Ozone oxidation catalyst and its preparation method and application

By combining modified γ-activated alumina support with copper nitrate and lanthanum nitrate, combined with a co-dispersant and a co-binding agent, an efficient ozone oxidation catalyst was prepared, which solved the poor complex wastewater treatment capacity and COD removal efficiency in the prior art. The problem of low results in more efficient sewage treatment and cost reduction.

CN115138367BActive Publication Date: 2024-11-26PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110343677.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-11-26
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Existing ozone oxidation catalysts have poor capabilities when treating complex wastewater and have low COD removal efficiency.

Method used

Modified γ-activated alumina as a support, copper nitrate and lanthanum nitrate are mixed with co-dispersant β-cyclodextrin and co-binding agent ammonia by impregnation to form a catalyst precursor, and dried and calcined to prepare Ozone oxidation catalyst containing copper oxide and lanthanum oxide.

Benefits of technology

The catalytic activity and stability of the catalyst are improved, the treatment capacity of complex wastewater is enhanced, the COD removal rate is improved, and the preparation cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003000097740000061
    Figure BDA0003000097740000061
Patent Text Reader

Abstract

The present invention provides an ozone oxidation catalyst and a preparation method and application thereof. The preparation method comprises the following steps: S1, mixing copper nitrate, lanthanum nitrate, a dispersant and a binder to obtain an impregnation solution; S2, immersing a modified γ-activated alumina carrier in the impregnation solution to obtain a catalyst precursor; S3, drying and calcining the catalyst precursor to obtain an ozone oxidation catalyst. Among them, the dispersant is a mixed solution of β-cyclodextrin and ethanol, and the binder is ammonia water. The present invention prepares an ozone oxidation catalyst by an impregnation method, using modified γ-activated alumina as a carrier, copper oxide and lanthanum oxide as active components, and by introducing an ethanol mixture of a dispersant β-cyclodextrin and a binder ammonia water, the synergistic effect promotes the catalytic activity and stability of the ozone oxidation catalyst to be better, and when it is subsequently applied to the oxidation of sewage after biochemical treatment, the ability to treat complex sewage is better and the COD removal rate is higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalysts, and in particular to an ozone oxidation catalyst and a preparation method and application thereof. Background Art

[0002] Chemical wastewater is a combination of multiple chemical wastewaters. Due to the diversity of its sources, its water quality is complex and has many characteristic pollutants. Furthermore, the organic matter and organic fragments remaining in the effluent after biochemical reaction treatment are even more complex. In order to achieve the final discharge of the sewage plant effluent in compliance with the standards, the biochemical effluent needs to be deeply treated.

[0003] Ozone is an allotrope of oxygen. Its redox potential is 2.07V under standard conditions. It is an extremely strong oxidant and is widely used in the fields of domestic sewage treatment and industrial sewage treatment. In order to overcome the problems of selective oxidation, large ozone consumption and high energy consumption of single ozone oxidation technology, a catalyst is introduced into the reaction system. Under the action of the catalyst, the efficiency of ozone oxidation can be greatly improved, the amount of ozone used can be reduced, and the catalytic ozone oxidation reaction is non-selective. Therefore, ozone catalytic oxidation technology has become an important chemical comprehensive sewage deep treatment technology. In the ozone catalytic oxidation of sewage treatment, traditional homogeneous catalysts have the problems of catalyst cannot be recovered, secondary pollution is introduced, and the treatment cost is high. The reaction system of heterogeneous catalytic ozone oxidation technology has three phases: solid, liquid and gas. The catalyst is solid, and the reactants and products are liquid or gaseous, which is convenient for the separation and reuse of the catalyst, and does not cause secondary pollution of the effluent, becoming the mainstream technology of sewage deep treatment technology.

