Parts for molten metal baths
By using a ceramic thermal spray film based on non-oxide ceramics on the components for the molten metal bath, combined with an oxide ceramic and a cermet base layer, the problems of insufficient resistance to molten metal and wear resistance in the existing technology are solved, and the problem is achieved Efficient durability and corrosion resistance.
Patent Information
- Application Number
- CN202180015706.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-02-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-02-08
AI Technical Summary
In existing technologies such as hot-dip galvanizing and hot-dip aluminum plating, the molten metal bath components have insufficient resistance to molten metal and wear resistance, and the existing ceramic films are easily decomposed or sublimated at high temperatures, resulting in thin film thickness and poor wear resistance. Low, it is difficult to maintain excellent performance for a long time.
The ceramic thermal spray film is mainly composed of non-oxide ceramics, dispersed with oxide ceramics, and has an oxygen content of 5 to 35 wt%. It forms a dense film through high-speed flame spraying and combines the carbide cermet and boride cermet base layers. , improve durability and corrosion resistance.
The components used in the molten metal bath can maintain excellent resistance to molten metal and wear resistance for a long time at high temperatures, improve the adhesion and durability of the film, and reduce the risk of wear and corrosion.
Smart Images

Figure CN115151677B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to various rollers, bearings, sleeves, bushings, metal parts for adjusting the coating amount, and other molten metal bath parts used in the fields of hot-dip galvanizing, hot-dip galvanneal alloy coating, and hot-dip aluminizing. Background Art
[0002] Hot-dip metal coating technologies such as hot-dip galvanizing, hot-dip aluminum coating, and hot-dip galvanized-aluminum alloy coating can demonstrate excellent rust resistance and corrosion resistance. Therefore, they have long been used in major parts of automobiles, aircraft, vehicles, buildings, home appliances, etc., and are still a useful surface treatment technology that plays an important role today.
[0003] Generally, the plating treatment of hot-dip galvanized steel sheets produced in large quantities is often performed by a continuous plating process, in which various molten metal bath components such as a sink roll immersed in the plating bath and a support roll arranged near the surface of the plating bath are used.
[0004] Such molten metal bath parts are immersed in the plating bath, or are placed at a position where molten metal is likely to splash and adhere, and are used in a state of contact with a high-temperature steel plate to which the molten metal adheres. Therefore, the properties required are: (1) not easily corroded by the molten metal, (2) not easily worn even when in contact with a plate (steel plate), (3) easy peeling of the attached molten metal and maintenance and inspection, (4) long life and low cost as plating parts, (5) good thermal shock resistance when immersed in a high-temperature molten metal bath, etc. In addition, various studies have been conducted in the past to meet these requirements.
[0005] Patent document 1 describes a component for a molten metal bath, in which a thermal spray coating containing only nitrides and no metal components is formed on a base layer on the surface of a substrate. As a thermal spray nitride, tiny primary particles of 0.01 to 0.1 μm are prepared, and the primary particles are adjusted to secondary particles of a predetermined particle size with an organic binder to form a thermal spray powder, and the thermal spray powder is used to perform plasma spraying to provide a component having a thermal spray coating having excellent resistance to molten metal on the surface.
[0006] Patent Document 2 describes a ceramic-coated roller for use in a molten zinc bath, which has a ceramic film on the outermost surface thereof formed by an ion plating method and made of a nitride or carbonitride of Ti, Al, Hf, or Zr.
[0007] Patent document 3 describes a component for immersion in a molten metal bath having excellent corrosion resistance and wear resistance, wherein the surface film is composed of a composite boride of one or more of tungsten carbide, titanium carbide, niobium carbide, and molybdenum carbide and one or more of tungsten-cobalt boride, molybdenum-cobalt boride, and niobium-cobalt boride.
[0008] Patent Document 4 describes a molten metal bath component having a lower layer film and an upper oxide film, wherein the lower layer film is made of a mixed material of boride and carbide and is formed of a thermal spraying material containing no metal component.
