Hollow particles, resin composition, and resin molded product and laminate using the same

By using plate-shaped hollow particles with an aspect ratio of 2 or more and a resin composition to form a resin molded body and a laminated body, the problem of balancing durability and low dielectric constant in the existing technology is solved, and the weight of electronic components is realized. and improved dielectric properties.

CN115175873BActive Publication Date: 2024-10-29SETOLAS HLDG INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202180016759.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-01-25
Publication Date
2024-10-29
Estimated Expiration
2041-01-25

AI Technical Summary

Technical Problem

It is difficult to achieve low dielectric constant and light weight of electronic components while ensuring durability. Especially in high-frequency communications, it is difficult to achieve both low dielectric constant and low dielectric loss tangent of components.

Method used

Using plate-shaped hollow particles with an aspect ratio of 2 or more, such as silica hollow particles, combined with a resin composition to form a resin molded body and a laminate, the hollow particles have a hollow ratio of 20% or more and 95% or less, and the long diameter and thickness are within Within a specific range, the shape and structure of the hollow particles are optimized through surface treatment and manufacturing methods.

Benefits of technology

While ensuring durability and mechanical strength, it achieves low dielectric constant and lightweight, is suitable for miniaturization and thinning of electronic components, and improves the dielectric properties and processability of components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115175873B_ABST
    Figure CN115175873B_ABST
Patent Text Reader

Abstract

The present invention relates to hollow particles, resin compositions, and resin molded products and laminates using the resin compositions. Provided is a hollow particle that achieves low dielectric constant and light weight while ensuring durability. The hollow particle of the present invention contains silicon dioxide, has an aspect ratio of 2 or more, and is plate-shaped.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to hollow particles, a resin composition, and a resin molded body and a laminate using the resin composition. Background Art

[0002] For example, in recent years, in the field of information communication equipment, in order to cope with the communication in the high frequency band, the low dielectric constant and low dielectric loss tangent of electronic components (representatively resin components) are required. In order to achieve this purpose, for example, a scheme of making the component contain air with a low relative dielectric constant is proposed. Specifically, a scheme of using hollow particles to import air is proposed (for example, with reference to patent documentation 1). In this way, by containing air, it is also possible to contribute to the lightweight of the component.

[0003] On the other hand, it is also required to ensure the durability of the member (for example, mechanical strength such as bending modulus, and dimensional stability).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-56158 Summary of the invention

[0007] Problems to be solved by the invention

[0008] The present invention has been made to solve the above-mentioned problems, and one of its objects is to achieve a lower dielectric constant and a lighter weight while ensuring durability.

[0009] Means for solving problems

[0010] According to one aspect of the present invention, there is provided a hollow particle containing silicon dioxide, having an aspect ratio of 2 or more and being in a plate shape.

[0011] In one embodiment, the major diameter of the hollow particles is 0.1 μm or more and 10 μm or less.

[0012] In one embodiment, the thickness of the hollow particles is 0.01 μm or more and 5 μm or less.

[0013] In one embodiment, the shell thickness of the hollow particles is 10 nm or more and 100 nm or less.

[0014] In one embodiment, the hollow particles have a hollow ratio of 20% to 95%.

[0015] According to another aspect of the present invention, a resin composition is provided, which comprises a resin and the above-mentioned hollow particles.

[0016] According to another aspect of the present invention, a resin molded body is provided. The resin molded body is formed from the above resin composition.

[0017] According to another aspect of the present invention, there is provided a laminate having a resin layer formed from the above resin composition.

[0018] In one embodiment, the resin layer has a thickness of 25 μm or less.

[0019] Effects of the Invention

[0020] According to the present invention, by using plate-shaped hollow particles, it is possible to achieve a lower dielectric constant and a lighter weight while ensuring durability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram explaining the major diameter and thickness.

[0022] Figure 2 This is a schematic cross-sectional view of a laminated body in one embodiment of the present invention.

[0023] Figure 3A This is a TEM observation photograph of the hollow particles of Example 1 (magnification 10,000 times).

[0024] Figure 3B This is a TEM observation photograph of the hollow particles of Example 1 (100,000 times).

