Desulfurization of lead waste

By controlling the pH value in lead-acid battery recycling and converting lead sulfate into lead oxide, the problem of low desulfurization efficiency and pollution in the existing technology is solved, and an efficient and low-energy lead recycling process is realized.

CN115135782BActive Publication Date: 2024-10-15AURELIUS ENVIRONMENTAL LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202080069496.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-12
Filing Date
2020-08-12
Publication Date
2024-10-15
Estimated Expiration
2040-08-12

AI Technical Summary

Technical Problem

In the existing lead-acid battery recycling process, the desulfurization efficiency is low, it is prone to high pollution and energy-intensive, and when sodium hydroxide is used, unnecessary by-product lead hydroxide is produced, resulting in serious lead load loss.

Method used

By controlling the pH value in the range of 11 to 15 during the desulfurization process, using hydroxide alkali to treat lead-containing waste, convert lead sulfate into lead oxide, avoid the formation of lead hydroxide, and achieve efficient conversion of lead sulfate into lead oxide. .

Benefits of technology

Efficient desulfurization is achieved, the purity and efficiency of lead recovery are improved, energy consumption and pollution are reduced, the generation of by-products is reduced, and the feasibility of the process is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003580098790000121
    Figure BDA0003580098790000121
Patent Text Reader

Abstract

The present invention relates to the desulfurization of lead-containing waste. In particular, the present invention relates to a method for desulfurizing lead-containing waste to obtain desulfurized lead-containing waste suitable for recovering lead or lead-containing oxides. The method is particularly suitable for desulfurization of lead-acid battery slurry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the desulfurization of lead-containing waste. In particular, the present invention relates to a method for desulfurizing lead-containing waste to obtain desulfurized lead-containing waste suitable for recovering lead or lead-containing oxides. The method is particularly suitable for desulfurization of lead-acid battery slurry. Background Art

[0002] Lead-acid batteries are widely used in industries such as automobiles due to their rechargeable nature and relatively low cost.

[0003] During discharge, the lead and lead dioxide on the battery plates are converted to lead sulfate. Charging the battery converts the lead sulfate back to lead and lead dioxide. Although lead-acid batteries are rechargeable, over time the lead sulfate crystallizes into large, passive crystals in the battery plates, which reduce the tendency of the lead sulfate to convert back to lead and lead dioxide. This results in a deterioration in battery performance. Eventually the battery will have to be replaced.

[0004] In Europe and the United States, a high percentage of scrap lead-acid batteries are recycled. In a typical process, scrap batteries are shredded and lead-containing solids are separated from other battery waste components, such as plastic materials and electrolytes. Lead-containing solids originate from battery plates, which consist of battery grids and battery slurry. The battery waste slurry is sent to a furnace for pyrometallurgical processing into lead ingots. The lead ingots can then be used to make new lead-acid batteries. For example, the lead ingots can be used to make new battery grids, or they can be oxidized using a Barton jar or ball milling process to produce lead-containing oxides, typically a mixture of lead oxide and free metallic lead. This lead-containing oxide can then be reused as an active redox material in lead-acid battery plates.

[0005] These conventional recycling processes are highly energy intensive, with temperatures of around 1100°C required for the decomposition of lead sulphate. Conventional recycling processes can also be highly polluting. In particular, sulphur dioxide, nitrogen dioxide and often lead particles are produced in high temperature furnaces. Specialised equipment and time are required to prevent pollutants from being released into the atmosphere. These can represent significant expenses in the recycling process.

[0006] Therefore, many current lead-acid battery recycling processes include a step in which the waste battery slurry is desulfurized before entering the furnace directly or indirectly. Typically, the waste battery slurry is desulfurized by mixing the slurry with an aqueous sodium carbonate solution in a leaching tank and mechanically stirring the mixture. The lead component is converted into lead carbonate, while the sulfate component is dissolved in the aqueous system in the form of sodium sulfate and can then be separated from the desulfurized slurry by filtration (see Lyakov et al., J. Power Sources 2007, 171, 960-965). However, it is difficult to achieve high levels of desulfurization using these methods, and the desulfurization level is typically in the range of 92% to 94%.

[0007] Although sodium hydroxide has been successfully used to desulfurize spent battery slurries to significant amounts—typically in the 94% to 97% range (see Lyakov above), this is still below the ideal level of desulfurization in industrial processes—without removing sulfur dioxide during the smelting process. In addition, these methods require the use of excess sodium hydroxide, which increases the reagent load of the process.

[0008] The limitation on the level of desulfurization achieved using sodium hydroxide in the prior art is believed to be due to the formation of lead hydroxides. These are hydrated forms of lead oxide, primarily in the form of Pb(OH)2 (or PbO·H2O), but other forms such as Pb5O3(OH)4 and Pb3O2(OH)2 (or 3PbO·H2O) may also be present. However, lead hydroxide tends to precipitate from aqueous solutions to form a colloidal mixture. The particles in the colloidal mixture may be large enough to cause stirring difficulties and filtering difficulties, thereby reducing the industrial feasibility of the prior art hydroxide desulfurization process. Soluble by-products formed in the prior art process, such as sodium lead acid, can also reduce the proportion of lead-containing waste that is recovered. The loss of lead loading is particularly severe in the prior art methods that use relatively large amounts of aqueous phase.

[0009]

[0006] Therefore, there is a need for a method of desulfurizing lead-containing waste, particularly waste from lead-acid batteries, that addresses one or more of the problems set forth above. Summary of the invention

[0010] The present invention is based on the surprising discovery that by maintaining the pH in the range of 11 to 15 during the desulfurization of lead-containing waste, a more selective formation of lead (II) oxide compared to other lead compounds can be achieved. In particular, in prior art methods where the pH is not controlled during the desulfurization reaction, the pH level drops rapidly as the hydroxide reagent is used up, which is believed to promote the formation of lead hydroxide. By controlling the pH value of the entire desulfurization step, thereby avoiding the formation of unwanted by-products, a near stoichiometric conversion of lead sulfate to lead (II) oxide can be achieved even when the sulfate content of the raw material is unknown. Therefore, the reaction may be highly selective and near stoichiometric for lead (II) oxide. This makes the process very efficient.

[0011] Therefore, in a first aspect, the present invention provides a method for desulfurization of lead-containing waste, wherein the lead-containing waste contains PbSO4, the method comprising:

[0012] (a) treating an aqueous slurry of the lead-containing waste with a hydroxide base, thereby forming a desulfurized lead-containing waste in which PbSO4 has been converted to PbO and an aqueous solution comprising sulfate anions; and

[0013] (b) separating the desulfurized lead-containing waste from the aqueous solution containing sulfate anions,

[0014] wherein the pH is maintained in the range of 11 to 15 during step (a).

[0015] The present invention further provides a desulfurized lead waste obtainable by the process defined herein, and a desulfurized lead waste, preferably a desulfurized lead-acid battery slurry, comprising by weight:

[0016] A content of at least 40% PbO;

[0017] A content of at least 10% PbO2;

[0018] A content of at least 1% Pb; and

[0019] Lead hydroxide containing less than 5%.

[0020] Also provided herein is a method for recycling lead-containing waste, the method comprising processing desulfurized lead-containing waste into lead-containing material, wherein the desulfurized lead-containing waste is as defined herein. The method preferably comprises providing desulfurized lead-containing waste using the method defined herein. DETAILED DESCRIPTION

[0021] Lead waste

[0022] The present invention provides a desulfurization method for lead-containing waste. The lead-containing waste includes lead sulfate (hereinafter referred to as PbSO4). The lead-containing waste may contain PbSO4 in an amount of at least 1% by weight, preferably at least 10% by weight, and more preferably at least 20% by weight.

