Granular citric acid-soluble silicon fertilizer and preparation method thereof
Through the mixed granulation of silicon source, activator and auxiliary agent and the assisted microwave activation of expanded graphite, the long activation time of silicon fertilizer and the problem of binder dilution is solved, and a high content and high strength granular wolfberry soluble silicon fertilizer is obtained, which is simplified The production process.
Patent Information
- Application Number
- CN202110311933.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-03-24
AI Technical Summary
In the existing silicon fertilizer production methods, high temperature activation time is long and binder needs to be added, resulting in a decrease in the proportion of active ingredients and affecting the performance of silicon fertilizer.
Mixed silicon source, activator and additives, add water to granulate, and aged and microwave activation, and use expanded graphite to assist in coordinated activation to avoid adding binder, shorten activation time, and increase effective silicon content.
It has achieved efficient shortening of activation time, increased the effective silicon, calcium and potassium content in granular wolfberry-soluble silicon fertilizer, met the standards and simplified production process.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicon fertilizers, and in particular to a granular citric acid-soluble silicon fertilizer and a preparation method thereof. Background Art
[0002] Compared with powdered silicon fertilizer, granular silicon fertilizer does not generate dust during use and has better fertilization effect. Therefore, granular silicon fertilizer is generally produced by adding a binder to powdered silicon fertilizer for granulation, and a muffle furnace or a rotary kiln is mostly used for high-temperature activation during the production of silicon fertilizer. However, this production method has the following main problems: 1) The addition of a binder will dilute the active ingredients in the silicon fertilizer, reduce the proportion of the active ingredients, and affect the performance of the silicon fertilizer. 2) The heating method of heat conduction makes the activation time long and the energy consumption high.
[0003] Therefore, it is urgent to provide a method for preparing granular citric acid-soluble silicon fertilizer with a short high-temperature activation time and without adding a binder. Summary of the invention
[0004] The purpose of the present invention is to solve the problem that the high temperature activation time of silicon fertilizer is long and the addition of binder will reduce the effective components of silicon fertilizer, and to provide a granular citric acid soluble silicon fertilizer and a preparation method thereof. The method has the advantages of short activation time, high effective silicon content in the obtained granular citric acid soluble silicon fertilizer, and can meet the standard requirements of silicon fertilizer.
[0005] In order to achieve the above object, the first aspect of the present invention provides a method for preparing granular citric acid-soluble silicon fertilizer, the method comprising the following steps:
[0006] (1) mixing a silicon source, an activator and an auxiliary agent, adding water and granulating to obtain a granular material; wherein the content of silicon dioxide in the silicon source is ≥44wt%;
[0007] (2) aging the granular material to obtain an aged material;
[0008] (3) mixing the aged material with expanded graphite and performing microwave activation to obtain an activated material;
[0009] (4) separating the activated material to obtain granular citric acid-soluble silicon fertilizer.
[0010] The second aspect of the present invention provides a granular citric acid-soluble silicon fertilizer prepared by the preparation method described in the first aspect of the present invention.
[0011] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:
[0012] 1) The preparation method of the granular citric acid-soluble silicon fertilizer provided by the present invention uses fly ash, fly ash aluminum extraction residue or silica sand as a silicon source, and then mixes with an activator and an auxiliary agent and adds water to granulate, without adding a binder, and is assisted by the subsequent aging and microwave activation steps and conditions of the present invention, while simplifying the production process, it is possible to obtain a granular citric acid-soluble silicon fertilizer with an effective silicon content of 20-40wt%, an effective calcium content of 10-30wt%, an effective potassium content of 5-25wt%, and a strength between 10-80N;
[0013] 2) The preparation method of the granular citric acid-soluble silicon fertilizer provided by the present invention utilizes expanded graphite to assist microwaves in the coordinated activation of aged materials, which greatly shortens the activation time, so that the content of effective silicon in the obtained granular citric acid-soluble silicon fertilizer is above 20wt%;
[0014] 3) The preparation method of the granular citric acid-soluble silicon fertilizer provided by the present invention selects a calcium-based activator and a potassium-based auxiliary agent, thereby increasing the content of effective calcium and effective potassium in the obtained granular citric acid-soluble silicon fertilizer. DETAILED DESCRIPTION
[0015] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0016] The first aspect of the present invention provides a method for preparing granular citric acid-soluble silicon fertilizer, the method comprising the following steps:
[0017] (1) mixing a silicon source, an activator and an auxiliary agent, adding water and granulating to obtain a granular material; wherein the content of silicon dioxide in the silicon source is ≥44wt%;
[0018] (2) aging the granular material to obtain an aged material;
[0019] (3) mixing the aged material with expanded graphite and performing microwave activation to obtain an activated material;
[0020] (4) separating the activated material to obtain granular citric acid-soluble silicon fertilizer.
