A method for processing tin-immersion plate to prevent rats from biting
Through steps such as acidic cleaning, oil removal, micro-etching, activation and chemical tin deposition, a tin plating layer is formed and tin whiskers are repaired, which solves the problem of spontaneous growth of tin whiskers in the chemical tin deposition layer and improves the signal transmission stability and reliability of electronic products. sex.
Patent Information
- Application Number
- CN202210720223.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-06-23
AI Technical Summary
The chemical immersion tin layer spontaneously grows tin whiskers in electronic products, leading to the risk of circuit short circuits and incomplete signal transmission, affecting product reliability and performance. The rat bite phenomenon of chemical immersion tin has an important impact on the stability of signal transmission.
Acidic cleaning, oil removal, micro-etching, copper surface activation and chemical tin deposition are used to form a tin plating layer, and the growing tin whiskers are inspected and repaired in post-processing. The growth of tin whiskers is reduced by doubling the solder and absorbing tin tape. Increase the thickness of the tin layer and sink the tin again every 1 hour to enhance signal transmission stability.
It effectively reduces the growth of tin whiskers, avoids the impact on signal integrity and stability, improves the reliability and performance of electronic products, and ensures the continuity and quality of signal transmission.
Smart Images

Figure CN115135025B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of PCB boards, and in particular relates to a method for processing a tin-immersion board that can prevent rats from biting. Background Art
[0002] As the world promotes environmental protection, lead-containing solder is banned, and products begin to use lead-free solder to complete the welding between PCB and components, such as the currently commonly used solder Sn, Ag, Cu alloy system. Traditional leaded tin spraying is gradually replaced by a wide variety of lead-free surface treatments, such as: immersion gold, immersion silver, immersion tin, lead-free tin spraying, OSP, etc. Among them, the chemical immersion tin process has better wetting performance than other surface treatments and has become a popular surface treatment.
[0003] However, with the promotion of PCB chemical tinning surface treatment, it is found that the chemical tinning layer spontaneously grows tin whiskers, which bury the fatal risk for the reliability of electronic products. Tin whiskers are a kind of slender pure tin crystal whiskers that grow spontaneously from the surface of pure tin or tin alloy plating. The existence of tin whiskers not only puts the circuit at risk of short circuit, but also may affect the integrity of signal transmission, and have an adverse effect on the reliability and performance of the whole product. In addition, compared with the Giovanni phenomenon of chemical silver, the rat bite phenomenon of chemical tinning has less effect on the electrical performance of the circuit, so it has not attracted enough attention. However, with the development of communication technology, due to the excellent flatness of chemical tinning surface treatment and the low attenuation of transmission signals, it has been widely used in the surface treatment of communication boards, especially chemical tinning of Teflon antenna materials. This type of chemical tinning requires that the attenuation of its material is small during signal transmission. At this time, the rat bite problem of chemical tinning will have an important impact on signal transmission and stability. Summary of the invention
[0004] The object of the present invention is to provide a method for processing a tin-immersion board that can prevent rat bites, so as to avoid the signal integrity transmission being affected by tin whiskers and rat bites.
[0005] The present invention provides a method for processing a tin-immersion plate for preventing rats from biting, comprising the following steps:
[0006] (1) Acid cleaning: Use PSH-1640 cleaner to clean the copper substrate to remove light grease and oxides on the copper surface, make the copper surface clean and increase wettability. 2 20ml of cleaning agent needs to be added to the PCB board;
[0007] (2) Degreasing: Use 3-8% Enthone PC-7086 degreasing solution to remove grease from the board surface and ensure that the copper surface of the substrate is evenly micro-etched. 2 The substrate needs to be added with 25ml of degreasing solution;
[0008] (3) Micro-etching: Use a 30% micro-etching agent, PSH-1630, to slightly etch the copper surface to ensure that the oxide on the copper foil surface is completely removed. 2 Copper substrate needs to add 1L micro-etching agent;
[0009] (4) Copper surface activation: Use pre-dip solution to soak the copper substrate for 15 minutes each time the copper substrate is treated. 2 It is necessary to add 1L of tin solution and replace the pre-dip solution once a month. The pre-dip solution should be PSH-2200.