[0023] The lead-containing waste used in step (a) may also contain lead in various forms other than PbSO4. For example, the lead-containing waste may contain metallic lead (referred to herein as Pb) or lead in the form of compounds, such as lead oxide (referred to herein as PbO for lead (II) oxide and PbO2 for lead (IV) oxide) or lead carbonate (referred to herein as PbCO3). It should be understood that these materials may be present in the form of compounds of these materials, such as PbO.PbSO4, 3PbO.PbSO4 or 4PbO.PbSO4 and hydrates thereof, although these forms may generally be present only in negligible amounts.

[0024] Preferably, the lead-containing waste used in step (a) contains at least one of Pb and PbO. More preferably, the lead-containing waste used in step (a) contains Pb and PbO. The lead-containing waste used in step (a) may further contain PbO2. Of course, the content of different lead-containing substances in the lead-containing waste will vary depending on the source of the lead-containing waste.

[0025] Non-lead components may also be present in the lead-containing waste, for example in an amount of at least 0.1 wt%, although they are typically present in an amount of less than 10 wt%, preferably less than 5 wt%, such as less than 3 wt% or less than 1 wt%. Non-lead components may include metal compounds, insoluble carbon materials and fibers. Metal compounds include barium sulfate, which is an additive that is typically included in lead-acid battery plates to minimize or control the crystallization of lead sulfate. Insoluble carbon materials are typically added as expanders for lead-acid battery plates and include carbon black, graphene and carbon nanotubes. Fibers typically included in lead-acid battery plates include lignin sulfonates. Non-lead components may also include polymers or glass, such as from separators that can be used in lead-acid batteries.

[0026] The method of the present invention is particularly suitable for recycling lead-acid battery slurry. Therefore, in some embodiments, the lead-containing waste used in step (a) is derived from lead-acid battery slurry. Lead-acid battery slurry typically contains PbSO4, PbO, PbO2 and Pb. The proportions of these components in the lead-acid battery slurry of a single cell may vary greatly, depending on the degree of "consumption" of the battery, that is, the degree of use. For example, the lead-acid battery slurry of a battery that is rarely used may itself be "waste", but will typically contain relatively large amounts of Pb and PbO2, and relatively small amounts of PbSO4 and PbO. In addition, if the lead-acid battery slurry is taken only from the negative plate, it may not contain any PbO2.

[0027] However, waste lead-acid batteries are typically composed of slurries from a large number of batteries, so the contents of different lead-containing materials are standardized to some extent. Therefore, the waste lead-acid battery slurry used in step (a) may contain at least 40 wt% PbSO4. The waste lead-acid battery slurry used in step (a) may contain at least 5 wt% PbO. The waste lead-acid battery slurry used in step (a) may contain at least 10 wt% PbO2. The waste lead-acid battery slurry used in step (a) may contain at least 1 wt% Pb.

[0028] Lead-acid battery slurry can be obtained from lead-acid batteries by known methods. For example, lead-acid battery slurry can be obtained by crushing one or more lead-acid batteries and separating the lead-containing waste from other components of the battery (e.g., plastic material and electrolyte). Therefore, in some embodiments, the present invention involves a pretreatment step in which the used batteries are crushed and the lead-containing solids are separated from other battery waste components such as plastic material and electrolyte before being used in step (a).

[0029] Leaded waste can also be obtained from many other sources. Leaded waste may come from mining, metallurgy or chemical plants. Leaded waste may be the product of PbS ore mining, which has been oxidized by roasting to contain impurities such as PbSO4 and silica.

[0030] In some cases, the method of the present invention is used to recycle electric arc furnace dust. Electric arc furnace dust is a residue from the steel production process. The presence of zinc in the dust and the increasing cost of disposal have led to schemes to recycle the dust. This is usually done using the Waelz process, in which zinc-containing materials are processed in a rotary kiln furnace. The process is usually carried out in the presence of carbon (e.g. in the form of coke), and preferably also in the presence of calcium oxide (CaO) or silicon dioxide (SiO2). The kiln is usually operated at a temperature of 1000 to 1500°C.

[0031] However, electric arc furnace dust contains many impurities, including lead-containing compounds. Therefore, in some embodiments, the lead-containing waste used in step (a) is derived from electric arc furnace dust.

[0032] The lead-containing waste material used in step (a) may be electric arc furnace dust obtained directly from steel production. In other words, the electric arc furnace dust has not been subjected to further processing steps, such as zinc recovery processes.

[0033] However, in a preferred embodiment, the lead-containing waste used in step (a) is the material remaining after zinc has been removed from electric arc furnace dust (e.g. in the Waelz process). This material is known as slag (or Waelz clinker) and typically contains at least 40 wt% PbSO4. Thus, the lead-containing waste used in step (a) may preferably be slag from the Waelz process, which contains at least 10 wt% PbSO4, preferably at least 20 wt%, more preferably at least 40 wt%.

[0034] In the case where the lead-containing material used in step (a) is slag from the Waelz process, the slag has preferably been subjected to a thermal pretreatment. It is believed that this can remove carbon-containing materials used in the Waelz process and that may be present in the Waelz slag, for example in an amount of at least 10 wt%. In some embodiments, the method of the present invention includes a step of pretreating the Waelz slag with heat, but in other embodiments the slag has been pretreated.

[0035] The pretreatment of the slag may be carried out at a temperature of at least 500° C., preferably at least 550° C., more preferably at least 600° C. The pretreatment of the slag may be carried out at a temperature of up to 800° C., preferably up to 750° C., more preferably up to 700° C. The pretreatment of the slag may be carried out at a temperature of 500 to 800° C., preferably 550 to 750° C., more preferably 600 to 700° C.

[0036] The pretreatment of slag can be carried out for at least 15 minutes, preferably at least 30 minutes, more preferably at least 45 minutes. The pretreatment of slag can be carried out for up to 4 hours, preferably up to 2 hours, more preferably up to 90 minutes. Therefore, the pretreatment of slag can be carried out for 15 minutes to 4 hours, preferably 30 minutes to 2 hours, more preferably 45 to 90 minutes.

[0037] Lead-containing waste may exist in various forms, such as in the form of dust, slag or sludge, or even in the form of minerals. However, the lead-containing waste used in step (a) is generally in the form of crushed, such as particles or powder. For example, the lead-containing waste used in step (a) can be in the form of particles, wherein the particles pass through a screen with a mesh diameter of 1 cm, preferably 5 mm, more preferably 2 mm. The lead-containing waste used in step (a) is generally a fairly coarse slurry mixture prepared by crushing the lead-containing waste.

[0038] As explained in more detail below, the particle size of the lead-containing waste may be further reduced in step (a) by comminution.

[0039] It will be appreciated that the lead-containing waste used in step (a) is in solid form. However, due to the process by which it is obtained, it may be coated in a liquid, such as battery acid, although any such liquid is not considered to be part of the lead-containing waste.

[0040] Step (a) - Treatment in the presence of a base

[0041] In step (a) of the process of the present invention, an aqueous slurry of lead-containing waste is treated with a hydroxide base. This results in the formation of a desulfurized lead-containing waste and an aqueous solution, wherein PbSO4 in the desulfurized lead-containing waste has been converted into PbO and sulfate ions have been extracted into the aqueous solution.

[0042] Step (a) is carried out at a pH in the range of 11 to 15. It has been found that by maintaining the pH in this range, PbSO4 can be selectively converted to PbO, which is the preferred form of lead for downstream treatment of desulfurized lead-containing waste. In particular, it has been found that if the pH drops below 11, a large amount of lead hydroxide and unconverted PbSO4 may be present in the desulfurized slurry. If the pH is above 15, a large amount of lead salts (i.e., containing PbO2) may be formed. 2- ions), such as cations with hydroxide bases; these salts are highly soluble in aqueous systems, resulting in lead losses.

[0043] The pH in step (a) may be maintained at at least 11.5, preferably at least 12, more preferably at least 12.5. The pH in step (a) may be maintained at a maximum of 14.5, preferably at a maximum of 14.25, more preferably at a maximum of 14. Thus, the pH may be maintained in the range of 11.5 to 14.5, preferably 12 to 14.25, more preferably 12.5 to 14 in step (a).