[0004] Invention patent CN106964333A discloses a rare earth-loaded catalyst for treating sewage, its preparation method and application, and a method for treating sewage by ozone catalytic oxidation, wherein the carrier is activated carbon, and the active components are lanthanum oxide and gadolinium oxide. Invention patent CN107008449A discloses a method for preparing a solid catalyst for heterogeneous oxidation of ozone. The catalyst is used for heterogeneous reactions, and the carrier is a porous material such as erionite, garnet, medical stone, wollastonite, potassium feldspar and boraxite. The auxiliary agent is an organic salt containing scandium, yttrium, lanthanum and lutetium, and the active components are elements such as titanium, vanadium and osmium. Invention patent CN107758971A discloses a domestic sewage treatment process based on magnetic particle photocatalyst. The catalyst composition includes magnetic nanoparticles, titanium dioxide, graphene, aluminum oxide, and carboxymethyl-β-cyclodextrin. Invention patent CN108499574A discloses a catalyst for catalytic ozone oxidation of low-concentration volatile organic compounds, the catalyst MnO x -CeO x -LaO x -CuO xAluminum oxide, manganese nitrate, cerium nitrate, lanthanum nitrate and copper nitrate are the main raw materials. The catalyst is used in the field of ozone catalytic oxidation treatment of low-concentration volatile organic compounds, belonging to the field of gas purification. Invention patent CN103586026A discloses a carbon-supported catalyst for ozone oxidation, its preparation method and its use. The catalyst is composed of activated carbon-supported iron, copper, nickel or manganese transition metal active components and cerium, lanthanum or potassium co-catalysts. The active component is 0.5% to 10.0%, the co-catalyst is 0.00% to 0.50%, and the remainder is a carrier. The catalyst is a general ozone catalyst for water treatment, and the carrier is modified activated carbon.

[0005] The above existing ozone heterogeneous catalytic oxidation technologies all have the problems of removing single pollutants, poor ability to treat complex sewage, and low COD removal efficiency. Summary of the invention

[0006] The main purpose of the present invention is to provide an ozone oxidation catalyst and a preparation method and application thereof, so as to solve the problems of poor ability of ozone oxidation catalysts in the prior art to treat complex sewage and low COD removal efficiency.

[0007] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing an ozone oxidation catalyst is provided, and the preparation method comprises the following steps: S1, mixing copper nitrate, lanthanum nitrate, a dispersant and a binder to obtain an impregnation solution; S2, immersing a modified γ-activated alumina carrier in the impregnation solution to obtain a catalyst precursor; S3, drying and calcining the catalyst precursor to obtain an ozone oxidation catalyst; wherein the dispersant is a mixed solution of β-cyclodextrin and ethanol, and the binder is aqueous ammonia.

[0008] Furthermore, the weight ratio of the modified γ-activated alumina carrier to the impregnation solution is (3-4): (10-20).

[0009] Furthermore, the molar ratio of copper ions in copper nitrate to ammonia in ammonia water is 1:(6-8). Preferably, the molar concentration of ammonia water is 0.1-2 mol / L.

[0010] Furthermore, the weight concentration of β-cyclodextrin in the impregnation solution is 0.05-1.5%.

[0011] Furthermore, the molar ratio of copper ions in copper nitrate to lanthanum ions in lanthanum nitrate in the impregnation solution is (14-8):1.

[0012] Furthermore, the weight ratio of ethanol to β-cyclodextrin is (10-8):(1-2).

[0013] Furthermore, the calcination process includes heating the dried catalyst precursor to 280-320°C at a rate of 8-20°C / min and calcining it for 1-3h, and then heating it to 390-510°C at a rate of 3-8°C / min and calcining it for 6-15h to obtain an ozone oxidation catalyst.

[0014] In order to achieve the above object, according to one aspect of the present invention, an ozone oxidation catalyst is provided. The ozone oxidation catalyst is prepared by the above-mentioned preparation method of the ozone oxidation catalyst.

[0015] To achieve the above object, according to one aspect of the present invention, there is provided an ozone oxidation catalyst for use in the oxidation process of wastewater after biochemical treatment, wherein the ozone oxidation catalyst is prepared by the above-mentioned preparation method of the ozone oxidation catalyst.

[0016] Furthermore, the COD of the sewage is 75.2-90.0 mg / L.

[0017] The present invention prepares an ozone oxidation catalyst by an impregnation method, uses modified γ-active alumina as a carrier, copper oxide and lanthanum oxide as active components, and introduces an ethanol mixed solution of β-cyclodextrin as a dispersant and ammonia water as a binder to synergistically enhance the catalytic activity and stability of the ozone oxidation catalyst. When the catalyst is subsequently applied to the oxidation of sewage after biochemical treatment, the catalyst has better ability to treat complex sewage and a higher COD removal rate. At the same time, the preparation method of the present invention is simpler and has a lower preparation cost. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0019] As described in the background technology section, the ozone oxidation catalyst in the prior art has poor ability to treat complex sewage and low COD removal efficiency.

