A black phosphorus-carbon composite material and its preparation method and application
The black phosphorus-carbon composite material is prepared by reacting amorphous red phosphorus and conductive carbon materials at high temperature and high pressure in the next step, which solves the problems of complex process and high cost in the existing technology and achieves the stability of black phosphorus in lithium/sodium ion batteries. applications and efficient electrochemical performance.
Patent Information
- Application Number
- CN202210890698.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-07-27
AI Technical Summary
The preparation process of existing black phosphorus-carbon composite materials is complex and costly, which limits their application in lithium/sodium ion batteries. Moreover, there are large differences in the structure and properties of materials prepared by different synthesis methods, which affects their application in the energy field. promotion.
Amorphous red phosphorus and conductive carbon materials are ball milled under a protective atmosphere to form a red phosphorus-carbon material mixture, and then reacted in the next step under high temperature and high pressure conditions to prepare black phosphorus-carbon composite materials, forming a composite with high crystallinity and high covalent P-C bonds. materials, simplifying processes and reducing costs.
It achieves the suppression of volume expansion of black phosphorus during the charge and discharge process of lithium/sodium ion batteries, maintains stable charge and discharge cycle performance, and the preparation method is simple and controllable, making it suitable for popularization and application.
Smart Images

Figure BDA0003767410190000051 
Figure BDA0003767410190000061 
Figure BDA0003767410190000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano functional materials, and specifically relates to a black phosphorus-carbon composite material and a preparation method and application thereof. Background Art
[0002] Black phosphorus (BP), as a new type of two-dimensional semiconductor material, has a high theoretical specific capacity (2596mAh / g) and high conductivity (300S / m), and has been widely studied as an anode material in lithium / sodium ion batteries. However, BP undergoes a huge volume expansion during the charge and discharge process, resulting in rapid capacity decay, which hinders its widespread application. Carbon materials are usually used as skeletons for loading high-capacity active materials in secondary ion batteries due to their low cost, good stability and excellent electronic conductivity. The high specific surface area of carbon materials helps to increase the mass load of active materials, and the pore structure is conducive to adapting to the volume change of electrode materials during the charge and discharge process, thereby increasing the charge and discharge cycle performance of active materials. Therefore, based on the excellent properties of black phosphorus and carbon materials, the two are combined to form a black phosphorus-carbon composite material, which can effectively inhibit the huge volume expansion of black phosphorus during the charge and discharge process, improve Coulomb efficiency and inhibit specific capacity decay.
[0003] At present, in the process of synthesizing black phosphorus-carbon composite materials, black phosphorus and various carbon materials are usually used as starting materials. For example, in patent CN110498404B, black phosphorus-carbon nanotube composite materials are synthesized using red phosphorus and carbon nanotubes as starting materials. However, this method is mainly derived from the method of synthesizing black phosphorus by Stefan Lange et al. (S. Lange, P. Schmidt, T. Nilges., Inorganic Chemistry, 2007, 47, 4028-4035.) and is improved. Moreover, the composite material synthesized by this method has a large particle size, which is not conducive to application in lithium / sodium ion batteries; Park et al. (Park. CM, Sohn. HJ, Advanced Materials, 2007, 19, 2465-2468.) first synthesize black phosphorus by ball milling using red phosphorus as the starting material, and then compound black phosphorus and superconducting carbon black by ball milling to obtain a black phosphorus-carbon composite material; Jin et al. (H.Jin, S.Xin, C.Chuang, W.Li, H.Wang, J.Zhu, H.Xie, T.Zhang, Y.Wan, Z.Qi, W.Yan, Y.-R.Lu, T.