[0009] Patent documents 5-8 describe a method in which a slurry consisting of a mixture of oxides and nitrides is coated on the surface of a WC-Co metal ceramic thermal spray film coated on a substrate, and then heated and fired, thereby filling the tiny pores of the WC-Co metal ceramic thermal spray film with fired particles consisting of the mixture.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. H07-062516
[0013] Patent Document 2: Japanese Patent Application Publication No. H09-025583
[0014] Patent Document 3: Japanese Patent Application Publication No. H11-080917
[0015] Patent Document 4: Japanese Patent Application Publication No. 2004-346395
[0016] Patent Document 5: Japanese Patent Application Publication No. 2000-54095
[0017] Patent Document 6: Japanese Patent Application Publication No. 2000-54096
[0018] Patent Document 7: Japanese Patent Application Publication No. 2000-144358
[0019] Patent Document 8: Japanese Patent Application Publication No. 2000-144364 Summary of the invention
[0020] -Problems to be solved by the invention-
[0021] The construction method described in Patent Document 1 has the problem that the nitride used decomposes or sublimates, making it difficult to form a film. The ion plating method of Patent Document 2 has a slow film formation speed and a thin film thickness. In the components of Patent Document 3, since a small amount of metal layer remains on the outermost layer, corrosion caused by bath components is a concern. The outermost layer of the components of Patent Document 4 is an oxide layer, which has problems in terms of resistance to molten metal.
[0022] In addition, the common problem of Patent Documents 1 and 4 is that nitride ceramics, boride ceramics, and carbide ceramics that are easily sublimated and decomposed at high temperatures are used directly as thermal spray materials. Therefore, if the thermal spraying conditions are not adequately selected, a film will not be formed, or even if a film is formed, it will be difficult to form a dense film with sufficient adhesion.
[0023] In contrast, as shown in Patent Documents 5 to 8, if a method is used in which sintered fine particles formed of a mixture of oxides and nitrides are filled into the micropores of the thermal spray coating using a slurry, the nitrides can be retained on the outermost surface. However, the coating obtained by applying and sintering the slurry has low wear resistance, and this method has the disadvantage that a film of sufficient thickness cannot be covered as a whole.
[0024] The present invention has been made in view of the problems of the prior art, and an object of the present invention is to provide a member for a molten metal bath, the outermost surface of which has a film which can maintain excellent molten metal resistance and wear resistance for a long period of time.
[0025] -Solutions to solve the problem-
[0026] The molten metal bath component of the present invention is characterized in that it has a ceramic thermal spray coating as an outermost layer on a substrate, wherein the ceramic thermal spray coating has a non-oxide ceramic as a main component, contains oxide ceramic dispersed therein, and contains 5 to 35 wt % of oxygen.
[0027] In the present invention, the thermal spray film constituting the outermost surface contains non-oxide ceramics as the main component, and through the effect of the non-oxide ceramics, excellent molten metal resistance and wear resistance can be exerted. In addition, by appropriately dispersing the oxide ceramics in the thermal spray film mainly composed of non-oxide ceramics, the oxide ceramics act as a binder to connect the non-oxide ceramics, improve the inter-particle bonding force of the non-oxide ceramic particles, and obtain a dense film, which shows a high adhesion to the substrate. Moreover, even if such a film is immersed in a molten metal bath, it can also exert excellent molten metal resistance and wear resistance that can withstand actual use. In the present invention, "non-oxide ceramics as the main component" means that non-oxide ceramics are the most in mass units among the constituent components of the thermal spray film. As the existence ratio of oxide ceramics, it is necessary to make the entire thermal spray film contain 5 to 35wt% of oxygen. If it is less than 5wt%, the function as a binder for oxide ceramics will be impaired, and if it is greater than 35wt%, the function as a non-oxide ceramic cannot be fully exerted. By setting the oxygen content as described above, the characteristics of non-oxide ceramics and oxide ceramics can be presented in a well-balanced manner. From the viewpoint of maximizing the characteristics of the non-oxide ceramic, it is preferred that the thermal spray coating consists only of the non-oxide ceramic, the oxide ceramic, and inevitable impurities, and contains 5 to 35 wt % of oxygen.
[0028] Examples of the non-oxide ceramics include ceramics containing one or more elements selected from Cr, Ti, Zr, Al, B, Nb, and Si, and one or more selected from nitrides, borides, and carbides.
[0029] Examples of the oxide ceramics include one or more ceramics selected from the group consisting of chromium oxide, titanium oxide, zirconium oxide, aluminum oxide, silicon oxide, boron oxide, and niobium oxide.