[0025] Figure 4 This is a SEM observation photograph of the core particles used in Example 1 (magnification 20,000 times). DETAILED DESCRIPTION

[0026] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0027] (Definition of terms)

[0028] The definitions of terms in this specification are as follows.

[0029] 1. The long diameter of the particle

[0030] It is a value measured by observation using a scanning electron microscope (SEM) or a transmission electron microscope (TEM) and is the major diameter of a randomly selected primary particle (e.g., Figure 1 It should be noted that the primary particles refer to the smallest particles observed by SEM or TEM, and are distinguished from agglomerated particles (secondary particles).

[0031] 2. Particle thickness

[0032] is the value measured by SEM or TEM observation and is the thickness of a randomly selected primary particle (e.g. Figure 1 The average value of T).

[0033] 3. Aspect ratio (long diameter / thickness)

[0034] It is a value calculated by dividing the major axis of the particle by the thickness of the particle.

[0035] 4. Particle size

[0036] The particle size is the average particle size in the particle size distribution measurement.

[0037] A. Hollow particles

[0038] The hollow particles according to one embodiment of the present invention are typically formed of silicon dioxide. The content of silicon dioxide in the hollow particles is, for example, 95% by weight or more, preferably 97% by weight or more, and more preferably 98% by weight or more.

[0039] The above-mentioned hollow particles are in the shape of a plate. By adopting a plate-like shape, the above-mentioned durability and low dielectric constant and light weight can be achieved simultaneously. In addition, the miniaturization (filmization) of the components used can also be fully dealt with. And then, it is also easy to achieve a balance between high hollowness and the strength of the hollow particles.

[0040] The aspect ratio of the hollow particles is 2 or more, preferably 3 or more, and more preferably 4 or more. On the other hand, the aspect ratio of the hollow particles is, for example, 100 or less, preferably 60 or less, and more preferably 50 or less. With such an aspect ratio, for example, excellent processability is achieved when preparing a resin composition described later.

[0041] The major diameter of the hollow particles is preferably 0.1 μm or more, more preferably 0.2 μm or more. According to such a major diameter, the hollow ratio described below can be fully satisfied. On the other hand, the major diameter of the hollow particles is preferably 10 μm or less, more preferably 5 μm or less. According to such a major diameter, the above-mentioned miniaturization (thin film) can be greatly contributed.

[0042] The thickness of the hollow particles is preferably 0.01 μm or more, more preferably 0.05 μm or more, and particularly preferably 0.1 μm or more. According to such a thickness, the hollow ratio described below can be fully satisfied. On the other hand, the thickness of the hollow particles is preferably 5 μm or less, more preferably 3 μm or less, and particularly preferably 2 μm or less. According to such a thickness, the above-mentioned miniaturization (thin film) can be greatly contributed.

[0043] The thickness of the shell of hollow particle is preferably more than 10nm, more preferably more than 15nm. According to such thickness, for example, when making resin combination described later, hollow particle can be effectively prevented from being destroyed. On the other hand, the thickness of the shell of hollow particle is preferably less than 100nm, more preferably less than 60nm. According to such thickness, the hollow ratio described later can be fully satisfied, and low dielectric constant and light weight can be greatly contributed. It should be noted that the thickness of shell can be measured by TEM observation. For example, by measuring the thickness of the shell of randomly selected hollow particle and calculating its average value to obtain.

[0044] The hollow ratio of the hollow particles is preferably 20% or more, more preferably 30% or more, further preferably 40% or more, and particularly preferably 50% or more. Such a hollow ratio can, for example, greatly contribute to low dielectric constant and light weight. On the other hand, the hollow ratio of the hollow particles is preferably 95% or less, further preferably 90% or less. Such a hollow ratio can, for example, effectively prevent the hollow particles from being destroyed when making a resin composition described later. It should be noted that the hollow ratio can be calculated based on the volume of the core particles described later and the volume of the hollow particles.

[0045] The pore volume of the hollow particles is preferably 1.5 cm 3 / g or less, more preferably 1.0 cm 3 / g or less.

