring device is used to measure the running speed of the steel strip, the online steel strip cross-section measuring device is used to measure the width and thickness of the steel strip cross-section, and the control device is used to control the powder feeding speed of the powder filling device according to the speed, thickness and width of the steel strip.
4. A flux-cored welding wire forming machine main machine, characterized in that: A flux-cored welding wire powder filling device comprising any one of claims 1-2.
5. A flux-cored welding wire forming machine main machine according to claim 4, characterized in that: The molding machine mainframe comprises a machine platform (61), to which a positioning rod (63) is fixedly connected, and the positioning rod (63) is adapted to a positioning hole provided on the flux-cored welding wire powder filling device.
6. A flux-cored welding wire forming unit, characterized in that: It comprises a tape unwinding machine and the flux-cored welding wire forming machine main machine of claim 5.
7. A flux-cored welding wire production line, characterized in that: A flux-cored welding wire forming machine unit comprising the flux-cored welding wire forming machine unit of claim 6.