[0021] Among them, the inventor of the present invention has found through research that when a silicon source with a silicon dioxide content of ≥44wt% is used as a raw material to prepare a granular citric acid soluble silicon fertilizer, the silicon source can be directly granulated without adding any binder after being mixed with an activator and an auxiliary agent. Moreover, after the aged material is mixed with expanded graphite, expanded graphite is used to assist microwave synergistic activation to replace the muffle furnace roasting activation, which can not only greatly shorten the activation time, but also improve the degree of activation, and further increase the content of effective silicon in the obtained granular citric acid soluble silicon fertilizer.
[0022] In step (1),
[0023] In a preferred embodiment, the content of silicon dioxide in the silicon source is ≥50 wt%, preferably ≥56 wt%.
[0024] In a preferred embodiment, the silicon source is selected from at least one of fly ash, fly ash aluminum extraction residue, and silica sand and gravel, preferably fly ash aluminum extraction residue.
[0025] In a preferred embodiment, the activator is selected from calcium oxide and / or calcium hydroxide, preferably calcium hydroxide.
[0026] In a preferred embodiment, the auxiliary agent is selected from potassium carbonate and / or potassium hydroxide, preferably potassium carbonate.
[0027] In a preferred embodiment, the mass ratio of the silicon source, the activator and the auxiliary agent is 1:0.42-0.76:0.15-0.7, preferably 1:0.5-0.68:0.2-0.4.
[0028] In a preferred embodiment, the silicon source, activator and auxiliary agent are preferably ground before adding water to granulate after mixing; wherein the average particle size of the ground material is 100-400 mesh, preferably 200-325 mesh.
[0029] In the present invention, the inventor has found through research that the particle size of the material after grinding is between 100-400 meshes, which is conducive to the generation of starters and the growth of particles, and can promote granulation. If the particle size of the material after grinding is too small, it will cause dust.
[0030] In a preferred embodiment, the amount of water added during the granulation is 20-50wt%, preferably 30-40wt%, of the total amount of the silicon source, the activator and the auxiliary agent.
[0031] In the present invention, if too much water is added, it will cause adhesion between particles or make the particle size of the granulated product larger, and if too little water is added, it will cause insufficient viscosity to affect the molding effect and reduce the particle strength. When the amount of water added is controlled within the above range, the strength of the obtained granular material is optimal, thereby improving the particle strength of the granular citric acid-soluble silicon fertilizer.
[0032] In a preferred embodiment, the particle size of the granular material is 1-10 mm, preferably 1-5 mm.
[0033] In step (2),
[0034] In a preferred embodiment, the aging conditions include: an aging temperature of 30-90°C, preferably 30-60°C; an aging time of 0.5-10h, preferably 2-6h. The aging process helps to improve the strength of the granular citric acid soluble silicon fertilizer and enhance the stability of the shape of the granular citric acid soluble silicon fertilizer.
[0035] In a preferred embodiment, the water content of the aged material is 5-20 wt %, preferably 7-15 wt %.
[0036] In step (3),
[0037] In a preferred embodiment, the mass ratio of the aged material to the expanded graphite is 1:0.2-1.5, preferably 1:0.3-0.8. Among them, the use of expanded graphite to assist microwave synergistic activation of the aged material can better utilize microwaves, improve the adaptability of raw materials for microwave activation, shorten the activation time, and improve the activation effect. The present invention does not specifically limit the particle size of the expanded graphite, and the expanded graphite can be separated from the prepared granular citric acid-soluble silicon fertilizer by screening.
[0038] In a preferred embodiment, the microwave activation conditions include: heating to 600-900° C. within 0.5-5 min and keeping warm for 2-30 min; preferably, heating to 700-900° C. within 1-3 min and keeping warm for 5-20 min.
[0039] In a preferred embodiment, the microwave activation condition further includes being carried out under the protection of an inert gas, wherein the inert gas is preferably nitrogen.
[0040] In step (4),
[0041] In a preferred embodiment, the activated material includes granular citric acid-soluble silicon fertilizer and expanded graphite, and the activated material is separated to obtain expanded graphite. The present invention does not specifically limit the separation, and screening is preferred. The separated expanded graphite can be reused.
[0042] The second aspect of the present invention provides a granular citric acid-soluble silicon fertilizer prepared by the preparation method described in the first aspect of the present invention.