[0044] In particularly preferred cases, the pH in step (a) can be maintained above 13. For example, the pH can be maintained in the range of 13 to 14, for example by setting a target pH of 13.5 and allowing the pH value to fluctuate by ±0.5.

[0045] The pH is measured using conventional methods under the conditions used in step (a), for example: a pH probe. It will be appreciated that where step (a) is carried out in a mill (or other comminution equipment) - as described in more detail below - the pH probe will not typically be inserted into the grinding portion of the mill, but rather will be placed at a location where the pH measured is substantially the same as the pH of the grinding portion, such as in a chamber in fluid communication with the slurry, or where a classifier is used, preferably in the classifier (e.g., a classifier bath). By placing the pH probe away from the grinding portion, mechanical wear on the probe can be reduced.

[0046] The pH is preferably maintained by monitoring the pH during step (a) and, if necessary, further addition of hydroxide base to the slurry. This ensures that the pH of the aqueous slurry is within the target range at the end of the desulfurization step (a). The amount of base required to maintain a particular pH will of course vary depending on the source of the lead-containing waste and the course of the reaction, and can be readily determined by a person skilled in the art.

[0047] Various hydroxide bases can be used in step (a) of the present invention. Preferably, the base is selected from metal hydroxides, such as alkali metal hydroxides (such as NaOH, KOH or LiOH) and alkaline earth metal hydroxides. It is particularly preferred to use alkali metal hydroxides such as NaOH as the base.

[0048] As described above, by controlling the pH, thereby avoiding the formation of unwanted byproducts, near stoichiometric conversions can be achieved. The stoichiometry of the reaction with an alkali metal hydroxide (MOH, where M is, for example, Na or another alkali metal) is shown below:

[0049] PbSO4+2MOH→M2SO4+PbO+H2O

[0050] Therefore, the consumption of alkali in step (a) is at least 1.9 moles of alkali per mole of lead sulfate in the lead-containing waste, preferably at least 1.95 moles, more preferably at least 1.98 moles. The consumption of alkali in step (a) is at most 2.1 moles of alkali per mole of lead sulfate in the lead-containing waste, preferably at most 2.05 moles, more preferably at most 2.02 moles. Therefore, the consumption of alkali in step (a) is 1.9 to 2.1 moles of alkali per mole of lead sulfate in the lead-containing waste, preferably 1.95 to 2.05 moles, more preferably 1.98 to 2.02 moles. It should be understood that in the case of using alkaline earth metal hydroxide, the stoichiometry of the reaction changes, therefore, the consumption of alkali in step (a) is preferably half of the above. Any hydroxide alkali present but not used up during the reaction can be recycled for further use.

[0051] The solid content of the aqueous slurry in step (a) may be at least 30 wt %, preferably at least 50 wt %, more preferably at least 55 wt %. The solid content of the aqueous slurry may be up to 80 wt %, preferably up to 70 wt %, more preferably up to 65 wt %. Thus, the solid content of the aqueous slurry may be from 30 to 80 wt %, preferably from 50 to 70 wt %, more preferably from 55 to 65 wt %. Prior art methods typically use low solid contents, and the low water system used in the present invention is surprisingly effective.

[0052] As will be discussed in further detail below, the desulfurization process of the present invention may include a conditioning step in which water is added to the desulfurized lead-containing waste and the aqueous solution containing sulfate ions formed in step (a). In the absence of this step, i.e. the product of step (a) is directly separated in step (b), the aqueous slurry of the lead-containing waste preferably has a solids content of up to 35%, such as 25 wt% to 35 wt%, to ensure that the sulfate ions (e.g., in the form of a metal salt, such as Na2SO4 if the base is NaOH) generated during step (a) remain in solution.

[0053] Step (a) can be carried out at a temperature of at least 0°C, preferably at least 10°C, more preferably at least 20°C. Step (a) can be carried out at a temperature of up to 70°C, preferably up to 65°C, more preferably up to 60°C. Thus, step (a) can be carried out at a temperature of 0 to 70°C, preferably 10 to 65°C, more preferably 20 to 60°C. Typically, neither heating nor cooling is performed during step (a). However, it is preferred that the temperature is maintained at or below 60°C to avoid any undesirable dissolution of lead compounds. Since heat is typically generated during the desulfurization reaction, in some embodiments, for example if the PbSO4 concentration of the lead-containing waste is high, cooling may be performed during step (a) so that the temperature does not exceed 60°C.

[0054] Step (a) is generally carried out at ambient pressure, ie without application or removal of pressure.

[0055] Step (a) can be carried out for at least 10 minutes, preferably at least 20 minutes, more preferably at least 30 minutes. Step (a) is usually carried out for up to 3 hours, preferably up to 2 hours, more preferably up to 90 minutes. Therefore, step (a) can be carried out for 10 minutes to 3 hours, preferably 20 minutes to 2 hours, more preferably 30 minutes to 90 minutes. It should be understood that in the continuous desulfurization process, these values ​​represent the median average residence time in the system.

[0056] In a preferred embodiment, the lead-containing waste is crushed during step (a). It should be understood that the particle size of the lead-containing waste is reduced during the crushing process. Preferably, when crushed, the desulfurized lead-containing waste produced in step (a) is in the form of particles, wherein at least 80wt% (i.e., d80) of the particles by weight pass through a sieve with a mesh diameter of 150μm, preferably 75μm, and more preferably 63μm. Preferably, when crushed, the desulfurized lead-containing waste produced in step (a) is in the form of particles, wherein 100wt% (i.e., d100) of the particles by weight pass through a sieve with a mesh diameter of 250μm, preferably 125μm, and more preferably 75μm. Particles of this size can provide excellent desulfurization levels.

[0057] The lead-containing waste can be comminuted using a variety of methods, such as crushing, grinding or shattering. Preferably, the lead-containing waste is comminuted by grinding. The grinding can be carried out in a mill. Grinding media, such as balls or rods, are preferably used in the mill to improve the grinding process. Therefore, in a preferred embodiment, step (a) is carried out in a ball mill or a rod mill, preferably in a ball mill.

[0058] The preferred operating speed of the mill depends on a number of factors, including its size. Preferably, the ball mill is operated at a speed below 90% of the critical speed, more preferably at a speed of 60% to 85% of the critical speed of the mill (i.e., the speed at which the mill becomes a centrifuge). Since the critical speed is related to the diameter of the mill barrel, the preferred operating speed will depend on the scale of desulfurization. The mill can typically be operated at a speed of at least 5 rpm, preferably at least 10 rpm, more preferably at least 15 rpm. The mill can be operated at a speed of up to 60 rpm, preferably up to 40 rpm, more preferably up to 30 rpm. Therefore, the mill can be operated at a speed of 5 to 60 rpm, preferably 10 to 40 rpm, more preferably 15 to 30 rpm.

[0059] The mill can be operated in batch mode, but is preferably operated in continuous mode, i.e. leaded waste is fed into the mill and desulfurized leaded waste is continuously removed from the mill. This continuous grinding reduces pH fluctuations due to the addition of feed, which is usually acidic, and because there is a reservoir of material already at the correct pH in the mill. In addition, any temperature increase that may occur due to the grinding and desulfurization is eliminated.

[0060] In particularly preferred embodiments, the mill is operated as a closed circuit mill. This term is understood to mean a system in which the ground material is discharged to a classifier which returns any oversized material to the mill for further grinding. These embodiments are particularly preferred because they allow the continuous processing of different feedstocks with different and unknown sulfate contents by simply maintaining the pH level of the system.

[0061] Adjustment steps

[0062] The mixture of the aqueous solution containing sulfate ions and the lead-containing waste formed in step (a) can also be used directly in step (b). However, the method of the present invention usually includes a conditioning step between step (a) and step (b). The conditioning step is usually carried out in one or more conditioning tanks, but can also be carried out in a container, for example in a mill carrying out step (a).