[0030] Preferably, the thickness of the ceramic thermal spray film is 15 to 500 μm. If the thickness of the thermal spray film is 15 μm or more, the durability as a component for a molten metal bath is sufficiently excellent. In addition, if the thickness of the thermal spray film is 500 μm or less, the mechanical strength reduction caused by the influence of the residual stress inside the film can be prevented.
[0031] A base layer may be further provided between the substrate and the ceramic thermal spray coating, the base layer containing one or more metal ceramics selected from carbide metal ceramics, boride metal ceramics, and carbide-boride metal ceramics. By forming such a base layer, the metal component is not exposed to the outermost surface, thereby improving the durability and corrosion resistance of the entire surface layer of the molten metal bath component. From the viewpoint of maximizing the characteristics of the above-mentioned metal ceramic, preferably, the above-mentioned base layer is composed only of one or more metal ceramics selected from carbide metal ceramics, boride metal ceramics, and carbide-boride metal ceramics and inevitable impurities.
[0032] -Effects of the Invention-
[0033] The molten metal bath component of the present invention has a ceramic thermal spray coating on the outermost surface of the substrate. The ceramic thermal spray coating is mainly composed of non-oxide ceramics with a certain amount of oxide ceramics dispersed therein, and thus can exhibit excellent molten metal resistance and wear resistance for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic cross-sectional view of the surface layer of the component for the molten metal bath.
[0035] Figure 2 This is a schematic diagram of the main parts showing an example of a thermal spraying device for performing the suspended high velocity flame spraying method.
[0036] Figure 3 This is a schematic cross-sectional view of a continuous hot-dip galvanizing facility using components for a molten metal bath.
[0037] Figure 4This is a table summarizing scanning electron microscope (SEM) cross-sectional observation photographs of each film formed in Examples 1 to 6 and Comparative Example 1, and numerical values of hardness HV and film thickness of each cross section.
[0038] Figure 5 The following are scanning electron microscope (SEM) cross-sectional observation photographs of the respective films produced in Examples 1 to 6, and mapping photographs showing the distribution of the respective components in the cross-sectional observation range.
[0039] Figure 6 This is a graph showing the results of the Suga abrasion test of the test pieces prepared in Examples 2 and 3 and Comparative Examples 1 to 3.
[0040] Figure 7 The photographs show how the contact angles of the test pieces prepared in Examples 1, 2, and 6 and Comparative Example 1, and the test piece of Comparative Example 4 were measured with respect to molten zinc on their surfaces.
[0041] Figure 8 This is a summary table showing cross-sectional observation photographs of the test pieces prepared in Examples 7, 8, 9 and Comparative Example 5 after the immersion test, the content (wt%) of zinc components contained in the upper film, and the film thicknesses of the upper and lower films. DETAILED DESCRIPTION
[0042] An embodiment of the present invention will be described. Figure 1 2 is a schematic cross-sectional view of the surface layer of the molten metal bath component 20 of the present embodiment. The molten metal bath component 20 includes a substrate 100, a lower layer portion (base layer) 21 formed on the surface of the substrate 100, and an upper layer portion 22 formed on the surface of the lower layer portion 21. As the substrate 100, for example, a steel substrate can be cited.
[0043] The upper layer 22 of the outermost layer is a ceramic thermal spray film with non-oxide ceramic as the main component and oxide ceramic dispersed therein. The oxygen contained in the thermal spray film is 5 to 35 wt % of the entire film. As the non-oxide ceramic, one or more ceramics selected from carbide ceramics, nitride ceramics, and boride ceramics can be listed.
[0044] Specifically, the non-oxide ceramics include ceramics containing one or more metal elements selected from Cr, Ti, Zr, Al, B, Nb, and Si, and one or more ceramics selected from nitrides, borides, and carbides.
[0045] Examples of carbide ceramics include TiC, B4C, SiC, ZrC, Cr3C2, and NbC. Examples of nitride ceramics include TiN, CrN, Cr2N, AlN, BN, Si3N4, NbN, and ZrN. Examples of boride ceramics include TiB2, ZrB2, AlB2, NbB2, CrB2, and SiB4.