[0043] In a preferred embodiment, the effective silicon content in the granular citric acid-soluble silicon fertilizer is 20-40wt%, preferably 25-35wt%, and more preferably 31-34.5wt%; the effective calcium content is 10-30wt%, preferably 14-25wt%, and more preferably 18-20wt%; the effective potassium content is 5-25wt%, preferably 8-20wt%, and more preferably 12-14.5wt%. Wherein, the effective silicon in the granular citric acid-soluble silicon fertilizer is calculated as SiO2, the effective calcium is calculated as Ca element, and the effective potassium is calculated as K2O.
[0044] In a preferred embodiment, the strength of the granular citric acid-soluble silicon fertilizer is 10-80N, preferably 14-40N.
[0045] The present invention will be described in detail below through examples. The effective silicon content in the examples and comparative examples is determined according to the industry standard NY-T 797-2004 "Silicon Fertilizer", and the effective silicon content is qualified when it exceeds 20%. The effective calcium content is determined according to NY-T 2272 "Determination of Calcium, Magnesium and Silicon Content of Soil Conditioners", and the effective potassium content is determined according to NY-T 2273 "Determination of Phosphorus and Potassium Content of Soil Conditioners". The strength of the granular citric acid-soluble silicon fertilizer is determined by a particle strength tester.
[0046] Example 1
[0047] (1) A fly ash acid-process aluminum extraction residue (silicon dioxide content 68%), calcium hydroxide and potassium carbonate are mixed in a mass ratio of 1:0.58:0.3 and ground, wherein the average particle size of the ground material is 200 meshes, the ground material is placed in a granulator, and water is added for granulation, wherein the amount of water is 35wt% of the total amount of the fly ash acid-process aluminum extraction residue, calcium hydroxide and potassium carbonate, to obtain a granular material with an average particle size of 3mm;
[0048] (2) aging the granular material obtained in step (1) at 30° C. for 6 h to obtain an aged material having a water content of 10 wt %;
[0049] (3) mixing the aged material obtained in step (2) with expanded graphite in a mass ratio of 1:0.5 and placing the mixture in a quartz crucible, heating the mixture in a microwave oven under a nitrogen atmosphere until the temperature rises to 760° C. for 1 min, and then keeping the temperature at 760° C. for 7 min. Then turning off the microwave, cooling the mixture naturally, and taking it out to obtain an activated material;
[0050] (4) Screening the activated material obtained in step (3) to obtain granular citric acid-soluble silicon fertilizer.
[0051] After testing, the obtained granular citric acid-soluble silicon fertilizer had an effective silicon content of 32.6wt%, an effective calcium content of 19.6wt%, an effective potassium content of 13wt%, and a strength of 32N.
[0052] Example 2
[0053] (1) Silica sand (silicon dioxide content 79%), calcium hydroxide and potassium carbonate are mixed in a mass ratio of 1:0.65:0.35 and ground, wherein the average particle size of the ground material is 200 meshes, the ground material is placed in a granulator, and water is added for granulation, wherein the amount of water is 35wt% of the total amount of silica sand, calcium hydroxide and potassium carbonate, to obtain a granular material with an average particle size of 3 mm;
[0054] (2) aging the granular material obtained in step (1) at 60° C. for 2 h to obtain an aged material having a water content of 11 wt %;
[0055] (3) mixing the aged material obtained in step (2) with expanded graphite in a mass ratio of 1:0.4 and placing the mixture in a quartz crucible, heating the mixture in a nitrogen atmosphere by microwave, heating the mixture to 860° C. for 1 min, keeping the mixture at 860° C. for 10 min, turning off the microwave, cooling the mixture naturally and taking it out to obtain an activated material;
[0056] (4) Screening the activated material obtained in step (3) to obtain granular citric acid-soluble silicon fertilizer.
[0057] After testing, the obtained granular citric acid-soluble silicon fertilizer has an effective silicon content of 22wt%, an effective calcium content of 20.5wt%, an effective potassium content of 14.6wt%, and a strength of 15N.
[0058] Example 3
[0059] (1) fly ash (silicon dioxide content 56%), calcium hydroxide and potassium carbonate are mixed in a mass ratio of 1:0.52:0.28 and ground, wherein the average particle size of the ground material is 200 meshes, the ground material is placed in a granulator, and water is added for granulation, wherein the amount of water is 35wt% of the total amount of fly ash, calcium hydroxide and potassium carbonate, to obtain a granular material with an average particle size of 3 mm;
[0060] (2) aging the granular material obtained in step (1) at 30° C. for 6 h to obtain an aged material having a water content of 10 wt %;
[0061] (3) mixing the aged material obtained in step (2) with expanded graphite in a mass ratio of 1:0.5 and placing the mixture in a quartz crucible, heating the mixture in a microwave oven under a nitrogen atmosphere until the temperature rises to 800° C. for 1 min, and then keeping the temperature at 800° C. for 7 min. Then turning off the microwave, cooling the mixture naturally, and taking it out to obtain an activated material;
[0062] (4) Screening the activated material obtained in step (3) to obtain granular citric acid-soluble silicon fertilizer.