[0020] In order to solve this problem, the present invention provides a method for preparing an ozone oxidation catalyst. The preparation method comprises the following steps: S1, mixing copper nitrate, lanthanum nitrate, a dispersant and a binder to obtain an impregnation solution; S2, immersing a modified γ-activated alumina carrier in the impregnation solution to obtain a catalyst precursor; S3, drying and calcining the catalyst precursor to obtain an ozone oxidation catalyst. The dispersant is a mixed solution of β-cyclodextrin and ethanol, and the binder is ammonia water.

[0021] The present invention immerses the modified γ-active alumina carrier in a liquid containing active substances copper nitrate and lanthanum nitrate, dispersants β-cyclodextrin and ethanol, and ammonia water as a binder, and the active substances are gradually adsorbed on the carrier surface. After the impregnation equilibrium, a catalyst precursor is obtained, and then the catalyst precursor is dried and calcined to obtain an ozone oxidation catalyst, wherein the active components in the ozone oxidation catalyst are copper oxide and lanthanum oxide. Among them, the modified γ-active alumina is used as a carrier, and its higher specific surface area and pore volume can be used to improve the dispersibility of the active components thereon, thereby improving the catalytic activity of the catalyst. The mixed solution of β-cyclodextrin and ethanol is used as a dispersant, which can improve the utilization rate of the active components, thereby improving the catalytic activity of the catalyst. Ammonia water is used as a binder, and its weak alkalinity can be used to improve the acid strength distribution on the carrier surface, so as to promote a higher binding strength between the active components and the carrier, thereby improving the stability of the catalyst. The present invention introduces β-cyclodextrin, ethanol and ammonia water to synergistically enhance the catalytic activity and stability of the ozone oxidation catalyst, and when it is subsequently applied to the oxidation of sewage after biochemical treatment, it has better ability to treat complex sewage and higher COD removal rate. At the same time, the preparation method of the present invention is simpler and has lower cost.

[0022] In addition, the carrier γ-activated alumina used in the present invention has a specific surface area of ​​about 177 m 2 / g, pore volume 0.40mL / g, particle size 2mm~4mm. The preparation method of γ-Al2O3 is as follows: take 1000mL of alumina, wash it with distilled water 3 times to remove floating dust. Soak the alumina in 1200mL of 0.1mol / L citric acid at 80℃ for 4h, drain the residual liquid, dry it in a ventilated place away from light at room temperature, put the dried carrier into a forced air drying oven, and dry it at 120℃ for 5h to obtain the γ-activated alumina carrier.

[0023] Preferably, the weight ratio of the modified γ-activated alumina carrier to the impregnation liquid is (3-4): (10-20). Within this range, the dispersion effect of the active component in the impregnation liquid is better, and good dispersibility can improve the utilization rate of the active component. At the same time, the binding strength between the active component and the carrier is stronger, and the distribution of the active component on the carrier is more uniform, which can further balance the high catalytic activity and high stability of the catalyst.

[0024] Preferably, the molar ratio of copper ions in copper nitrate to ammonia in ammonia water is 1:(6-8). Within this range, the binding strength between the active component and the carrier can be further improved, which can improve the stability of the catalyst. More preferably, the molar concentration of ammonia water is 0.1-2 mol / L, based on which the acid strength distribution on the carrier surface can be more effectively improved.

[0025] In a preferred embodiment, the weight concentration of β-cyclodextrin in the impregnation solution is 0.05-1.5%, which can promote better dispersion of active substances in the impregnation solution, higher utilization of active components, and better catalytic activity of the catalyst.

[0026] For the purpose of promoting better catalytic activity of the catalyst, the molar ratio of copper ions in copper nitrate and lanthanum ions in lanthanum nitrate in the impregnation solution is (14-8):1.

[0027] In order to further promote better dispersion effect and higher utilization rate of active substances in the impregnation solution, the weight ratio of β-cyclodextrin and ethanol in the dispersant is (10-8): (1-2).