[0046] As the oxide ceramic contained in the upper layer 22, one or more ceramics selected from the group consisting of chromium oxide, titanium oxide, zirconium oxide, aluminum oxide, silicon oxide, boron oxide, and niobium oxide can be cited. When the oxide ceramic is chromium oxide, preferably, the oxygen contained in the thermal spray film is 5 to 15 wt%. When the oxide ceramic is titanium oxide, preferably, the oxygen contained in the thermal spray film is 25 to 35 wt%. When the oxide ceramic is zirconium oxide, preferably, the oxygen contained in the thermal spray film is 15 to 25 wt%. When the oxide ceramic is aluminum oxide, preferably, the oxygen contained in the thermal spray film is 15 to 25 wt%. When the oxide ceramic is silicon oxide, preferably, the oxygen contained in the thermal spray film is 15 to 25 wt%. When the oxide ceramic is boron oxide, preferably, the oxygen contained in the thermal spray film is 25 to 35 wt%. When the oxide ceramic is niobium oxide, preferably, the oxygen contained in the thermal spray film is 15 to 25 wt%. From the viewpoint of maintaining a good balance between non-oxide ceramics and oxide ceramics, the preferred oxygen content varies slightly depending on the type of oxide ceramics contained in the thermal spray coating.
[0047] The lower layer 21 formed between the upper layer 22 and the substrate 100 can be appropriately selected according to the required characteristics without any particular limitation. From the viewpoint of improving durability and corrosion resistance, it is preferably a thermal spray film containing one or more metal ceramics selected from carbide cermets, boride cermets, and carbide-boride cermets. Thus, the metal component will not be exposed to the outermost surface, and the durability and corrosion resistance of the entire surface layer can be improved. In particular, by forming the lower layer 21 with a thermal spray film, a layer having a film thickness of more than a certain value can be continuously formed on the substrate 100 even for a complex shape, so that it is easier to ensure corrosion resistance and corrosion resistance.
[0048] Examples of carbide cermets include cermets containing at least one of TiC, NbC, WC, Cr3C2, B4C, TaC, BiC, ZrC, HfC, and VC. Examples of boride cermets include cermets containing at least one of TiB, ZrB2, HfB2, VB2, TaB2, NiB2, W2B5, and CrB2. Examples of carbide-boride cermets include cermets containing at least one of TiC, NbC, WC, Cr3C2, B4C, TaC, BiC, ZrC, HfC, and VC; and cermets containing at least one of TiB, ZrB2, HfB2, VB2, TaB2, NiB2, W2B5, and CrB2. In addition, as metal components contained in these metal ceramics, metal components containing at least one of Ni, Cr, Co, Al, Ta, Y, W, Nb, V, Ti, B, Si, Mo, Zr, Fe, Hf, and La can be listed.
[0049] It is preferred to use a high-velocity flame spraying method to form the thermal spray coating constituting the upper layer 22 and the lower layer 21. The high-velocity flame spraying method is a spraying method that uses the combustion energy of the combustion gas as a heat source, and generates a supersonic flame by increasing the pressure in the combustion chamber, supplies the thermal spray powder to the center of the supersonic flame jet and accelerates it to a molten or semi-molten state, and continuously sprays it at a high speed.
[0050] Since the molten thermal spray particles collide with the substrate at supersonic speed, a dense thermal spray film with high adhesion can be formed, and in particular, since the thermal spray film can be formed continuously, a homogeneous thermal spray film can be obtained. The combustion gas that can be used as a heat source can use hydrogen, acetylene, ethylene, propane and other combustible gases with carbon and hydrogen as main components, and oxygen-containing combustion-supporting gases. Liquid fuels such as kerosene can also be used instead of combustible gases.
[0051] Specifically, for example, a mixed gas such as oxygen / propane, oxygen / propylene, oxygen / natural gas, oxygen / ethylene, oxygen / hydrogen, etc. can be used as a combustion gas to generate a supersonic flame with a flame speed of 900 to 2500 m / s and a flame temperature of 1800 to 3800°C. The thermal spraying distance is maintained at 100 to 350 mm, and the substrate temperature during the thermal spraying process is controlled below 200°C for thermal spraying.