[0046] The particle size of the hollow particles is preferably 0.1 μm or more, and more preferably 0.5 μm or more. On the other hand, the particle size of the hollow particles is preferably 10 μm or less, and more preferably 5 μm or less.

[0047] The BET specific surface area of ​​the hollow particles can be, for example, 10 m 2 / g or more, can also be 30m 2 On the other hand, the BET specific surface area of ​​the hollow particles is preferably 250 m 2 / g or less, more preferably 200m 2 / g or less.

[0048] In one embodiment, the hollow particles are subjected to surface treatment using any appropriate surface treatment agent. As the surface treatment agent, for example, at least one selected from higher fatty acids, anionic surfactants, cationic surfactants, phosphates, coupling agents, esters of polyols and fatty acids, acrylic polymers, and silicone treatment agents is used.

[0049] Any appropriate method may be adopted as a method for producing the hollow particles. In one embodiment, the method for producing the hollow particles includes: coating core particles with a shell-forming material to obtain core-shell particles; and removing the core particles from the core-shell particles.

[0050] As the above-mentioned core particle, any appropriate particle can be used as long as the above-mentioned hollow particle can be manufactured. Specifically, the shape of the core particle is preferably plate-like. The aspect ratio of the core particle is preferably more than 2, and more preferably more than 3. On the other hand, the aspect ratio of the core particle is preferably less than 100, and more preferably less than 70.

[0051] The major diameter of the core particle is preferably 0.1 μm or more, more preferably 0.2 μm or more. On the other hand, the major diameter of the core particle is preferably 10 μm or less, more preferably 5 μm or less. The thickness of the core particle is preferably 0.01 μm or more, more preferably 0.1 μm or more. On the other hand, the thickness of the core particle is preferably 5 μm or less, more preferably 2 μm or less.

[0052] As the formation material of the core particle, for example, a material that can be dissolved in an acidic solution described later is used. In this case, as the formation material of the core particle, for example, carbonate compounds such as hydroxides such as magnesium hydroxide, hydrotalcite, magnesium oxide, calcium hydroxide, oxides such as hydrotalcite, zinc oxide, calcium oxide, and calcium carbonate can be cited. Among them, magnesium hydroxide and hydrotalcite are preferably used, and magnesium hydroxide is particularly preferably used. The reason is that, for example, it can stably exist in an aqueous system. In addition, the reason is that when it is dissolved in an acidic solution described later, no gas (such as carbon dioxide) is produced, and defects can be suppressed in the hollow particles obtained.

[0053] As the shell-forming material, for example, water glass (Na2O·nSiO2) or alkoxysilane represented by tetraethoxysilane (Si(OCH2CH3)4) is used.

[0054] The coating amount produced by the shell forming material can be adjusted by any appropriate method. For example, the coating amount can be adjusted by controlling the pH value when the core particles are covered with a shell forming material containing water glass. Specifically, the water glass can be stable in a high pH region (for example, above pH 11). Therefore, for example, by using a pH adjusting agent to reduce the pH value (for example, to below pH 7), the water glass molecules are condensed, and silicon dioxide can be efficiently precipitated on the core particles. As a pH adjusting agent, an acidic solution is preferably used. Specifically, a solution of a strong acid such as hydrochloric acid, nitric acid, and sulfuric acid, and a solution of a weak acid such as ammonium nitrate and ammonium sulfate are preferably used. The amount of the pH adjusting agent added is preferably set to 85% to 98% relative to the neutralization rate of water glass. If the neutralization rate is too high, not only silicon dioxide is precipitated on the core particles, but also separate silicon dioxide particles may be generated. In addition, when the shell forming material is used for coating, it is possible to dissolve the core particles. In addition, by heating (for example, 80° C. to 90° C.) when the core particles are covered with the shell-forming material, the formation of the shell (specifically, the precipitation and formation rate of the shell) can also be accelerated.

[0055] The removal of the core particles is typically performed by dissolving the core particles in an acidic solution. As the acidic solution, for example, hydrochloric acid, sulfuric acid, or nitric acid is used. The dissolution temperature is, for example, 30°C to 90°C, preferably 50°C to 70°C. According to such a temperature, the core particles can be efficiently dissolved while suppressing undesirable situations such as the shell becoming easily damaged. In one embodiment, for example, from the viewpoint of reusing a substance (such as a salt) obtained by reacting with the core particles, hydrochloric acid is used as the acidic solution.