[0028] Preferably, the calcination process includes heating the dried catalyst precursor to 280-320°C at a rate of 8-20°C / min for 1-3h, and then heating it to 390-510°C at a rate of 3-8°C / min for 6-15h to obtain an ozone oxidation catalyst. This operation can make the performance of the active components in the catalyst more uniform and stable during the calcination process.

[0029] The present invention also provides an ozone oxidation catalyst, which is prepared by the above-mentioned preparation method of the ozone oxidation catalyst.

[0030] Based on the reasons mentioned above, the ozone oxidation catalyst of the present invention has better catalytic activity and stability. When it is subsequently used in the oxidation process of sewage after biochemical treatment, it has better ability to treat complex sewage and higher COD removal rate.

[0031] The present invention also provides an application of an ozone oxidation catalyst in the oxidation process of biochemically treated sewage, wherein the ozone oxidation catalyst is prepared by the above-mentioned preparation method of the ozone oxidation catalyst. In a preferred embodiment, the COD of the sewage is 75.2-90.0 mg / L.

[0032] Based on the reasons mentioned above, the ozone oxidation catalyst of the present invention has better catalytic activity and stability, especially when used in the oxidation process of sewage after biochemical treatment, it has better ability to treat complex sewage and higher COD removal rate.

[0033] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0034] Example 1

[0035] Preparation of modified γ-activated alumina carrier

[0036] Take 700g of alumina, put it into a 3000mL beaker, wash it with distilled water for 3 times to remove the floating dust, then soak it with 1200mL of 0.1mol / L citric acid at 80℃ for 4h, drain the residual liquid, dry it in a ventilated place away from light at room temperature, put the dried carrier into a forced air drying oven, and dry it at 120℃ for 5h to obtain the modified γ-activated alumina carrier.

[0037] Example 2

[0038] Take analytical pure copper nitrate to prepare 1 mol / L copper nitrate mother solution. Take analytical pure lanthanum nitrate to prepare 1 mol / L lanthanum nitrate mother solution. Use the prepared copper nitrate mother solution, lanthanum nitrate mother solution, analytical pure ammonia water, anhydrous ethanol and analytical pure β-cyclodextrin to prepare the impregnation solution. The formula of the impregnation solution is as follows: the molar concentration of copper nitrate is 0.6 mol / L. The molar ratio of copper nitrate to lanthanum nitrate is 10:1, the molar ratio of copper nitrate to ammonia water is 1:6, the weight concentration of β-cyclodextrin in the impregnation solution is 0.5%, and the weight ratio of ethanol to β-cyclodextrin in the dispersant is 10:1.

[0039] Take 150g of the modified γ-activated alumina carrier prepared in Example 1 and immerse it in 600g of the impregnation solution, stirring it every 0.5h. After impregnation for 4h, drain the residual liquid, dry it in a ventilated place away from light at room temperature, put the dried catalyst precursor into a blast drying oven, dry it at 120℃ for 6h, put it into a muffle furnace, and program the temperature to roast, quickly heat it to 300℃ at a heating rate of 20℃ / min, roast it at a constant temperature for 2h, then heat it to 450℃ at a heating rate of 5℃ / min, and roast it at a constant temperature for 6h to obtain the catalyst. Among them, the weight ratio of the modified alumina carrier and the impregnation solution is 1:4.

[0040] Example 3

[0041] The difference from Example 2 is that the molar ratio of copper nitrate to lanthanum nitrate in the impregnation solution is 14:1.

[0042] Example 4

[0043] The difference from Example 2 is that the molar ratio of copper nitrate to lanthanum nitrate in the impregnation solution is 8:1.

[0044] Example 5

[0045] The difference from Example 2 is that the weight concentration of β-cyclodextrin in the impregnation solution is 0.05%.

[0046] Example 6

[0047] The difference from Example 2 is that the weight concentration of β-cyclodextrin in the impregnation solution is 1.5%.

[0048] Example 7

[0049] The difference from Example 2 is that during the programmed temperature-raising calcination, the temperature is rapidly raised to 280°C at a heating rate of 20°C / min, and the temperature is kept constant for 2 hours, and then the temperature is raised to 450°C at a heating rate of 5°C / min, and the temperature is kept constant for 6 hours.