[0063] The conditioning step may serve two purposes: to ensure that any sulfate ions are in solution; and / or to ensure that desulfurization is complete.

[0064] To ensure that any sulfate ions are in solution, the conditioning step may include a dilution step in which water is added to the aqueous solution containing sulfate ions and the desulfurized lead waste formed in step (a). This also has the advantage of lowering the pH of the system. The product of step (a) is typically mixed during the dilution step.

[0065] Water may be added to obtain a slurry having a solid content of up to 40 wt%, preferably up to 35 wt%, more preferably up to 30 wt%. Water may be added to obtain a slurry having a solid content of at least 15 wt%, preferably at least 20 wt%, more preferably at least 25 wt%. Thus, water may be added to obtain a slurry having a solid content of 15 to 40 wt%, preferably 20 to 35 wt%, more preferably 25 to 30 wt%.

[0066] To ensure that desulfurization is complete - for example if the particles are small enough to pass through the classifier in a closed circuit mill, but they are large particles from newly crushed particles with a high PbSO4 content - the conditioning step may include: leaving the desulfurized leaded waste formed in step (a) and the aqueous solution containing sulfate ions in a tank for a period of time. It should be understood that in the case of a closed circuit mill, the alkali is removed from the slurry with the classified particles so that the desulfurization can continue in the tank through which the classified particles have passed. The tank is preferably the conditioning tank in which the dilution step is performed, but it can also be the container in which step (a) is performed, or another conditioning tank. In these embodiments, where a dilution step is also performed, it should be understood that the product of step (a) is left in the tank for a period of time before dilution is performed.

[0067] The product of step (a) may remain in the tank for at least 1 minute, preferably at least 2 minutes, more preferably at least 5 minutes. This period of time may be up to 30 minutes, preferably up to 20 minutes, more preferably up to 15 minutes. Thus, this period of time may be from 1 to 30 minutes, preferably from 2 to 20 minutes, more preferably from 5 to 15 minutes.

[0068] Generally, it is not necessary to leave the product of step (a) in the tank for a period of time, especially when the desulfurized lead-containing waste produced in step (a) is in the form of particles and passes through a sieve with an opening below 100 μm.

[0069] Step (b) – Separation of desulfurized lead waste

[0070] The desulfurized lead waste can be separated from the aqueous solution containing sulfate ions by filtration, but various other methods can also be used, such as settling tanks or centrifugation.

[0071] Preferably, pressure filtration is used to separate the desulfurized lead-containing waste from the aqueous solution containing sulfate ions. During filtration, a pressure of at least 2 bar, preferably at least 4 bar, more preferably at least 5 bar can be applied. A pressure of up to 50 bar, preferably up to 20 bar, more preferably up to 10 bar can be applied. Therefore, a pressure of 2 to 50 bar, preferably 4 to 20 bar, more preferably 5 to 10 bar can be applied.

[0072] The slurry of desulfurized lead waste and aqueous solution containing sulfate ions is preferably filtered using a filter press through a filter cloth, for example with a pore size of at most 50 μm, preferably at most 30 μm, more preferably at most 20 μm. Other filtration methods include belt filter presses.

[0073] Step (b) may include washing the separated desulfurized lead-containing waste (whether separated by filtration or other means) with water to ensure that all sulfate ions have been removed. In some embodiments, the method includes monitoring the sulfate content of the used wash water to determine that the target level of sulfate has been reached. Monitoring can be carried out by directly measuring the sulfate content, but it is preferably carried out indirectly, such as by measuring the conductivity of the wash water. The target conductivity of the used wash water is at most 4000μS / cm greater than the conductivity of the wash water before contacting the separated desulfurized lead-containing waste, preferably at most 2000μS / cm, and more preferably at most 1000μS / cm. The conductivity of the wash water can be monitored using conventional methods, such as using a conductivity meter.

[0074] In some embodiments, the method may further include separating sulfate ions, such as by evaporating water from the filtrate (i.e., an aqueous solution containing sulfate ions) and crystallizing, and optionally using sulfate ions in another application. For example, the recovered sulfate can be used to produce glass. Washing water can be mixed with the filtrate for this treatment or other further treatment. However, the filtrate and wash water streams are usually kept separate to maintain a high concentration of sulfate ions in the filtrate.

[0075] The method of the present invention can be used to remove very high proportions of sulfate from lead-containing waste. Preferably, at least 95% of the sulfur load is removed from the lead-containing waste, preferably at least 98%, more preferably at least 99%. The reduction of sulfur can be measured using known methods, such as spectroscopic techniques, such as ICP-AES (inductively coupled plasma atomic emission spectroscopy). ICP-AES can be performed as detailed in the examples.

[0076] Therefore, the method can be used to produce a desulfurized leaded waste containing a very small amount of lead sulfate at the end of step (b). The desulfurized leaded waste obtained at the end of step (b) preferably contains less than 1wt% PbSO4, preferably less than 0.1wt%, more preferably less than 0.01wt%.

[0077] The desulfurized lead waste obtained at the end of step (b) preferably contains less than 1 wt% of lead hydroxide form, more preferably less than 0.5 wt%, and most preferably less than 0.1 wt%. Particularly preferred embodiments of the present invention can produce desulfurized lead waste that is substantially free of lead hydroxide in any form. It should be understood that the lead hydroxide form can include Pb(OH)2 and other hydroxide forms, such as Pb5O3(OH)4 and Pb3O2(OH)2.

[0078] The desulfurized lead-containing waste obtained at the end of step (b) preferably contains less than 2 wt% PbCO3, preferably less than 1 wt%, more preferably less than 0.5 wt%. Typically, the desulfurized lead-containing waste obtained at the end of step (b) contains no PbCO3.

[0079] The amount of PbSO4, lead hydroxide forms and PbCO3 can be determined using known methods, such as XRD (X-ray diffraction). XRD can be performed as detailed in the examples.

[0080] The desulfurized lead-containing waste obtained at the end of step (b) may contain at least 95% lead loading present in the lead-containing waste used in step (a), preferably at least 99%, more preferably at least 99.9%. Lead loading can be measured using known methods, such as spectroscopy techniques, such as ICP-AES (inductively coupled plasma atomic emission spectroscopy). In particular, the lead-containing waste can be dissolved in nitric acid (8 parts) and hydrogen peroxide (2 parts) at about 80°C while stirring for 30 minutes. Then ICP-AES can be used to measure the lead content in the solution. ICP-AES can be carried out as described in detail in the examples.

[0081] The desulfurized leaded waste obtained at the end of step (b) may contain at least 40wt% of PbO, preferably at least 50wt%, more preferably at least 60wt%. The weight proportion of PbO present in the desulfurized leaded waste can be measured using known methods, such as spectroscopy techniques, such as ICP-AES. In particular, the leaded waste can be dissolved in 5% aqueous acetic acid at room temperature while stirring for 1 minute. ICP-AES can then be used to measure the lead content in the solution. ICP-AES can be performed as described in detail in the examples.

[0082] The present invention provides a desulfurized lead-containing waste material that can be obtained using the method of the present invention. The present invention also provides a desulfurized lead-containing waste material, preferably a desulfurized lead-acid battery slurry, which can be obtained using the method of the present invention, comprising by weight:

[0083] PbO containing at least 40%;

[0084] PbO2 with a content of at least 10%;

[0085] Pb in an amount of at least 1%; and

[0086] Lead hydroxide containing less than 5%.

[0087] Further treatment of desulfurization waste

[0088] The desulfurized lead waste described herein can be further processed by a variety of different ways, preferably into lead-containing materials. Therefore, the present invention provides a method for recovering lead-containing waste, the method comprising:

[0089] (i) preparing desulphurised lead waste using the process as defined herein; and

[0090] (ii) further processing the desulfurized lead waste into lead-containing materials.

[0091] Step (i) can also be omitted and step (ii) carried out using the desulfurized lead-containing waste obtainable by the process of the invention.