-S.Chan, X.Wu, JBGoodenough, H.Ji, X.Duan., Science, 2020, 370, 192-197.) Black phosphorus is first synthesized by chemical vapor transport, and then the prepared black phosphorus and graphite are ball-milled to synthesize black phosphorus-carbon composite materials. The black phosphorus used in these preparation processes must first be prepared by various methods, and the preparation processes involved are relatively complicated and costly, which is not conducive to the promotion and application of black phosphorus-carbon composite materials in the energy field. In addition, there are differences between black phosphorus prepared by different synthesis methods, resulting in large differences in the structure and properties of black phosphorus-carbon composite materials synthesized using black phosphorus and carbon materials as initial materials. Therefore, there is an urgent need to further develop an efficient, low-cost, stable and controllable preparation process of black phosphorus-carbon composite materials, apply them to lithium / sodium ion battery anode materials, and then promote their popularization and application in the energy field. Summary of the invention
[0004] The main purpose of the present invention is to provide a method for preparing a black phosphorus-carbon composite material in view of the problems and shortcomings of the prior art. The method uses low-cost amorphous red phosphorus and conductive carbon materials as raw materials, and realizes the preparation of black phosphorus and its composite with carbon materials through a one-step reaction. The black phosphorus in the obtained composite material has high crystallinity and high content of covalent PC bonds, which is beneficial to inhibiting the volume expansion of black phosphorus during the charging and discharging process of lithium / sodium ion batteries, and effectively maintains stable charging and discharging cycle performance. The preparation method involved is simple, the synthesis reaction is controllable, the cost is low, and it is suitable for popularization and application.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a black phosphorus-carbon composite material comprises the following steps:
[0007] 1) preparing a red phosphorus-carbon material mixture;
[0008] ball-milling amorphous red phosphorus and conductive carbon material under a protective atmosphere to obtain a red phosphorus-carbon material mixed raw material;
[0009] 2) Sample assembly;
[0010] The obtained red phosphorus-carbon material mixed raw material is pressed into shape; the obtained block sample is placed in a high temperature and high pressure assembly;
[0011] 3) Preparation of black phosphorus-carbon composite materials under high temperature and high pressure;
[0012] The sample assembly is placed in a high-temperature and high-pressure device (including a piston cylinder, a six-sided top large press, etc.) for high-temperature and high-pressure reaction; after cooling and reducing the pressure, the sample assembly is taken out, and the pressure transmission medium and the sample cavity of the assembly are removed to obtain the black phosphorus-carbon composite material.
[0013] In the above scheme, the particle size of the amorphous red phosphorus powder is less than 150 μm and the purity is more than 98.9%; the particle size of the conductive carbon material used is less than 20 μm.
[0014] In the above scheme, the conductive carbon material can be selected from one or more of (expandable) graphite, conductive carbon black, carbon nanotubes, (oxidized) graphene, etc. Among them, graphite, as a currently commercial lithium-ion battery anode material, has good stability and low cost, which is conducive to forming a composite material with black phosphorus for use in lithium / sodium ion batteries.
[0015] In the above scheme, the mass ratio of the amorphous red phosphorus to the conductive carbon material is (4-1):1.
[0016] In the above scheme, the protective atmosphere is argon or the like.
[0017] In the above scheme, the ball milling step adopts a dry powder ball milling process, the ball-to-material ratio adopted is (20-60):1, the rotation speed is 200-600r / min, and the ball milling time is 20-120h.
[0018] Preferably, during the ball milling process, the ball milling is performed for 30 to 60 minutes and then stopped for 5 to 10 minutes.
[0019] Preferably, the ball-to-material ratio is (30-50):1.
[0020] Preferably, the rotation speed is 520-600 r / min.
[0021] Preferably, the ball milling time is 30 to 50 hours.
[0022] In the above scheme, the pressure used in the compression molding step is 3 to 7 MPa and the time is 10 to 30 seconds.
[0023] In the above scheme, the high temperature and high pressure reaction step adopts a pressure of 1.0 to 3.0 GPa, a temperature of 600 to 1000° C., a heating rate of 25 to 100° C. / min, and a holding time of 5 to 30 min.
[0024] In the above scheme, the cooling rate used in step 3) is 25°C / min or a quenching process (directly stopping the temperature control system) is used for cooling, wherein the heating, insulation and cooling processes are all in the high pressure holding stage.