[0010] (5) Chemical tinning: The pickled, microetched and activated copper substrate is placed in a tinning solution, and the chemical potential of the copper ions is changed to cause a chemical replacement reaction of the stannous ions in the plating solution, and the reduced tin metal is deposited on the surface of the copper substrate to form a tin plating layer;
[0011] (6) Post-processing: Check and determine whether tin whiskers grow in the tin layer;
[0012] (7) Hot water washing and drying: Use hot water to clean the substrate, and then dry and store it.
[0013] Furthermore, during the cleaning process of step (1), the temperature is maintained at 40-50° C. and the cleaning time is 2-4 minutes.
[0014] Furthermore, during the degreasing process in step (2), the temperature is maintained at 45-55° C. and the cleaning is performed for 20 seconds.
[0015] Furthermore, during the micro-etching process of step (3), the temperature is maintained at 25-30° C. and the cleaning time is 30-90 seconds.
[0016] Furthermore, the temperature of the pre-soak in step (4) is maintained at 22-32° C., and the pre-soak is continuously stirred and circulated, and is continuously filtered with a filter element with a pore size of less than 5 μm, and soaked for 1-2 minutes.
[0017] Furthermore, in the step (5), the temperature during the tinning process is maintained at 50-70° C. for 1-25 minutes, and heating is continued during the process, and continuous filtering is performed using a filter element with a pore size of less than 5 um.
[0018] Furthermore, the tinning process of step (5) needs to be repeated after 1 hour.
[0019] Furthermore, in step (6), if tin whiskers are found after inspection, fresh solder is first added to the tin whiskers to double the amount of solder, and then excess solder is absorbed with a wicking tape, and finally necessary solder is applied to complete the rework.
[0020] Furthermore, the braid needs to be clean.
[0021] The present invention has the following beneficial effects: after cleaning and drying the substrate after tinning, the present invention performs post-processing. If tin whiskers are found to have grown after inspection, fresh solder is first added to the tin whiskers to double the amount of solder, and then excess solder is adsorbed with a tin-absorbing tape. Finally, necessary solder is applied to complete rework, thereby reducing the growth of tin whiskers and avoiding affecting the integrity of signal transmission. In addition, tinning needs to be performed again every 1 hour during the tinning process to increase the thickness of the tin layer and avoid affecting signal transmission and stability due to rat bites. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 : is the flow chart of the processing method of the present invention. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] The present invention is described in detail below in conjunction with the embodiments and drawings: A method for processing a tin-immersion plate to prevent rat bites comprises the following steps:
[0025] (1) Acid cleaning: Use PSH-1640 cleaner to clean the copper substrate to remove light grease and oxides on the copper surface, clean the copper surface and increase wettability. Keep the temperature at 40-50°C, clean for 2-4 minutes, and treat for 1m 2 PCB board needs to add 20ml of cleaning agent, which has the advantages of good water washability and does not attack the solder mask ink and image dry film of the circuit board;
[0026] (2) Degreasing: Use 3-8% Enthone PC-7086 degreasing solution to remove grease from the board surface. Keep the temperature at 45-55°C to ensure uniform micro-etching of the copper surface of the substrate. 2 The substrate needs to be added with 25ml of degreasing solution;
[0027] (3) Micro-etching: Use a micro-etching agent with a concentration of 30%. The micro-etching agent is PSH-1630. The micro-etching stage adopts a spraying method instead of an immersion method. Slightly etch the copper surface to ensure that the oxide on the surface of the copper foil is completely removed. The temperature is maintained at 25-30°C. Cleaning is performed for 30-90 seconds. The micro-etching amount is maintained at 1.0-2.0um. The SPS concentration is maintained at 60-120g / L. The treatment lasts for 1m 2 Copper substrate needs to add 1L micro-etching agent;
[0028] (4) Copper surface activation: Use pre-dip solution to soak the copper substrate. The pre-dip solution temperature is maintained at 22-32°C, the acidity is maintained at 0.25-1.0 mol / L, the complex is 10-60 g / L, the organic metal concentration is 10-60 mg / L, the silver content is 70-300 mg / L, and the Cu 2+ The concentration is less than 175mg / L, the water jet flow rate should be maintained at 30-60mg / L, and the water jet should be continuously stirred and circulated, and the filter should be continuously filtered with a filter element with a pore size of less than 5um, soaking for 1-2 minutes, and 15m per copper substrate. 2 It is necessary to add 1L of tin solution and replace the pre-dip solution once a month. The pre-dip solution should be PSH-2200.