[0092] In the first case, the desulfurized leaded waste can be further processed into lead ingots in a furnace (e.g., a smelting furnace). Since the desulfurized leaded waste contains very low levels of lead sulfate, the smelting furnace can be operated at a relatively low temperature. For example, the smelting furnace can be operated at a temperature of 800 to 1000°C. In addition, the low lead hydroxide content in the desulfurized leaded waste means that less energy is consumed to convert the lead hydroxide form into lead oxide in the smelting furnace and to treat the water produced in the conversion process. The substantial absence of carbonates (there is a carbonate desulfurization method) also means that CO2 is not produced in the smelting furnace. Due to the low content of PbSO4 in the desulfurized waste, it is also possible to avoid using iron, soda and silicon dioxide in the smelting furnace. Therefore, in some embodiments, the smelting furnace is operated in the absence of iron, soda and / or silicon dioxide.

[0093] In the second case, the desulfurized lead waste can be further processed by:

[0094] (a) treating the waste with an aqueous solution of citric acid to produce lead citrate;

[0095] (b) separating the lead citrate from the aqueous solution; and

[0096] (c) converting the separated lead citrate into Pb and / or PbO.

[0097] In the second case, further processing may be performed as described in WO 2008 / 056125.

[0098] In the third preferred case, the desulfurized lead waste can be further processed by:

[0099] (a) dissolving the lead-containing waste in an aqueous solution of a first acid to form a solution of a first lead salt;

[0100] (b) adding a second acid to the solution of the first lead salt to form a lead-depleted solution and a precipitate of the second lead salt; and

[0101] (c) converting the precipitate of the second lead salt into a lead-containing oxide,

[0102] The solubility of the first lead salt in water is higher than that of the second lead salt.

[0103] In the first step (a) of the third further treatment method, the lead-containing waste is dissolved in an aqueous solution of a first acid to form a solution of a first lead salt.

[0104] It should be understood that the first lead salt has a lead cation and an anion from the first acid. In a preferred embodiment, the first lead salt is a lead (II) salt. The solubility of the first lead salt in water is preferably at least 100 g / L, preferably at least 200 g / L, more preferably at least 300 g / L. The solubility mentioned herein refers to the equilibrium solubility in water at 25°C.

[0105] The first acid is preferably a Bronsted-Lowry acid, i.e. a proton donor. The first acid may be an organic acid or an inorganic acid, however the preferred first acid is an organic acid. A particularly suitable organic acid is acetic acid, which forms a solution of lead acetate Pb(CH3COO)2. Other organic acids that may be used include carboxylic acids, such as maleic acid, lactic acid and acrylic acid. Suitable inorganic acids include nitric acid.

[0106] The aqueous solution of the first acid preferably has a molar concentration of at least 0.1 mol / L, preferably at least 0.25 mol / L, more preferably at least 0.5 mol / L. The aqueous solution of the first acid preferably has a molar concentration of at most 7 mol / L, preferably at most 3 mol / L, more preferably at most 1.5 mol / L. Therefore, the molar concentration of the acidic aqueous solution of the first acid may be 0.1 to 7 mol / L, preferably 0.25 to 3 mol / L, more preferably 0.5 to 1.5 mol / L.

[0107] The leaded waste is preferably added to the first acid aqueous solution in an amount of at least 10 g of leaded waste per liter of acid aqueous solution, preferably at least 50 g, more preferably at least 80 g. The leaded waste can be added to the first acid aqueous solution in an amount of up to 650 g of leaded waste per liter of acid aqueous solution, preferably up to 300 g, more preferably up to 150 g. Therefore, the leaded waste can be added to the first acid aqueous solution in an amount of 10 to 650 g of leaded waste per liter of acid aqueous solution, preferably 50 to 300 g, more preferably 80 to 150 g.

[0108] The lead-containing waste can be dissolved in the aqueous solution of the first acid at a temperature of at least 0° C., preferably at least 10° C., more preferably at least 15° C. The lead-containing waste can be dissolved in the aqueous solution of the first acid at a temperature of up to 90° C., preferably up to 50° C., more preferably up to 30° C. Therefore, the lead-containing waste can be dissolved in the aqueous solution of the first acid at a temperature of 0 to 90° C., preferably 10 to 50° C., more preferably 15 to 30° C.

[0109] It will be appreciated that higher temperatures and higher concentrations of first acid are typically used in the dissolution step (a) where larger amounts of lead-containing waste are used.

[0110] The lead-containing waste is typically dissolved in an aqueous solution of the first acid at ambient pressure, ie without applying or removing pressure.

[0111] The lead-containing waste may be dissolved in the aqueous solution of the first acid for 1 to 120 minutes, preferably 5 to 60 minutes, and more preferably 15 to 45 minutes.

[0112] In some embodiments, it may be desirable to contact the lead-containing waste with a redox agent. Dissolution of the lead-containing material is aided by converting a material that is not in the +2 oxidation state to the +2 oxidation state. For example, a redox agent can convert a lead-containing material such as PbO2 in the +4 oxidation state to PbO, which then readily reacts with an aqueous solution of a first acid to form a soluble salt. Without the use of a redox agent, the conversion of PbO2 to a salt is typically quite slow. A redox agent can also assist in the conversion of metallic lead to PbO, although Pb can also form a salt with the first acid without contact with a redox agent.

[0113] Preferably, the redox reagent is a reducing agent, for example for lead compounds in the +4 oxidation state. Preferably, the redox reagent is also an oxidizing agent, for example for metallic lead. Particularly preferred redox reagents include hydrogen peroxide, which acts as both an oxidizing agent and a reducing agent. However, other redox reagents may also be used. For example, metal hydrides, hydrogen or inorganic salts may be used as reducing agents. Organic redox reagents may also be used.

[0114] The redox reagent may be brought into contact with the lead-containing waste before or during step (a) of the recovery method. When the redox reagent is brought into contact with the lead-containing waste in step (a), the redox reagent may be introduced into the aqueous solution of the first acid before the lead-containing waste dissolves, or the redox reagent may be introduced immediately when the lead-containing waste has partially dissolved.

[0115] The redox reagent can be used in the form of a solution having a molar concentration of at least 1 mol / L, preferably at least 3 mol / L, more preferably at least 5 mol / L. The redox reagent can be used in the form of a solution having a molar concentration of up to 25 mol / L, preferably up to 20 mol / L, more preferably up to 15 mol / L. Therefore, the redox reagent can be used in the form of a solution having a molar concentration of 1 to 25 mol / L, preferably 3 to 20 mol / L, more preferably 5 to 15 mol / L.

[0116] The redox reagent solution may be added to the aqueous solution of the first acid in an amount of at least 1 ml of the redox reagent solution per liter of the aqueous solution of the acid, preferably at least 5 ml, more preferably at least 10 ml. The redox reagent solution may be added to the aqueous solution of the first acid in an amount of up to 100 ml of the redox reagent solution per liter of the aqueous solution of the acid, preferably up to 50 ml, more preferably up to 30 ml. Thus, the redox reagent solution may be added to the aqueous solution of the first acid in an amount of 1 to 100 ml of the redox reagent solution per liter of the aqueous solution of the acid, preferably 5 to 50 ml, more preferably 10 to 30 ml.

[0117] In some embodiments, the lead-containing waste used in step (a) may contain materials that are insoluble in the aqueous solution of the first acid and thus the materials remain as insoluble materials in the solution of the first lead salt. The insoluble materials may be present in the lead-containing waste in an amount of at least 0.01 wt%, more typically at least 0.1 wt%, and even more typically at least 1 wt%. For example, lead-acid battery slurry typically contains 2 to 5% insoluble materials, more typically 3 to 3.5 wt%.

[0118] Insoluble materials can include one or more metal compounds such as barium sulfate, carbon such as carbon black, graphene and / or carbon nanotubes, and fibers such as lignin sulfonates. In some embodiments, the insoluble material includes metal compounds, carbon and fibers. The insoluble material can also include polymers or glass. The insoluble material may also contain some lead, although this is generally less preferred. For example, the insoluble material may contain Pb, for example if it is present in a relatively large particle size or has a short dissolution time.