[0052] It is particularly preferred to use a suspended high-velocity flame spraying method to form a ceramic thermal spray film that is mainly composed of non-oxide ceramics, dispersed with oxide ceramics, and contains 5 to 35 wt% of oxygen, which constitutes the upper portion 22. The reason is that, first of all, in order to obtain a thermal spray film that is mainly composed of non-oxide ceramics and appropriately dispersed with oxide ceramics, it is important to use non-oxide ceramic materials with smaller particle sizes. The smaller the particle size of the material, the easier it is for the non-oxide ceramic material to become oxide ceramics during the thermal spraying process, which acts as a binder for tightly connecting the particles of the non-oxide ceramics that constitute the thermal spray film. However, on the other hand, when using thermal spray material particles, there is a difficulty in agglomerating the materials when the thermal spray material is transported to the thermal spray flame.
[0053] In contrast, in the case of the suspended high-speed flame spraying method, since the non-oxide ceramic material is transported as a suspension dispersed in a solvent, it can be directly thrown into the flame while maintaining a particle state. In addition, the film thus formed is not only a dense film formed by the filmization of materials with small particle sizes, but also a state in which the oxide is dispersed in an appropriate amount, which helps to improve the inter-particle bonding force of the particles constituting the film, thereby improving the adhesion to the substrate.
[0054] It should be noted that there is also a suspension plasma spraying method as another spraying method using a thermal spray material as a suspension. However, since the suspension plasma spraying method generally uses a very high temperature plasma flame, there is a tendency that too much oxide is generated, or the material sublimates, resulting in a significant decrease in the yield rate. Therefore, if the purpose is to form a thermal spray film with non-oxide ceramics as the main component, the suspension high-velocity flame spraying method is more preferred.
[0055] Figure 2 1 is a schematic diagram of the main parts of an example of a thermal spraying device 1 for implementing a suspended high-velocity flame spraying method. The thermal spraying device 1 is a suspended high-velocity flame thermal spraying device configured to supply a thermal spraying material from the outside as a slurry (suspension). The thermal spraying device 1 is an external supply type device that supplies a slurry prepared by dispersing a thermal spraying powder in a solvent from the outside, and includes a thermal spraying gun 2 and a nozzle 3 for slurry supply.
[0056] The thermal spray gun 2 includes a combustion container portion 5 forming a combustion chamber 4, a thermal spray nozzle 6 connected to the combustion container portion 5, and an ignition device 7. A gas containing high-pressure oxygen and fuel is supplied to the combustion chamber 4, and the gas is ignited by the ignition device 7. Then, the flame 10 generated in the combustion chamber 4 is converged by the thermal spray nozzle 6, expanded and supersonic flamed, and ejected at high speed from the tip of the thermal spray nozzle 6. The slurry 11 is supplied from the slurry supply nozzle 3 to the ejected flame 10. The thermal spray powder in the slurry 11 becomes a molten or semi-molten body, and is accelerated by the flame 10, and collides with the substrate 100 at high speed, thereby forming a thermal spray film on the substrate 100.
[0057] The slurry 11 is prepared by dispersing the thermal spray powder in a solvent containing a dispersion medium composed of water or alcohol and an organic dispersant as an option. The slurry 11 contains particles of the thermal spray powder at a mass ratio of 5 to 40%. The slurry 11 is supplied to the flame 10 sprayed from the tip of the thermal spray nozzle 6.
[0058] If the slurry is supplied to the inside of the thermal spray nozzle by an internal supply method, the thermal spray material will be deposited in the nozzle tube, and there is a possibility that it will condense and splash. Figure 2 As shown, by adopting an external supply method in which the slurry 11 is supplied from the outside to the flame 10, the occurrence of splashing can be prevented.
[0059] The thermal spraying powder may be only non-oxide ceramic powder or a mixed powder containing non-oxide ceramic powder and oxide ceramic powder. When only non-oxide ceramic powder is used, preferably, the average particle size of the powder is 0.1 to 5.0 μm, and more preferably, the particle size distribution of the non-oxide ceramic powder is at least in the range of 0.1 μm to less than 1.0 μm, and in the range of 1.0 μm to less than 10.0 μm, respectively. The average particle size of the above-mentioned powder is defined in this specification as: the particle size (median particle size) with a cumulative value of 50% when the particle size distribution is measured by a laser diffraction scattering method (micro-track method).