[0025] The black phosphorus-graphite composite material prepared according to the above scheme has a lamellar structure and can form a relatively high content of stable covalent PC bonds (the PC bond content can reach 13.68%); when used as an electrode material, it can exhibit high electrochemical activity and stability.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1) The present invention uses amorphous red phosphorus and conductive carbon materials as starting materials, firstly performs ball milling (and regulates the ball milling process) to form a red phosphorus-carbon material mixture, and at the same time increases the degree of graphite disorder; then the obtained mixed raw materials react under high temperature and high pressure conditions to simultaneously achieve the synthesis of black phosphorus and its composite with carbon materials; wherein, in the phase transition process from red phosphorus to black phosphorus, it is more conducive for black phosphorus and carbon materials to interact to form covalent PC bonds, thereby forming a black phosphorus-carbon composite material with stable covalent PC bonds;
[0028] 2) The raw materials involved in the present invention are low in cost and easy to obtain, the preparation method is one-step and simple to operate, the synthesis conditions are stable and controllable, and the high-temperature and high-pressure preparation process can be repeated on various high-temperature and high-pressure devices, which is suitable for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The scanning electron microscope images of the black phosphorus-graphite composite materials obtained in Examples 1 and 2 of the present invention;
[0030] Figure 2 The X-ray diffraction patterns of the starting materials red phosphorus, graphite, the red phosphorus-graphite mixture of the embodiment (RP-G-6) and the red phosphorus-graphite mixture of the comparative example (RP-G-9) of the present invention;
[0031] Figure 3 The Raman spectra of the starting materials red phosphorus, graphite, the red phosphorus-graphite mixture of the embodiment (RP-G-6) and the red phosphorus-graphite mixture of the comparative example (RP-G-9) of the present invention are shown;
[0032] Figure 4 The X-ray diffraction patterns of the black phosphorus of the present invention, the black phosphorus-graphite composite material of Example 10 (BP-G-10), and the black phosphorus-graphite composite material of Comparative Example 5 (BP-G-16);
[0033] Figure 5 The Raman spectra of the graphite of the present invention, the black phosphorus-graphite composite material of Example 10 (BP-G-10), and the black phosphorus-graphite composite material of Comparative Example 5 (BP-G-16);
[0034] Figure 6 This is an X-ray photoelectron spectrum of the black phosphorus-graphite composite material obtained in Example 6 of the present invention.
[0035] Figure 7 This is an X-ray photoelectron spectrum of the black phosphorus-graphite composite material obtained in Example 11 of the present invention.
[0036] Figure 8 The constant current charge-discharge cycle curve of a lithium-ion battery prepared using the black phosphorus-graphite composite material obtained in Example 8 of the present invention;
[0037] Fig. 9 The constant current charge-discharge cycle curve of a lithium-ion battery prepared using the black phosphorus-graphite composite material obtained in Comparative Example 7 of the present invention;
[0038] Fig.10 This is a graph showing the electrochemical performance of a sodium ion battery prepared using the black phosphorus-graphite composite material obtained in Example 11 of the present invention. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is further described below by specific implementation methods. To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments and comparative examples of the present invention are as follows.
[0040] In the following examples and comparative examples, the amorphous red phosphorus powder used has a particle size of less than 150 μm and a purity of more than 98.9%; the conductive carbon material used is natural graphite powder, whose particle size is less than 20 μm.
[0041] In the following examples, a piston-cylinder device was used to carry out high temperature and high pressure synthesis experiments, wherein:
[0042] The cylindrical samples obtained by pre-pressing have two sizes:
[0043] 1) Height 12mm, diameter 6mm, corresponding to the synthesis experiment of pressure 1.5GPa;
[0044] 2) Height 10mm, diameter 4mm, corresponding to the synthesis experiment of pressure 3.0GPa.
[0045] Boron nitride sample chambers are available in two sizes:
[0046] 1) Height 14mm, outer diameter 8mm, corresponding to the synthesis experiment of pressure 1.5GPa;
[0047] 2) Height 12mm, outer diameter 6mm, corresponding to the synthesis experiment of pressure 3.0GPa.