[0119] When the lead-containing waste contains insoluble materials, these materials are preferably recovered from the solution formed in step (a). By dissolving the lead-containing waste in the aqueous solution of the first acid, an opportunity is provided to remove insoluble components which represent impurities in the lead oxide but are valuable in their separated form. In some embodiments, the recovered insoluble materials are reused.

[0120] Suitable methods for recovering insoluble material from the solution of the first lead salt formed in step (a) include filtration, but a variety of other methods may be used, such as settling tanks or centrifugation.

[0121] In the second step (b) of the third further treatment method, a second lead salt is precipitated by adding a second acid to a solution of the first lead salt. This results in the formation of a lead-poor solution and precipitation of the second lead salt.

[0122] It should be understood that the second lead salt has a lead cation, while the anion comes from the second acid. In a preferred embodiment, the second lead salt is a lead (II) salt. The solubility of the second lead salt in water is lower than that of the first lead salt, for example, at least 100 g / L lower, preferably at least 200 g / L lower, more preferably at least 400 g / L lower. The solubility of the second lead salt in water is preferably at most 10 g / L, preferably at most 1 g / L, more preferably at most 0.1 g / L.

[0123] As with the first acid, the second acid is preferably a Bronsted-Lowry acid, i.e., the second acid is a proton donor. The second acid may be an organic acid or an inorganic acid, however, the preferred second acid is an organic acid. Particularly preferred is citric acid, which forms a lead citrate precipitate. Since the solubility of lead citrate in aqueous conditions is very low, the "loss" of citrate remaining in the solution is minimal.

[0124] The lead citrate precipitate is typically present as a compound having the formula Pb3(C6H5O7)2. Some lead citrate may also be present in its unstable Pb(C6H8O7) form, for example if an excess of citric acid is present, although the lead citrate precipitate typically consists of Pb3(C6H5O7)2. Advantageously, trilead citrate requires lower amounts of citric acid to form than monolead citrate. The lead citrate precipitate may be in a hydrated form, typically Pb3(C6H5O7)2xH2O, where x may be from 1 to 3.

[0125] The second acid is preferably added to the solution of the first lead salt in a stoichiometric amount at most to form the second lead salt from the lead ions in the solution of the first lead salt. By using a stoichiometric amount or slightly less than the stoichiometric amount of the second acid, it is ensured that the second acid is completely converted into the second lead salt.

[0126] The second acid may be added to the solution of the first lead salt in an amount of up to 100% of the stoichiometric amount required to form the second lead salt, preferably up to 98%, preferably up to 95%. The second acid may be added to the solution of the first lead salt in an amount of at least 60% of the stoichiometric amount required to form the second lead salt, preferably at least 75%, more preferably at least 80%. Thus, the second acid may be added to the solution of the first lead salt in an amount of 60 to 100% of the stoichiometric amount required to form the second lead salt, preferably 75 to 98%, more preferably 80 to 95%.

[0127] The amount of lead ions present in the solution of the first lead salt can be measured using known techniques. The amount of lead ions can be measured directly (e.g., using a lead ion sensor) or indirectly. The amount of the second acid required can then be calculated based on the measured amount of lead ions.

[0128] It should be understood that the stoichiometric amount of citric acid used to convert the lead ions in the solution of the first lead salt into Pb3(C6H5O7)2 is 0.67 moles of citric acid per mole of lead ions. This is demonstrated by the following equation, where lead acetate is converted into lead citrate:

[0129] 3Pb(CH3COO)2+2C6H8O7→Pb3(C6H5O7)2+6CH3COOH

[0130] Therefore, citric acid can be added to the solution of the first lead salt in an amount of at most 0.67 moles of citric acid per mole of lead ions in the solution, preferably at most 0.65 moles, more preferably at most 0.63 moles. Citric acid can be added to the solution of the first lead salt in an amount of at least 0.40 moles of citric acid per mole of lead ions in the solution, preferably at least 0.50 moles, more preferably at least 0.55 moles. Therefore, the amount of citric acid added can be 0.40 to 0.67 moles of citric acid per mole of lead ions in the solution of the first lead salt, preferably 0.50 to 0.65 moles, more preferably 0.55 to 0.63 moles.

[0131] The second acid may be added to the solution of the first lead salt in powder form or as an aqueous solution.

[0132] The precipitation of the second lead salt may occur at a temperature of at least -10°C, preferably at least 0°C, more preferably at least 5°C. The precipitation of the second lead salt may occur at a temperature of up to 80°C, preferably up to 40°C, more preferably up to 30°C. Thus, the precipitation of the second lead salt may occur at a temperature of -10 to 80°C, preferably 0 to 40°C, more preferably 5 to 30°C.

[0133] The second lead salt is typically precipitated from a solution of the first lead salt at ambient pressure (ie, without applied or removed pressure).

[0134] The precipitation of the second lead salt may be carried out for 2 to 120 minutes, preferably 5 to 60 minutes, more preferably 10 to 45 minutes.

[0135] The precipitate of the second lead salt is preferably separated from the lean lead solution before conversion to lead-containing oxide. This enables water-soluble impurities present in the lead-containing waste to be removed as part of the lean lead solution. Suitable methods for separating the second lead salt precipitate from the lean lead solution include filtration, but a variety of other methods, such as settling tanks or centrifugation, may also be used. Smaller mesh sizes are generally preferred to ensure that all of the second lead salt precipitate is captured. However, in some embodiments, the size of the second lead salt precipitate means that a larger mesh size may be appropriate.

[0136] The separated second lead salt can be washed, for example, with water to remove any water-soluble impurities from the precipitate.

[0137] The second lead salt may also be purified. Suitable purification methods include recrystallization. However, purification is usually not required to provide a highly pure second lead salt.

[0138] The poor lead solution is included in the first acid for dissolving the lead-containing waste in step (a). Although the acid forms a relatively soluble first lead salt in step (a), the first lead salt can be converted into a second lead salt in step (b). In a preferred embodiment, the poor lead solution is recovered and used as an aqueous solution of the first acid for dissolving the lead-containing waste in step (a). By reclaiming the poor lead solution, the first acid is not consumed but can be reused. Therefore, in the recovery process, the first acid can be regarded as a catalyst rather than a reagent.

[0139] The lead-depleted solution may also contain residual lead, preferably in the form of a dissolved first lead salt. This is particularly true when the second acid is used in less than a stoichiometric amount in step (b) (compared to the lead ions in the solution of the first lead salt). Recovering the residual lead as part of the lead-depleted solution ensures that no lead is lost in the third further processing method.

[0140] In the third step (c) of the third further treatment method, the precipitate of the second lead salt is converted into lead-containing oxides. The lead-containing oxides include PbO and usually also include some metallic lead.

[0141] Preferably, the precipitate of the second lead salt is converted to the lead-containing oxide by calcination. This involves introducing the second lead salt precipitate into a calciner and heating it to a temperature at which the salt decomposes and / or burns to produce the lead-containing oxide. Advantageously, where the second lead salt is lead citrate, the citrate acts as a fuel and burns during calcination, thereby reducing the energy required.

[0142] Calcination can be carried out at a temperature of at least 250°C, preferably at least 300°C, more preferably at least 325°C. Calcination can be carried out at a temperature of up to 1000°C, preferably up to 600°C, more preferably up to 450°C. Thus, calcination can be carried out at a temperature of 250 to 1000°C, preferably 300 to 600°C, more preferably 325 to 450°C. These temperatures are particularly suitable for the calcination of lead citrate precipitates. These temperatures generally provide lead-containing oxides comprising a mixture of PbO and Pb, with lower temperatures generally used to prepare lead-containing oxides that do not contain Pb.