[0029] (5) Chemical tinning: The copper substrate that has been pickled, micro-etched and activated is placed in a tinning solution. The chemical potential of the copper ions is changed to cause a chemical replacement reaction of the stannous ions in the plating solution. The reduced tin metal is deposited on the surface of the copper substrate to form a tin plating layer. The temperature is maintained at 50-70°C for 1-25 minutes. During the process, heating is continued and continuous filtering is performed with a filter element with a pore size of less than 5 μm. Tinning needs to be performed again every 1 hour.
[0030] (6) Post-processing: Check to determine whether tin whiskers grow in the tin layer. If tin whiskers are found after inspection, first add fresh solder to the tin whiskers to double the amount of solder, then use tin-absorbing tape to absorb excess solder, and finally apply necessary solder to complete the rework to reduce the growth of tin whiskers and avoid affecting the integrity of signal transmission. Clean tape needs to be used. Compared with clean tape, solder-impregnated tape is more likely to form tin whiskers;
[0031] (7) Hot water washing and drying: Use hot water to clean the substrate, and then dry and store it.
[0032] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the protection scope of the technical solutions of the present invention.
Claims
1. A method for processing tin-immersion plates to prevent rat bites. It is characterized in that The following steps are involved: (1) Acid cleaning: Use PSH-1640 cleaner to clean the copper substrate to remove light grease and oxides on the copper surface, clean the copper surface and increase wettability. To process 1㎡ of PCB board, 20ml of cleaner is required. (2) Degreasing: Use 3-8% Enthone PC-7086 degreasing solution to remove grease from the board surface and ensure that the copper surface of the substrate is evenly micro-etched. 2 The substrate needs to be added with 25ml of degreasing solution; (3) Micro-etching: Use a micro-etching agent with a concentration of 30%. The micro-etching agent is PSH-1630. Slightly etch the copper surface to ensure that the oxide on the surface of the copper foil is completely removed. 1L of micro-etching agent is required to process 1㎡ of copper substrate. (4) Copper surface activation: Use pre-dip solution to soak the copper substrate for 15 minutes each time the copper substrate is treated. 2 It is necessary to add 1L of tin solution and replace the pre-dip solution once a month. The pre-dip solution should be PSH-2200. (5) Chemical tinning: The pickled, microetched and activated copper substrate is placed in a tinning solution, and the chemical potential of the copper ions is changed to cause a chemical replacement reaction of the stannous ions in the plating solution, and the reduced tin metal is deposited on the surface of the copper substrate to form a tin plating layer; (6) Post-processing: prevent the tin surface from oxidizing and yellowing, and check whether the tin layer has tin whiskers; (7) Hot water washing and drying: Use hot water to wash the substrate, and then dry and store it; The temperature of the pre-dip solution in step (4) is maintained at 22-32° C., and the solution is continuously stirred and circulated, and is continuously filtered using a filter element with a pore size of less than 5 μm, and the solution is immersed for 1-2 minutes. In step (6), if tin whiskers are found to have grown after inspection, fresh solder is first added to the tin whiskers to double the amount of solder, and then excess solder is absorbed using a desoldering tape, and finally necessary solder is applied to complete the rework, and the tape needs to be a clean one.
2. A method for processing a tin-immersion plate to prevent rat bites according to claim 1, Features: During the cleaning process of step (1), the temperature is maintained at 40-50° C. and the cleaning time is 2-4 minutes.
3. A method for processing a tin-immersion plate to prevent rat bites according to claim 1, Features: During the degreasing process in step (2), the temperature is maintained at 45-55° C. and the cleaning is performed for 20 seconds.
4. A method for processing a tin-immersion plate to prevent rat bites according to claim 1, Features: During the micro-etching process of step (3), the temperature is maintained at 25-30° C. and the cleaning time is 30-90 seconds.
5. A method for processing a rat-proof tin plate according to claim 1, Features: During the tinning process in step (5), the temperature is maintained at 50-70° C. for 1-25 minutes, and heating is continued during the process, and continuous filtering is performed using a filter element with a pore size of less than 5 μm.
6. A method for processing a rat-proof tin plate according to claim 1, Features: The tinning process of step (5) needs to be repeated after 1 hour.