[0048] The cylindrical sample assemblies are available in two sizes:
[0049] 1) Outer diameter 19mm, corresponding to the synthesis experiment of pressure 1.5GPa;
[0050] 2) Synthesis experiment with an outer diameter of 13 mm and a corresponding pressure of 3.0 GPa.
[0051] Piston-cylinder unit pressure plates are available in two sizes:
[0052] 1) Synthesis experiment with an inner diameter of 19 mm and a corresponding pressure of 1.5 GPa;
[0053] 2) Synthesis experiment with inner diameter of 13 mm and corresponding pressure of 3.0 GPa.
[0054] All reagents or instruments without indicating the manufacturer are commercially available products.
[0055] Examples 1 to 11
[0056] The method for preparing the black phosphorus-graphite composite material described in Examples 1 to 11, the process parameters involved in step 1) are shown in Table 1; the process parameters involved in step 3) are shown in Table 2; specifically, the following steps are included:
[0057] 1) Preparation of red phosphorus-graphite mixture
[0058] Weigh amorphous red phosphorus and graphite raw materials in a mass ratio of 8:2 (4:1), 7:3 (2.33:1), 6:4 (1.5:1), and 5:5 (1:1), respectively, put them into a zirconia ball mill, add zirconia balls, fill with argon gas, and then grind and mix them on a planetary ball mill to obtain a red phosphorus-graphite mixture;
[0059] The ball milling process adopts dry powder ball milling technology, the set ball-to-material ratio is (30-60):1, the rotation speed is 520-600r / min, and the ball milling time is 20-120h; during the ball milling process, each ball milling is 30min and the static stop is 5min;
[0060] 2) Sample assembly
[0061] The red phosphorus-graphite mixture obtained in step 1) is pressed into a cylindrical sample by a tablet press (pressure of 3-7 MPa, time of 10-30 s); the obtained pre-pressed cylindrical sample is placed in a hexagonal boron nitride sample bin; the hexagonal boron nitride sample bin containing the sample is placed in a graphite furnace, a porous magnesium oxide column is placed at the upper end, and a solid magnesium oxide column is placed at the lower end, the sample bin is in the middle of the graphite furnace, a heat-resistant glass tube and a talc tube are sequentially placed outside the graphite furnace, and a graphite sheet is placed at the bottom to obtain a cylindrical sample assembly; wherein a porous magnesium oxide column is placed above the boron nitride sample bin to facilitate the insertion of a thermocouple for temperature measurement;
[0062] 3) Preparation of black phosphorus-graphite composites by high temperature and high pressure
[0063] Assembling the cylindrical sample obtained in step 2) and wrapping it with a layer of lead foil, the cylindrical sample is placed in a piston cylinder device for high temperature and high pressure reaction; taking out the sample after high temperature and high pressure treatment, removing the boron nitride on the surface of the sample, and obtaining a black phosphorus-graphite composite material;
[0064] Among them, the high-temperature and high-pressure synthesis experiment pressure is 1.5GPa and 3.0GPa, the temperature is 800 and 1000℃; the heating rate is 25-100℃ / min; the holding time is 5-30min; the cooling rate is 25℃ / min or rapid quenching (directly stop the temperature control system) is used for cooling. The heating, holding and cooling processes all maintain high-pressure holding conditions. After the cooling stage, the pressure is reduced after the oil pressure of the high-temperature and high-pressure device is stable.