[0063] After testing, the obtained granular citric acid-soluble silicon fertilizer had an effective silicon content of 25.9wt%, an effective calcium content of 18.5wt%, an effective potassium content of 12.4wt%, and a strength of 19N.
[0064] Example 4
[0065] The preparation method is the same as that of Example 1, except that:
[0066] In step (3), "mixing the aged material obtained in step (2) with expanded graphite in a mass ratio of 1:0.5" is replaced by "mixing the aged material obtained in step (2) with expanded graphite in a mass ratio of 1:0.2".
[0067] After testing, the obtained granular citric acid-soluble silicon fertilizer has an effective silicon content of 27.4wt%, an effective calcium content of 18.8wt%, an effective potassium content of 12.5wt%, and a strength of 28N.
[0068] Example 5
[0069] The preparation method is the same as that of Example 1, except that:
[0070] In step (3), “microwave heating under a nitrogen atmosphere, raising the temperature to 760°C for 1 min, and then keeping it at 760°C for 7 min” is replaced with “microwave heating under a nitrogen atmosphere, raising the temperature to 650°C for 1 min, and then keeping it at 650°C for 4 min”.
[0071] After testing, the obtained granular citric acid-soluble silicon fertilizer had an effective silicon content of 23.2wt%, an effective calcium content of 18.3wt%, an effective potassium content of 12.1wt%, and a strength of 27N.
[0072] Example 6
[0073] The preparation method is the same as that of Example 3, except that:
[0074] In step (1), “mix fly ash (silicon dioxide content 56%), calcium hydroxide and potassium carbonate in a mass ratio of 1:0.52:0.28” is replaced with “mix fly ash (silicon dioxide content 56%), calcium hydroxide and potassium carbonate in a mass ratio of 1:0.48:0.23”.
[0075] After testing, the obtained granular citric acid-soluble silicon fertilizer has an effective silicon content of 21.3wt%, an effective calcium content of 17wt%, an effective potassium content of 10.2wt%, and a strength of 17N.
[0076] Comparative Example 1
[0077] (1) A fly ash acid-process aluminum extraction residue (silicon dioxide content 68wt%), calcium hydroxide and potassium carbonate are mixed in a mass ratio of 1:0.58:0.3 and ground, wherein the average particle size of the ground material is 200 meshes, the ground material is placed in a granulator, and water is added for granulation, wherein the amount of water is 35wt% of the total amount of the fly ash acid-process aluminum extraction residue, calcium hydroxide and potassium carbonate, to obtain a granular material with an average particle size of 3mm;
[0078] (2) aging the granular material obtained in step (1) at 30° C. for 6 h to obtain an aged material having a water content of 10 wt %;
[0079] (3) placing the aged material obtained in step (2) in a muffle furnace, heating under a nitrogen atmosphere, rising to 760° C. for 70 min, keeping warm at 760° C. for 7 min, and taking out after natural cooling to obtain a granular citric acid-soluble silicon fertilizer.
[0080] After testing, the content of effective silicon in the obtained granular citric acid soluble silicon fertilizer was 10.4wt%, which did not meet the requirements of silicon fertilizer. The content of effective calcium was 18.9wt%, the content of effective potassium was 12.6wt%, and the strength of the granular citric acid soluble silicon fertilizer was 28N.
[0081] Comparative Example 2
[0082] The same as Example 1, except that: fly ash with a silicon dioxide content of 35wt% is used to replace the fly ash acid method aluminum extraction residue in Example 1 to obtain granular citric acid-soluble silicon fertilizer.
[0083] After testing, the content of effective silicon in the obtained granular citric acid soluble silicon fertilizer was 9.7wt%, which did not meet the requirements of silicon fertilizer. The content of effective calcium was 18wt%, the content of effective potassium was 12.2wt%, and the strength of the granular citric acid soluble silicon fertilizer was 14N.
[0084] Comparative Example 3
[0085] The same as Example 1, except that: flake graphite is used to replace expanded graphite to obtain granular citric acid soluble silicon fertilizer.