[0060] In the above, an example of a method for forming a thermal spray coating on the outermost surface of the molten metal bath component of the present invention is described, but other spraying methods may also be used as long as the thermal spray coating is a ceramic thermal spray coating having a non-oxide ceramic as a main component, dispersed oxide ceramics, and containing 5 to 35 wt% of oxygen.
[0061] The thickness of the thermal spray coating constituting the upper layer 22 is preferably in the range of 15 to 500 μm, and the thickness is appropriately set according to the purpose of use. If the thickness is 15 μm or more, the durability as a molten metal bath component is sufficiently excellent, and if it is 500 μm or less, the mechanical strength can be prevented from decreasing due to the influence of residual stress inside the coating.
[0062] The thickness of the thermal spray coating constituting the lower layer 21 is preferably in the range of 50 to 500 μm, and the thickness is appropriately set according to the purpose of use. If the thickness is 50 μm or more, it has a significant effect on improving the durability and corrosion resistance of the entire surface layer, and if it is 500 μm or less, it can prevent the mechanical strength from decreasing due to the influence of residual stress inside the coating.
[0063] The porosity of the thermal sprayed film constituting the upper portion 22 and the lower portion 21 may be approximately 0.1 to 5%. Taking into account the corrosion resistance to molten metal, the porosity of at least one of the upper portion 22 and the lower portion 21 is preferably 0.1 to 1%, and more preferably, the porosity of both the upper portion 22 and the lower portion 21 is 0.1 to 1%.
[0064] Figure 3 The schematic cross-sectional view of a continuous hot-dip galvanizing equipment 30 using a molten metal bath member 20. The equipment 30 includes a coating bath 31 for accommodating hot-dip galvanizing, a sinking roll 32 and a support roll 33 provided in the coating bath 31, a guide roll 34 for guiding the plated steel sheet M after passing through the sinking roll 32 and the support roll 33, and a spray nozzle 35 for blowing away excess zinc and the like attached to the steel sheet M. The sinking roll 32 and the support roll 33 are immersed in the coating bath 31. Among them, the coating bath 31, the sinking roll 32, the support roll 33, the guide roll 34, and the spray nozzle 35 can all be applied to the molten metal bath member 20 of the present invention.
[0065] According to the molten metal bath component 20 of the present embodiment, excellent molten metal resistance and wear resistance can be exhibited by the role of the non-oxide ceramic that serves as the base of the thermal spray film constituting the outermost surface thereof, and a dense film can be obtained by appropriately dispersing the oxide ceramic therein, and high adhesion to the substrate 100 can be exhibited. Therefore, when used as the molten metal bath component 20, very excellent molten metal resistance and wear resistance can be exhibited for a long time.
[0066] In addition, the lower layer 21 below the upper layer 22 formed by the thermal spraying film also has a thermal spraying film containing one or more metal ceramics selected from carbide metal ceramics, boride metal ceramics, and carbide-boride metal ceramics, thereby significantly improving the durability and corrosion resistance of the entire surface layer.
[0067] [Example]
[0068] Hereinafter, examples in which test pieces corresponding to the member for a molten metal bath of the present invention were prepared and verification test results of the physical properties of the test pieces prepared in the examples will be described.
[0069] (Test piece preparation)
[0070] As a substrate for forming a thermal spray coating, a steel (SUS304) flat plate with a length of 50 mm, a width of 50 mm, and a thickness of 5 mm was prepared. A suspension formed by dispersing thermal spray powder with an average particle size (D50) of 3 μm in a dispersion medium was used as a thermal spray material. Suspended high-velocity flame thermal spraying was performed in the atmosphere to produce each test piece. As thermal spray powder, aluminum nitride (Example 1), chromium nitride (Example 2), chromium carbide (Example 3), titanium nitride (Example 4), titanium carbide (Example 5), and titanium boride (Example 6) were used. As a nozzle for a thermal spray gun, a Figure 2 As the dispersion medium, water was used in Examples 3, 5, and 6, and ethanol was used in Examples 1, 2, and 4.
[0071] As a substrate for forming a film formed by coating and firing the slurry, a flat plate made of steel (SUS304) with a length of 50 mm, a width of 50 mm, and a thickness of 5 mm was prepared, a mixed slurry of an aqueous solution of chromic acid and boron nitride powder was coated on the surface, and heated and fired at 550°C for 1 hour to form a film on the substrate, which was used as a comparison material (Comparison Example 1).