[0143] Calcination can be carried out in an atmosphere comprising oxygen. It is understood that higher amounts of oxygen generally favor the formation of PbO, while low oxygen environments generally favor the formation of metallic lead.

[0144] Calcination can be carried out at an oxygen partial pressure of at least 0.01 atm, preferably at least 0.05 atm, more preferably at least 0.1 atm. Calcination can be carried out at an oxygen partial pressure of up to 5 atm, preferably up to 1 atm, more preferably up to 0.5 atm. Thus, calcination can be carried out at an oxygen partial pressure of 0.01 to 5 atm, preferably 0.05 to 1 atm, more preferably 0.1 to 0.5 atm. For example, calcination can be carried out in air at atmospheric pressure, i.e. without applying or removing pressure.

[0145] Calcination may be performed for 10 minutes to 6 hours, preferably 20 minutes to 2 hours, more preferably 30 minutes to 1 hour.

[0146] An advantage of the third further processing method is that the method is suitable for preparing very high purity leaded oxide. Therefore, the leaded oxide preferably contains a total amount of at least 99wt% PbO and Pb, preferably at least 99.5wt%, more preferably at least 99.9wt%. Leaded oxides with these purities are comparable to those obtained using the Barton jar method or ball milling method (in which the lead ingots are oxidized). Purity can be measured using known methods, such as spectroscopic techniques, such as ICP-AES (inductively coupled plasma atomic emission spectroscopy). ICP-AES can be performed as described in detail in the examples.

[0147] In some cases, metallic lead Pb rather than lead oxides may be the desired product, in which case temperatures in excess of 1000° C. are preferably used in step (c) of the third further treatment method. Reducing agents such as carbon monoxide or coke may also be used, in which case temperatures below 1000° C. (e.g. 400 to 600° C.) may also be used. Preferably, the partial pressure of oxygen in the system will be limited, for example to at most 0.000167 atm. Inert gases such as nitrogen or vacuum may be used to displace oxygen from the reaction environment.

[0148] In other cases, lead citrate may be the desired product, in which case the third further processing method does not include step (c).

[0149] Example

[0150] The invention will now be illustrated by the following non-limiting examples.

[0151] In the examples, X-ray diffraction was performed on a D8 Advance Bruker diffractometer and analyzed using Highscore software. The following settings were used: Cu Ka radiation, Ni-0.012 filter; run at 40 kV and 40 mA; range: 5 to 90° 2θ; step size: 0.03°; scan rate: 3.5° min-1.

[0152] Thermogravimetric analysis and differential scanning calorimetry experiments were performed using a STA 409EP Netzsch apparatus. The following settings were used: in static air (chamber approximately 0.15 L); sample size: 20 to 30 mg; temperature range: 0 to 600°C; heating rate: 5°C / min.

[0153] Inductively coupled plasma atomic emission spectroscopy (ICP-AES) was performed using a Perkin Elmer Optima 8000 ICP-OES. The following settings were used: gas: argon; plasma gas flow: 8 L / min; auxiliary gas flow: 0.2 L / min; nebulizer gas flow: 0.7 L / min; RF power: 1500 Watts.

[0154] Solid samples (usually 0.10 g to 0.50 g of powder) analyzed using ICP-AES are treated differently to suit the specific composition of each sample so that it is completely dissolved in an aqueous medium. Each treatment involves combining 1, 2 or 3 different solutions in a specific order. The solutions used are 70 wt% nitric acid, 30 wt% hydrogen peroxide and 1 M potassium hydroxide (all 99.9% pure). The preparation is then completed by mixing 100 ml of nitric acid of the selected concentration so that the concentration in the final solution nitric acid reaches 2 wt%.

[0155] The standard solutions were originally purchased from Sigma, but considering the matrix effects, standard solutions were subsequently prepared using ultrapure elements from Sigma, deionized water, and pure nitric acid.

[0156] Example 1: Desulfurization of waste battery slurry at different pH values

[0157] The waste lead-acid battery slurry is obtained from waste traction sealed lead-acid batteries. The slurry contains about 65 to 70 wt% PbSO4.

[0158] Desulfurization

[0159] Samples of waste lead-acid battery slurry (30.00 g) were added to aqueous sodium hydroxide solutions (different concentrations) to form aqueous slurries with a solid content of about 33 wt%. The pH level was maintained during the experiment and the experiment was terminated once the pH was stable without the addition of sodium hydroxide.

[0160] Separation

[0161] The desulfurized lead waste was separated from the aqueous solution by filtration and analyzed to determine their sulfate concentration.

[0162] result

[0163] The experimental results are shown in the following table:

[0164]

[0165] ( 1 Less than experiment B)

[0166] Example 2: Industrial scale desulfurization

[0167] Desulfurization is carried out on an industrial scale in lead waste treatment facilities, and very high levels of desulfurization are achieved.

[0168] Specifically, a lead-containing waste slurry (obtained from waste batteries) was passed through a closed-circuit ball mill. The classifier on the ball mill was set to recycle particles that did not pass through a sieve with a mesh diameter of 75 μm back into the ball mill for further grinding. Sodium hydroxide was added to maintain the pH level measured in the classifier bath, about 13.5.

[0169] The desulfurized waste is conditioned by adding water and then passing through a filter press at a pressure of 5 to 10 bar. The remaining solids are washed with water until the conductivity of the used wash water is no more than 1000 μS / cm greater than before washing.

[0170] The content of lead sulfate in the desulfurized lead-containing waste is less than 1wt%, and the content of lead hydroxide is negligible.

[0171] Example 3: Further treatment of desulfurized waste battery slurry (third method)

[0172] Dissolve

[0173] The desulfurized lead-acid battery slurry (10.00 g) was dissolved in a solution of glacial acetic acid (5.2 ml) in water (100 ml), and then H2O2 (2.0 ml, 30 wt%) was added. The dissolution of most of the solids could be directly observed within a few tens of seconds, producing a clear colorless solution with a small amount of insoluble material suspended in the liquid phase. The mixture was stirred at 500 rpm for 5 minutes at room temperature.

[0174] The clear, colorless solution was then filtered. The filtrate (3.4 wt% of the slurry) was analyzed and showed mainly BaSO4, carbon and fibers.

[0175] Lead citrate precipitation

[0176] Solid crystals of citric acid (5.17 g) were added to the filtrate from the dissolution step. Precipitation of white lead citrate started immediately, but the solution was allowed to react for 1 hour at 80°C with stirring at 400 rpm. The solution was then filtered, the filtrate (lead citrate) recovered, dried and weighed. The mass obtained was 13.12 g, very close to the expected 13.32 g. X-ray diffraction was used to confirm that the powder obtained was entirely Pb3(C6H5O7)2; thermogravimetric analysis of pure Pb3(C6H5O7)2 and the synthesized powder showed a perfect match. ICP-AES analysis of the powder showed a complete absence of S, Ba, Sn, Al, Fe, Zn and Sb (0%); the Cu content was of the order of 10 ppm; and the Na content was of the order of 500 ppm.

[0177] Using a more severe washing regimen, the Na content was reduced to below 100 ppm, demonstrating that the Na content in the above examples is related to water quality and washing efficiency.

[0178] Calcination of lead citrate

[0179] Lead citrate (10.00 g) was heated in a muffle furnace at 350°C in air for 1 hour and then cooled to room temperature. The resulting orange / yellow / green powder (lead monoxide) was then recovered and analyzed. The expected mass of Pb3(C6H5O7)2 burned to PbO was 6.70 g. The actual mass of the material obtained by this process was 6.18 g; this is because some of the PbO was reduced to lead metal (Pb) during the calcination combustion process. Differential scanning calorimetry confirmed the presence of Pb.

[0180] The powder was analyzed by XRD to confirm that the phase obtained was PbO. ICP-AES was used to confirm the high purity of the material, comparable to the purity levels of lead citrate described above.