[0086] After testing, the content of effective silicon in the obtained granular citric acid soluble silicon fertilizer was 8.9wt%, which did not meet the requirements of silicon fertilizer. The content of effective calcium was 17.9wt%, the content of effective potassium was 12.4wt%, and the strength of the granular citric acid soluble silicon fertilizer was 26N.
[0087] Comparative Example 4
[0088] The same as Example 1, except that: the fly ash acid method aluminum extraction residue (silicon dioxide content 68%), calcium hydroxide and potassium carbonate are mixed in a mass ratio of 1:0.2:0.1 to obtain granular citric acid-soluble silicon fertilizer.
[0089] After testing, the content of effective silicon in the obtained granular citric acid soluble silicon fertilizer was 5.1wt%, which did not meet the requirements of silicon fertilizer. The content of effective calcium was 8.9wt%, the content of effective potassium was 5.4wt%, and the strength of the granular citric acid soluble silicon fertilizer was 20N.
[0090] Comparative Example 5
[0091] The same as Example 1, except that step (2) is omitted, and the granular material obtained in step (1) is directly mixed with expanded graphite and then microwave activated. The silicon fertilizer thus obtained is partially cracked and the particles are incomplete.
[0092] According to the test, the content of effective silicon in the obtained citric acid-soluble silicon fertilizer was 27wt%, the content of effective calcium was 18.9wt%, and the content of effective potassium was 12.4wt%.
[0093] It can be seen from Examples 1-6 of the present invention that the preparation method of the granular citric acid-soluble silicon fertilizer provided by the present invention can greatly shorten the activation time, improve the activation effect, and obtain high-quality granular citric acid-soluble silicon fertilizer with relatively high contents of effective silicon, effective calcium and effective potassium.
[0094] By comparing Example 1 and Comparative Example 1, it can be seen that under the same activation temperature and activation time, compared with the muffle furnace roasting activation, the method of using expanded graphite to assist microwave synergistic activation in the present invention can significantly improve the degree of activation and increase the content of effective elements in the obtained granular citric acid-soluble silicon fertilizer.
[0095] By comparing Example 1 and Comparative Example 3, it can be seen that under the same conditions, the content of effective silicon in the granular citric acid-soluble silicon fertilizer obtained by using expanded graphite to assist microwave synergistic activation is 23.7wt% higher than the content of effective silicon in the granular citric acid-soluble silicon fertilizer obtained by using flake graphite to assist microwave synergistic activation.
[0096] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing granular citric acid-soluble silicon fertilizer, characterized in that: The method comprises the following steps: (1) A silicon source, an activator and an auxiliary agent are mixed and then water is added to granulate to obtain a granular material; wherein the content of silicon dioxide in the silicon source is ≥50wt%; wherein the activator is selected from calcium oxide and / or calcium hydroxide, and the auxiliary agent is selected from potassium carbonate and / or potassium hydroxide; and the mass ratio of the silicon source, the activator and the auxiliary agent is 1:0.42-0.76:0.15-0.7; (2) aging the granular material to obtain an aged material; (3) mixing the aged material with expanded graphite and performing microwave activation to obtain an activated material; (4) Separating the activated material to obtain expanded graphite and granular citric acid-soluble silicon fertilizer.
2. The preparation method according to claim 1, wherein The content of silicon dioxide in the silicon source is ≥56wt%.
3. The preparation method according to claim 1 or 2, wherein The silicon source is selected from at least one of fly ash, fly ash aluminum extraction residue, and silica sand.
4. The preparation method according to claim 1 or 2, wherein: The silicon source is the aluminum extraction residue from fly ash.
5. The preparation method according to claim 1, wherein The activator is calcium hydroxide.
6. The preparation method according to claim 1, wherein The auxiliary agent is potassium carbonate.
7. The preparation method according to claim 1, wherein The mass ratio of the silicon source, the activator and the auxiliary agent is 1:0.5-0.68:0.2-0.
4.
8. The preparation method according to claim 1, wherein The aging conditions include: aging temperature of 30-90° C., and aging time of 0.5-10 h.
9. The preparation method according to claim 8, wherein: The aging conditions include: aging temperature of 30-60° C., and aging time of 2-6 hours.
10. The preparation method according to claim 1, wherein: The mass ratio of the aged material to the expanded graphite is 1:0.2-1.
5.
11. The preparation method according to claim 9, wherein: The mass ratio of the aged material to the expanded graphite is 1:0.3-0.
8.
12. The preparation method according to claim 1, wherein: The microwave activation conditions include: heating to 600-900° C. within 0.5-5 minutes and keeping the temperature for 2-30 minutes.