[0072] (Film observation and hardness measurement)
[0073] The cross-sectional structures of the films formed in Examples 1 to 6 and Comparative Example 1 were observed. In addition, the surface hardness HV of each film was measured using a Vickers hardness tester. Figure 4 This is a summary table of scanning electron microscope (SEM) cross-sectional observation photographs of each film formed in Examples 1 to 6 and Comparative Example 1, as well as the numerical values of the hardness HV and film thickness of each cross section. The cross sections of the thermal sprayed films formed by the suspended high-velocity flame spraying method in Examples 1 to 6 are denser than the cross sections of the films formed by slurry coating and firing in Comparative Example 1. In addition, the surface hardness of the thermal sprayed films formed in Examples 1 to 6 is much greater than the surface hardness of the film formed in Comparative Example 1.
[0074] (Component Analysis)
[0075] The films formed in Examples 1 to 6 were subjected to component analysis. Figure 5The following are scanning electron microscope (SEM) cross-sectional observation photographs of each film produced in Examples 1 to 6, and mapping photographs showing the distribution of each component within the range, and the oxygen content within the range. The component analysis and mapping were performed using an energy dispersive X-ray analyzer (EDX).
[0076] like Figure 5 As shown in the figure, the distribution of O and the distribution of N, C or B are respectively present in different positions relative to the overall widespread presence of the main metal elements. In addition, their distribution is consistent with the color depth of the SEM photograph. That is, relative to the nitride ceramics, carbide ceramics, or boride ceramics as non-oxide ceramics, the oxide ceramics fill in between the non-oxide ceramics and are dispersed, which is presumed to contribute to the formation of a dense film with strong inter-particle bonding.
[0077] (Abrasion resistance)
[0078] The wear resistance of the thermal sprayed films formed in Examples 2 and 3 and the film formed in Comparative Example 1 were evaluated. In addition, in this test, test pieces in which the thermal sprayed films were formed by atmospheric pressure plasma spraying were used as Comparative Examples 2 and 3. In Comparative Example 2, the thermal spraying material used was aluminum oxide powder with a particle size of 10 to 45 μm, and in Comparative Example 3, the thermal spraying material used was chromium oxide powder with a particle size of 10 to 45 μm.
[0079] Figure 6 This is a graph showing the results of the Suga wear test of the test pieces prepared in Examples 2 and 3 and Comparative Examples 1 to 3. Figure 6 In the graph, the horizontal axis is the number of sliding times and the vertical axis is the wear loss (mm 3 ). In this test, the result showed that the test piece of Comparative Example 1, which formed a film by coating and firing the slurry, had low wear resistance and the substrate was exposed quickly. In addition, the test pieces of Examples 2 and 3 were compared with the test pieces of Comparative Examples 2 and 3. Compared with the test pieces of Comparative Examples 2 and 3, the test pieces of Examples 2 and 3 had less wear loss under the same number of sliding times, and it was confirmed that they had higher wear resistance.
[0080] (Wettability with molten metal)
[0081] The wettability of the thermal sprayed films formed in Examples 1, 2, and 6, the film formed in Comparative Example 1, and the steel (SUS304) substrate of Comparative Example 4 to molten metal (zinc) was evaluated. Figure 7 The photographs show how the contact angles of the test pieces prepared in Examples 1, 2, and 6 and Comparative Example 1, and the test piece of Comparative Example 4 were measured with respect to molten zinc on their surfaces.
[0082] The wettability was evaluated by placing the test piece in an electric furnace at 600°C and measuring the contact angle in a state of contact with molten zinc. As a result, in the test pieces of Examples 1, 2, and 6, the contact angles were about 130°, and in the test piece of Comparative Example 1, the contact angle was also about 125°, and it was confirmed that the wettability to molten metal was low. It can be seen that this is largely related to the presence of non-oxide ceramics on the surface of the film. In contrast, in the test piece of Comparative Example 4 exposed to steel, the contact angle was about 100°, and it was confirmed that the wettability to molten zinc was high.