[0050] Example 8

[0051] The difference from Example 2 is that during the programmed temperature-raising calcination, the temperature is rapidly raised to 300° C. at a heating rate of 20° C. / min, and the temperature is kept constant for 2 h, and then the temperature is raised to 400° C. at a heating rate of 5° C. / min, and the temperature is kept constant for 6 h.

[0052] Example 9

[0053] The difference from Example 2 is that the weight ratio of the modified alumina carrier to the impregnation solution is 3:10.

[0054] Example 10

[0055] The difference from Example 2 is that the weight ratio of the modified alumina carrier to the impregnation solution is 4:20.

[0056] Embodiment 11

[0057] The difference from Example 2 is that the weight concentration of β-cyclodextrin is 3%.

[0058] Example 12

[0059] The difference from Example 2 is that the molar ratio of copper ions in copper nitrate to ammonia in aqueous ammonia is 1:3.

[0060] Comparative Example 1

[0061] The only difference from Example 2 is that the mixed solution of anhydrous ethanol and analytical grade β-cyclodextrin as a dispersant is not added to the impregnation liquid.

[0062] Comparative Example 2

[0063] The only difference from Example 2 is that no ammonia water, a co-binding agent, is added to the impregnation solution.

[0064] Performance characterization:

[0065] 100 mL of each of the catalysts prepared in Examples 2 to 12, Comparative Examples 1 and 2, and the carrier prepared in Example 1 were taken for activity evaluation comparison experiments. The effluent from a sewage plant (COD of 75.2 mg / L) was used as the water source, and the activity evaluation was carried out using a continuous reaction. The ozone concentration in the aerated mixed gas was 1.43 g / m 3 The activity evaluation was carried out for 56 hours, and samples were taken and analyzed every 6 hours. The evaluation results are shown in Appendix 1.

[0066] Table 1

[0067]

[0068] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An application of an ozone oxidation catalyst in the oxidation process of wastewater after biochemical treatment, characterized in that: The preparation method of the ozone oxidation catalyst comprises the following steps: S1, mixing copper nitrate, lanthanum nitrate, a dispersant and a binder to obtain an impregnation solution; S2, immersing the modified γ-activated alumina carrier in the impregnation solution to obtain a catalyst precursor; S3, drying and calcining the catalyst precursor to obtain the ozone oxidation catalyst; The dispersant is a mixed solution of β-cyclodextrin and ethanol, and the binder is aqueous ammonia. The molar ratio of copper ions in the copper nitrate and lanthanum ions in the lanthanum nitrate in the impregnation solution is (14-8):

1. In the dispersant, the weight ratio of ethanol and β-cyclodextrin is (10-8):(1-2).

2. The use of the ozone oxidation catalyst according to claim 1 in the process of oxidizing wastewater after biochemical treatment, characterized in that: The weight ratio of the modified γ-activated alumina carrier to the impregnation solution is (3-4): (10-20).

3. The use of the ozone oxidation catalyst according to claim 2 in the process of oxidizing wastewater after biochemical treatment, characterized in that: The molar ratio of the copper ions in the copper nitrate to the ammonia in the ammonia water is 1:(6-8).

4. The use of the ozone oxidation catalyst according to claim 3 in the process of oxidizing wastewater after biochemical treatment, characterized in that: The molar concentration of the ammonia water is 0.1-2 mol / L.

5. Use of the ozone oxidation catalyst according to any one of claims 1 to 4 in the process of oxidizing wastewater after biochemical treatment, characterized in that: The weight concentration of the β-cyclodextrin in the impregnation solution is 0.05-1.5%.

6. Use of the ozone oxidation catalyst according to any one of claims 1 to 4 in the process of oxidizing wastewater after biochemical treatment, characterized in that: The calcination process comprises: The dried catalyst precursor is first heated to 280-320° C. at a rate of 8-20° C. / min and calcined for 1-3 hours, and then heated to 390-510° C. at a rate of 3-8° C. / min and calcined for 6-15 hours to obtain the ozone oxidation catalyst.

7. The use of the ozone oxidation catalyst according to claim 1 in the process of oxidizing wastewater after biochemical treatment, characterized in that: The COD of the sewage is 75.2~90.0 mg / L.