[0065] Table 1 Process parameters for preparing red phosphorus-graphite mixture in Examples 1 to 11
[0066] serial number Mass ratio of red phosphorus to graphite Ball to Material Ratio Ball milling time (h) Speed (r / min) RP-G-1 7:3 30:1 20 520 RP-G-2 7:3 40:1 40 600 RP-G-3 7:3 60:1 40 600 RP-G-4 8:2 60:1 40 600 RP-G-5 7:3 40:1 120 600 RP-G-6 6:4 40:1 40 600 RP-G-7 5:5 40:1 40 600
[0067] Table 2 Preparation process parameters of black phosphorus-graphite composite materials described in Examples 1 to 11
[0068]
[0069] Comparative Examples 1 to 8
[0070] The preparation method of the black phosphorus-graphite composite material described in Comparative Examples 1 to 8, the process parameters involved in step 1) are shown in Table 3; the process parameters involved in step 3) are shown in Table 4; specifically include the following steps:
[0071] 1) Preparation of red phosphorus-graphite mixture
[0072] Weigh amorphous red phosphorus and graphite raw materials in a mass ratio of 8:2 (4:1), 7:3 (2.33:1), and 5:5 (1:1), put them into a zirconia ball mill, add zirconia balls, fill with argon gas, and then grind and mix them on a planetary ball mill to obtain a red phosphorus-graphite mixture;
[0073] The ball milling process adopts dry powder ball milling technology, the ball-to-material ratio is set to 20:1 or 40:1, the rotation speed is 400r / min or 600r / min, and the ball milling time is 20h; during the ball milling process, each ball milling is 30min and the static stop is 5min;
[0074] 2) Sample assembly
[0075] The red phosphorus-graphite mixture obtained in step 1) is pressed into a cylindrical sample by a tablet press (pressure of 3-7 MPa, time of 10-30 s); the obtained pre-pressed cylindrical sample is placed in a hexagonal boron nitride sample bin; the hexagonal boron nitride sample bin containing the sample is placed in a graphite furnace, a porous magnesium oxide column is placed at the upper end, and a solid magnesium oxide column is placed at the lower end, the sample bin is in the middle of the graphite furnace, a heat-resistant glass tube and a talc tube are sequentially placed outside the graphite furnace, and a graphite sheet is placed at the bottom to obtain a cylindrical sample assembly; wherein a porous magnesium oxide column is placed above the boron nitride sample bin to facilitate the insertion of a thermocouple for temperature measurement;
[0076] 3) Preparation of black phosphorus-graphite composites by high temperature and high pressure
[0077] Assembling the cylindrical sample obtained in step 2) and wrapping it with a layer of lead foil, the cylindrical sample is placed in a piston cylinder device for high temperature and high pressure reaction; taking out the sample after high temperature and high pressure treatment, removing the boron nitride on the surface of the sample, and obtaining a black phosphorus-graphite composite material;
[0078] Among them, the high-temperature and high-pressure synthesis experiment pressure is 1.5GPa and 3.0GPa, the temperature is 800-1000℃; the heating rate is 25-100℃ / min; the holding time is 5-60min; the cooling rate is 25℃ / min or rapid quenching (directly stop the temperature control system) is used for cooling. The heating, holding and cooling processes all maintain high-pressure holding conditions. After the cooling stage, the pressure is reduced after the oil pressure of the high-temperature and high-pressure device is stable.
[0079] Table 3 Process parameters for preparing red phosphorus-graphite mixture in Comparative Examples 1 to 8
[0080] serial number Mass ratio of red phosphorus to graphite Ball to Material Ratio Ball milling time (h) Speed (r / min) RP-G-8 8:2 20:1 20 400 RP-G-9 7:3 20:1 20 400 RP-G-10 5:5 40:1 20 600
[0081] Table 4 Preparation process parameters of the black phosphorus-graphite composite materials described in Comparative Examples 1 to 8
[0082]
[0083]
[0084] The black phosphorus-graphite composite materials obtained in the above-mentioned embodiments and comparative examples are respectively used to prepare lithium-ion batteries. The specific preparation steps include: (1) weighing black phosphorus-graphite composite materials, superconducting carbon black (Super P) and polyvinylidene fluoride (PVDF) according to a mass ratio of 70:15:15, and mixing them into slurry using N-methylpyrrolidone (NMP) as a solvent; (2) coating the mixed slurry on a copper foil and drying it in a vacuum drying oven at 60° C. for 12 h; (3) cutting the dried electrode into a circular size with a diameter of 12 mm, and the loading amount of the electrode is 1.5 to 2.0 mg; (4) assembling a half-cell in a glove box, the battery housing model is CR2032, the separator used is Celgard 2400, and the electrolyte is 1MLiPF6+EC / DEC (v:v=1:1). The constant current charge and discharge experiment was carried out at a current density of 0.13 A / g and a voltage range of 0.001 V-2.5 V. The electrochemical performance test results of the obtained lithium-ion battery are shown in Table 5.