[0083] (Reactivity with plating bath components)
[0084] As a supplementary test piece, after forming a tungsten carbide-cobalt metal ceramic thermal spray film on the substrate, various materials such as aluminum nitride (Example 7), chromium nitride (Example 8), and titanium boride (Example 9) were used under the same conditions as Examples 1, 2, and 6, respectively, and the thermal spray film was made by suspended high-velocity flame spraying to make a test piece with the thermal spray film; in addition, after forming a tungsten carbide-cobalt metal ceramic thermal spray film on the substrate, the film was formed under the same conditions as Comparative Example 1 to make a test piece (Comparative Example 5). The lower layer of the tungsten carbide-cobalt metal ceramic thermal spray film uses a tungsten carbide-cobalt metal ceramic powder material with a particle size of 10 to 53 μm as a thermal spray material, and is formed by high-velocity flame thermal spraying. The reactivity with the plating bath components is evaluated by cross-sectional observation after each test piece is immersed in a molten zinc pot for 168 hours, and by component analysis of the upper film.
[0085] Figure 8 This is a summary table of cross-sectional observation photographs of the test pieces prepared in Examples 7, 8, 9 and Comparative Example 5 after the immersion test, the content (wt%) of the zinc component contained in the upper film, and the film thickness of the upper film and the lower film. The content of the zinc component was detected by an energy dispersive X-ray analyzer (EDX). As a result, it can be confirmed that the test pieces prepared in Examples 7, 8, and 9 have a smaller amount of zinc (Zn) detected in the film than the test piece prepared in Comparative Example 5, and the reactivity with molten zinc is lower.
[0086] The above embodiments and examples are illustrative and non-restrictive. As long as they are used as parts for molten metal baths, their applicable objects are not limited. For the manufacturing method of thermal spray coating, other processes may be included according to the film forming object and the construction form. As long as the effect of the present invention is not impaired, the structures and processes described in the above embodiments may be changed, and the forms of other structures and processes set as needed are not limited.
[0087] -Explanation of symbols-
[0088] 1: Thermal spraying device
[0089] 2: Thermal spray gun
[0090] 3: Nozzle for slurry supply
[0091] 4: Combustion Chamber
[0092] 5: Combustion container
[0093] 6: Thermal spray nozzle
[0094] 7: Ignition device
[0095] 10: Fire
[0096] 11: Slurry
[0097] 20: Parts for molten metal bath
[0098] 21: Lower part
[0099] 22: Upper part
[0100] 100: Base material
[0101] 30: Continuous hot dip galvanizing equipment
[0102] 31: Plating bath
[0103] 32: Sinking roller
[0104] 33: Support roller
[0105] 34: Guide roller
[0106] 35: Spray nozzle
[0107] M: Plated steel sheet.
Claims
1. A component for a molten metal bath, characterized in that The molten metal bath component has a ceramic thermal spray coating composed of non-oxide ceramics, oxide ceramics, and inevitable impurities as an outermost layer on a substrate, wherein the ceramic thermal spray coating has the non-oxide ceramic as a main component, dispersedly contains the oxide ceramic, and contains 5 to 35 wt % of oxygen.
2. The component for a molten metal bath according to claim 1, characterized in that The non-oxide ceramic is a ceramic containing one or more elements selected from Cr, Ti, Zr, Al, B, Nb, and Si, and one or more selected from nitrides, borides, and carbides.
3. The component for a molten metal bath according to claim 1 or 2, characterized in that: The oxide ceramic is one or more ceramics selected from chromium oxide, titanium oxide, zirconium oxide, aluminum oxide, silicon oxide, boron oxide, and niobium oxide.
4. The component for a molten metal bath according to claim 1 or 2, characterized in that: The thickness of the ceramic thermal spraying film is 15 to 500 μm.
5. The component for a molten metal bath according to claim 1 or 2, characterized in that: An underlayer is provided between the substrate and the ceramic thermal spray coating, and the underlayer contains one or more cermets selected from the group consisting of carbide cermets, boride cermets, and carbide-boride cermets.
Citation Information
Patent Citations
Roll member for hot-dip metal coating bath, and its production
JP2000054095A
Roll member for hot-dip metal coating bath, and its production
JP2000054096A
Roll member for hot-dip metal coating bath, and its manufacture
JP2000144358A
Roll member for hot-dip metal coating bath, and its manufacture
JP2000144364A
Thermal spraying material of excellent molten metal erosion resistance, and member for molten metal bath
JP2004346395A