[0056] Preferably, the method for manufacturing the hollow particles further comprises calcining the shell (e.g., in an atmospheric atmosphere). By calcining, for example, the hydrophobicity of the shell can be improved (specifically, the silanol groups of the shell are changed into siloxanes), thereby improving the dielectric properties of the obtained hollow particles. Calcination can be performed at any appropriate time. It is preferably performed after the core particles are removed from the core-shell particles. The calcining temperature is, for example, 300° C. to 1300° C. The calcining time is, for example, 1 hour to 20 hours.

[0057] In one embodiment of the present invention, the hollow particles are used as a function-imparting agent for a resin material. Hereinafter, a resin composition containing the hollow particles will be described.

[0058] B. Resin composition

[0059] A resin composition according to one embodiment of the present invention contains a resin and the above-mentioned hollow particles.

[0060] The above-mentioned resin can select any appropriate resin according to the purpose of the obtained resin composition, for example. For example, the resin can be a thermoplastic resin or a thermosetting resin. As specific examples of the resin, epoxy resin, polyimide resin, polyamide resin, polyamide-imide resin, polyether-ether-ketone resin, polyester resin, polyhydroxy polyether resin, polyolefin resin, fluororesin, liquid crystal polymer, modified polyimide can be cited. They can be used alone or in combination of two or more.

[0061] The content of the hollow particles in the resin composition is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, while the content is preferably 90% by weight or less, more preferably 85% by weight or less.

[0062] The resin composition preferably contains 0.5 parts by weight or more of hollow particles, more preferably 1 part by weight or more, relative to 100 parts by weight of the resin. On the other hand, preferably contains 300 parts by weight or less of hollow particles, more preferably 200 parts by weight or less, relative to 100 parts by weight of the resin.

[0063] The volume ratio of the hollow particles in the resin composition is preferably 0.1% or more, and more preferably 0.5% or more. On the other hand, the volume ratio of the hollow particles in the resin composition is preferably 70% or less, and more preferably 60% or less. The reason is, for example, excellent processability when making the resin composition.

[0064] The resin composition may contain optional components. As optional components, for example, a curing agent (specifically, a curing agent for the resin), a low stress agent, a colorant, a close fit enhancer, a release agent, a flow regulator, a defoaming agent, a solvent, and a filler may be listed. They may be used alone or in combination of two or more. In one embodiment, the resin composition includes a curing agent. The content of the curing agent is, for example, 1 to 150 parts by weight relative to 100 parts by weight of the resin.

[0065] As the preparation method of the above-mentioned resin combination, any appropriate method can be adopted. Specifically, the above-mentioned hollow particles are dispersed in the above-mentioned resin by adopting any appropriate dispersion method, thereby obtaining the resin combination. As the dispersion method, for example, the dispersion using various agitators such as a homomixer, a disperser, and a ball mill, the dispersion using a rotation and revolution mixer, the dispersion using the shear force of a triple roller, and the dispersion using ultrasonic treatment can be cited.

[0066] For the above-mentioned resin combination, it is representatively a resin molded body formed into a desired shape. For example, a resin molded body of a desired shape is formed using a mold. When the resin molded body is formed, any appropriate treatment (such as curing treatment) can be implemented to the resin combination.

[0067] In one embodiment of the present invention, the resin composition is a resin layer contained in a laminate. The laminate having a resin layer formed of the resin composition is described below.

[0068] C. Laminated body

[0069] Figure 2 1 is a schematic cross-sectional view of a laminate in one embodiment of the present invention. The laminate 10 has a resin layer 11 and a metal foil 12. The resin layer 11 is formed by the above-mentioned resin composition. Specifically, the resin layer 11 contains the above-mentioned resin and the above-mentioned hollow particles. In the resin layer 11, the in-plane direction of the plate-like hollow particles is preferably oriented in the in-plane direction of the resin layer 11. This is because it can contribute to the thin filmization of the resin layer. Although not shown, the laminate 10 may include other layers. For example, a substrate (representatively a resin film) laminated on one side of the resin layer 11 (the side where the metal foil 12 is not configured) can be cited. The laminate 10 is typically used as a wiring circuit substrate.