[0085] It can be seen from the table that the Coulombic efficiency of Examples 1-11 increases successively from the first cycle to the second cycle, while the Coulombic efficiency of the comparative example decreases successively, and after 5 cycles, the reversible specific capacity of the examples is greater than the reversible specific capacity of the comparative example.
[0086] Table 5 Cyclic test results of lithium-ion batteries obtained using the composite materials described in the examples and comparative examples
[0087]
[0088]
[0089] The black phosphorus-graphite composite material obtained in Example 11 is used to prepare a sodium ion battery. The specific preparation steps include: (1) weighing the black phosphorus-graphite composite material, superconducting carbon black (Super P) and polyvinylidene fluoride (PVDF) in a mass ratio of 70:15:15, and mixing them into a slurry using N-methylpyrrolidone (NMP) as a solvent; (2) coating the mixed slurry on a copper foil, and drying it in a vacuum drying oven at 60° C. for 12 h; (3) cutting the dried electrode into a circular size of 12 mm in diameter, and the loading amount of the electrode is 1.5 to 2.0 mg; (4) assembling a half-cell in a glove box, the battery shell model is CR2032, the diaphragm used is a glass fiber diaphragm (GF / D), and the electrolyte is 1MNaClO4+PC (100%)+5%FEC. The constant current charge and discharge experiment was carried out at a current density of 0.13A / g and a voltage range of 0.001-2.5V. The electrochemical performance test results of the obtained sodium ion battery are as follows Fig.10As shown, the initial coulombic efficiency of the obtained black phosphorus-graphite composite material in the half-cell constant current charge and discharge cycle test is as high as 68.22%, and the discharge specific capacity after 50 cycles is 341.6 mAh / g, indicating that the black phosphorus-graphite composite material synthesized by the present invention is suitable for preparing sodium ion batteries.
[0090] The scanning electron microscope photos of the black phosphorus-graphite composite materials obtained in Examples 1 and 2 are as follows: Figure 1 As shown, the obtained black phosphorus-graphite composite material exhibits lamellar structural characteristics.
[0091] The X-ray diffraction patterns of the red phosphorus-graphite mixture RP-G-6 obtained in the present invention and the red phosphorus-graphite mixture RP-G-9 obtained in the comparative example are as follows: Figure 2 As shown, the Raman spectrum is Figure 3 The results show that the red phosphorus powder is still amorphous after ball milling; the relative intensity of the D peak and the G peak of the graphite powder after ball milling (I D / I G The red phosphorus-graphite mixture RP-G-6 obtained by the present invention has a greater change, which is conducive to promoting more disordered red phosphorus and graphite.
[0092] The X-ray diffraction patterns of the black phosphorus-graphite composite material (BP-G-10) obtained in Example 10 and the black phosphorus-graphite composite material (BP-G-16) obtained in Comparative Example 5 are as follows: Figure 4 As shown, the Raman spectrum is Figure 5 The results show that: after the high temperature and high pressure treatment in step 3), the red phosphorus in the mixed raw material is converted into black phosphorus, and the black phosphorus has high crystallinity; the graphite characteristic peak intensity ratio of the black phosphorus-graphite composite material is D / I G Relative to the I of graphite in the mixed raw material D / I G Increased, and the graphite I in the black phosphorus-graphite composite material (BP-G-10) of Example 10 D / I G Relative to the graphite in the black phosphorus-graphite composite material of comparative example 5, D / I G The increase is more obvious.
[0093] The above results indicate that interaction occurs between black phosphorus and graphite in the black phosphorus-graphite composite material synthesized under high temperature and high pressure.