[0181] Example 4: Further treatment of the negative grid of desulfurized waste batteries (third method)

[0182] Dissolve

[0183] The desulfurized waste battery negative electrode grid (50.00 g) was dissolved in an acetic acid aqueous solution (400 ml, 8 wt%) and stirred at 400 rpm for 10 minutes. Since the grid was a negative electrode plate and did not contain any PbO2, no H2O2 was added. The solid volume in the suspension was significantly reduced due to dissolution.

[0184] The solution was then filtered and the filtrate was analyzed to be mainly BaSO4, carbon, fibers and metallic Pb fragments from the grid, accounting for 7 wt% of the total mass of the slurry.

[0185] A portion of the solution was evaporated to crystallize the material expected to be lead acetate. The XRD pattern of the crystals showed a perfect match with pure lead acetate trihydrate, and thermogravimetric analysis of the crystals showed a similar decomposition pattern, confirming that the resulting solution was indeed a lead acetate solution.

[0186] Lead citrate precipitation

[0187] A citric acid solution (10 ml, 50 wt%) was added to the filtrate (200 ml) and stirred at room temperature for 10 minutes. A white solid precipitate was immediately observed. The precipitate was then filtered off, dried and weighed. The mass obtained was 12.76 g, close to the expected 12.88 g, corresponding to the maximum amount of lead citrate that can be formed with the amount of citric acid used.

[0188] XRD and thermogravimetric analysis showed a perfect match with Pb3(C6H5O7)2.

[0189] Combustion of lead citrate

[0190] The precipitate was burned in a muffle furnace at 400 °C in air for 1 h and analyzed under XRD. The color change from pure white to bright orange indicated the formation of PbO, which was confirmed by XRD analysis. The only other phase that could be detected was metallic Pb.

[0191] Example 5: Further treatment of electric arc furnace dust (third method)

[0192] A sample of steel industry dust was obtained. The sample had previously been subjected to conventional zinc recovery processing and contained approximately 60 to 70 wt% PbSO4. The sample was desulfurized using NaOH and then converted to lead citrate and calcined.

[0193] Preliminary recovery experiments on the sample indicated that the process of desulfurization and conversion to lead citrate was slow. Further analysis of the sample indicated that C and SiO2 were present in an amount of about 20 to 30 wt%, which is believed to be coated on the sample particles.

[0194] Samples of the as-received material were preheated to 500 and 600°C to determine the optimal pretreatment temperature required to eliminate carbon. The samples were heated at a rate of 5°C per minute and the temperature was maintained at 500 or 600°C for 1 hour. Although the amount of carbon was reduced in both samples, the sample treated at 600°C showed a more significant reduction in carbon than the sample treated at 500°C.

[0195] The pretreated samples were desulfurized with NaOH, converted to lead citrate, and then calcined in air at 450°C to obtain lead oxide. The lead oxide product contained PbO and metallic Pb, with the highest purity coming from the sample pretreated at 600°C.

Claims

1. A method for desulfurizing lead-containing waste, wherein the lead-containing waste contains PbSO4, the method comprising: (a) treating an aqueous slurry of the lead-containing waste with a hydroxide base, thereby forming a desulfurized lead-containing waste in which PbSO4 has been converted to PbO and an aqueous solution comprising sulfate anions; and (b) separating the desulfurized lead-containing waste from the aqueous solution containing sulfate anions, wherein the pH is maintained in the range of 11 to 15 during step (a) by adding further hydroxide base to the aqueous slurry; The desulfurized lead-containing waste obtained at the end of step (b) contains less than 1% by weight of lead hydroxide.

2. The method according to claim 1, wherein the lead-containing waste contains at least one of Pb, PbO and PbO2.

3. The method according to claim 1 or 2, wherein the lead-containing waste is derived from lead-acid battery slurry or electric arc furnace dust.

4. The method according to claim 1 or 2, wherein the lead-containing waste used in step (a) is in the form of particles, wherein at least 100% by weight of the particles pass through a sieve having a mesh diameter of 1 cm.

5. The method according to claim 1 or 2, wherein in step (a) the pH is maintained in the range of 11.5 to 14.

5.

6. The method according to claim 1 or 2, wherein the hydroxide base is selected from metal hydroxide bases.

7. The method according to claim 1 or 2, wherein the consumption of the hydroxide base in step (a) is: 1.9 to 2.1 moles of the hydroxide base per mole of lead sulfate in the lead-containing waste.

8. The process according to claim 1 or 2, wherein the solids content of the aqueous slurry in step (a) is 30 to 80% by weight.

9. The method according to claim 1 or 2, wherein step (a) is carried out at a temperature of 0 to 70°C.

10. The method according to claim 1 or 2, wherein the lead-containing waste is pulverized during step (a).

11. The method of claim 10, wherein step (a) is performed in a mill.

12. The method of claim 11, wherein the mill is operated at a speed of 5 to 60 rpm.

13. The method of claim 11, wherein the mill is operated to: Continuous mode; and / or Closed circuit mill.

14. The method according to claim 10, wherein the desulfurized lead-containing waste produced in step (a) is in the form of particles, wherein at least 80% by weight of the particles pass through a sieve having a mesh diameter of 150 μm.

15. The method according to claim 1 or 2, wherein an adjustment step is performed between steps (a) and (b), the adjustment step comprising: leaving the desulfurized lead-containing waste and the aqueous solution containing sulfate anions formed in step (a) in a tank for a period of time; and / or A certain amount of water is then added to the desulfurized lead-containing waste and the aqueous solution containing sulfate anions formed in step (a).

16. The method according to claim 1 or 2, wherein the desulfurized lead-containing waste is separated from the aqueous solution containing sulfate anions using filtration.

17. The method of claim 16, wherein step (b) comprises washing the desulfurized lead-containing waste with water.

18. The method of claim 17, wherein step (b) comprises monitoring the sulfate content of the spent wash water to determine that the target level of sulfate is achieved.

19. The method of claim 18, wherein monitoring comprises: The conductivity of the used wash water was measured.

20. The method according to claim 1 or 2, wherein: removing at least 95% of the sulfur load from the lead-containing waste; and / or At least 95% of the lead loading present in the lead-containing waste used in step (a) is retained.

21. The process according to claim 1 or 2, wherein the desulfurized lead-containing waste obtained at the end of step (b) comprises by weight: PbSO4 with a content of less than 1%; Less than 2% PbCO3; and / or The content is at least 40% PbO.

22. A desulfurized lead-containing waste obtained by the method according to any one of claims 1 to 21.

23. A desulfurized lead waste obtained by the method according to any one of claims 1 to 21, comprising by weight: A content of at least 40% PbO; A content of at least 10% PbO2; and The content is at least 1% Pb.

24. A method for recycling lead-containing waste, the method comprising processing desulfurized lead-containing waste into lead-containing material, wherein the desulfurized lead-containing waste is as defined in claim 22 or 23.

25. The method according to claim 24, wherein the desulfurized lead-containing waste: It is further processed in a furnace to produce lead ingots; Or further processing by following the steps below: (a) treating the waste with aqueous citric acid to produce lead citrate, (b) separating lead citrate from the aqueous solution, and (c) converting the separated lead citrate into Pb and / or PbO; Or further processing by following the steps below: (a) dissolving the lead-containing waste in an aqueous solution of a first acid to form a first lead salt solution; (b) adding a second acid to the solution of the first lead salt to form a lead-depleted solution and a precipitate of the second lead salt; and (c) converting the precipitate of the second lead salt into a lead-containing oxide, The solubility of the first lead salt in water is higher than that of the second lead salt.

Citation Information

Patent Citations

  • Lead recycling

    WO2008056125A1

  • Method for preparing nano-lead dioxide powder from waste lead paste by wet process

    CN103305695A

  • Method for recycling lead oxide-containing waste

    CN104619645A

  • Method used for direct recovery of lead oxide used for lead-acid cell anodes from waste lead paste

    CN104868187A

  • Method for wet recovery of high-purity lead oxide from waste lead paste of lead-acid storage batteries