[0094] The X-ray photoelectron spectrum of the black phosphorus-graphite composite material obtained in Example 6 is as follows: Figure 6 The results show that covalent PC bonds are formed in the black phosphorus-graphite composite material, and the proportion of PC bonds is 8.92%.
[0095] The X-ray photoelectron spectrum of the black phosphorus-graphite composite material obtained in Example 11 is as follows: Figure 7 The results show that covalent PC bonds are formed in the black phosphorus-graphite composite material, and the proportion of PC bonds is 13.68%.
[0096] The constant current charge and discharge curves of Example 8 and Comparative Example 7 are as follows: Figure 8 and Fig. 9 The results show that Example 8 has better cycle stability and higher reversible specific capacity retention rate.
[0097] Fig.10 This is an electrochemical performance diagram of a sodium ion battery prepared using the black phosphorus-graphite composite material obtained in Example 11 of the present invention. The results show that the initial coulombic efficiency of the obtained black phosphorus-graphite composite material in the half-cell constant current charge and discharge cycle test is as high as 68.22%, and the discharge specific capacity after 50 cycles is 341.6 mAh / g, indicating that the black phosphorus-graphite composite material synthesized by the present invention is suitable for preparing sodium ion batteries.
[0098] The above embodiments and comparative examples are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a black phosphorus-carbon composite material, characterized in that: The steps include: 1) ball milling amorphous red phosphorus and conductive carbon material under a protective atmosphere to obtain a red phosphorus-carbon material mixed raw material; 2) pressing the obtained red phosphorus-carbon material mixture into a shape; placing the obtained block sample into a high-temperature and high-pressure assembly; 3) placing the sample assembly into a high-temperature and high-pressure device for a high-temperature and high-pressure reaction; removing the sample after cooling and reducing the pressure to obtain the black phosphorus-carbon composite material; The conductive carbon material is one or more of graphite, conductive carbon black, and carbon nanotubes; The amorphous red phosphorus is in the form of powder, the particle size of which is less than 150 μm; the particle size of the conductive carbon material is less than 20 μm; The mass ratio of the amorphous red phosphorus to the conductive carbon material is (4-1):1; The ball milling step adopts a dry powder ball milling process, uses argon as a protective atmosphere, adopts a ball-to-material ratio of (30-50):1, a rotation speed of 520-600 r / min, and a ball milling time of 30-50 h, with each ball milling time of 30-60 min and a rest time of 5-10 min; The high temperature and high pressure reaction step adopts a pressure of 1.0-3.0 GPa and a temperature of 600-1000°C.
2. The preparation method according to claim 1, characterized in that The pressure used in the compression molding step is 3-7 MPa and the time is 10-30 s.
3. The preparation method according to claim 1, characterized in that The high temperature and high pressure reaction step adopts a heating rate of 25-100°C / min and a holding time of 5-30 min.
4. The preparation method according to claim 1, characterized in that In step 3), the cooling rate is 25°C / min or a quenching process is used for cooling; the heating, holding, and cooling processes all maintain high pressure holding conditions. After the cooling stage is completed, the pressure is reduced after the oil pressure of the high temperature and high pressure device stabilizes.
5. The black phosphorus-carbon composite material prepared by the preparation method according to any one of claims 1 to 4.
6. Application of the black phosphorus-carbon composite material according to claim 5 in the field of lithium / sodium ion batteries.
Citation Information
Patent Citations
A method for in-situ preparation of black phosphorus-carbon nanotube composite materials
CN110498404B
Epoxy resin composition and semiconductor device
JP2000319488A
Method for preparing black Phosphorus and black Phosphorus-carbon composites, the prepared black Phosphorus and black Phosphorus-carbon composites and lithium rechargeable battery comprising the same and method for using the rechargeable battery
KR100788487B1
Method for preparing black phosphorus or black phosphorus-carbon composite, lithium rechargeable battery comprising the prepared black phosphorus or black phosphorus-carbon composite and method for using the rechargeable battery
US20080038626A1