[0070] The thickness of the resin layer is, for example, 5 μm or more, preferably 10 μm or more. On the other hand, the thickness of the resin layer is, for example, 100 μm or less, preferably 50 μm or less, and more preferably 25 μm or less. Such a thickness can fully cope with the miniaturization of electronic components in recent years.

[0071] As the metal forming the metal foil, any appropriate metal can be used. For example, copper, aluminum, nickel, chromium, and gold can be mentioned. These can be used alone or in combination of two or more. The thickness of the metal foil is, for example, 2 μm to 35 μm.

[0072] As a method for making the above-mentioned laminate, any appropriate method can be used. For example, the above-mentioned resin composition is applied to the above-mentioned substrate to form a coating layer, and the above-mentioned metal foil is stacked on the coating layer to obtain a laminate. As another specific example, the above-mentioned metal foil is applied to the above-mentioned resin composition to form a coating layer to obtain a laminate. Representatively, the coating layer is subjected to treatments such as heating or light irradiation at any appropriate time to cure the coating layer. When applying, the above-mentioned resin composition can be dissolved in any appropriate solvent for use.

[0073] Example

[0074] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples. It should be noted that, unless otherwise specified, the measuring methods of various properties are as follows.

[0075] 1. The long diameter of the particle

[0076] The major diameter is calculated by SEM observation or TEM observation. Specifically, the major diameters of 100 primary particles randomly selected from the SEM photo or TEM photo of the particle are measured, and the arithmetic mean (average major diameter) of the obtained measured values ​​is obtained. It should be noted that the magnification of the SEM observation of the core particle is set to 20000 times, and the magnification of the TEM observation of the hollow particle is set to 10000 times.

[0077] 2. Thickness

[0078] The thickness of the particle and the thickness of the shell of the particle are calculated by SEM observation or TEM observation. Specifically, the thickness of 100 primary particles randomly selected from the SEM photo or TEM photo of the particle is measured, and the arithmetic mean (average thickness) of the obtained measured value is obtained. It should be noted that the magnification of the SEM observation of the core particle is set to 50000 times, and the magnification of the TEM observation of the hollow particle is set to 10000 times and 10000 times.

[0079] 3. Aspect Ratio

[0080] The aspect ratio is calculated by SEM observation or TEM observation. Specifically, the aspect ratio is calculated by dividing the average major diameter of the particles by the average thickness of the particles.

[0081] 4. Hollowness

[0082] It is calculated from the volume of the core particles and the volume of the hollow particles. Specifically, it is calculated by (the volume of each core particle) / (the volume of each hollow particle)×100. It should be noted that the volume of each particle of the core particles and the hollow particles is calculated as follows: the actual shape is approximated by the volume of a cylinder, the major diameter is taken as the diameter of the circle, and the thickness is taken as the height of the cylinder.

[0083] 5. Particle size

[0084] The particle size (average secondary particle size) was measured by dynamic light scattering using "ELSZ-2" manufactured by Otsuka Electronics (analysis condition: scattering intensity distribution). The measurement sample was prepared by adding 0.05 g of particles to 70 mL of water and then subjecting the mixture to ultrasonic treatment at 300 μA for 3 minutes.

[0085] 6. Pore volume

[0086] The pore volume was measured using "BELsorp-max" manufactured by Microtrac Bell Co., Ltd. Specifically, the pore volume was measured by a constant volume gas adsorption method using nitrogen gas, and the pore volume was determined by analysis based on the BJH method.

[0087] 7.BET specific surface area

[0088] The surface area was measured using "BELsorp-mini" manufactured by Microtrac Bell Co., Ltd. Specifically, the surface area was measured by a constant volumetric gas adsorption method using nitrogen gas, and the specific surface area was determined by analysis based on a BET multipoint method.

[0089] [Example 1]

[0090] Plate-shaped magnesium hydroxide particles having a major diameter of 0.8 μm, a thickness of 0.2 μm, and an aspect ratio of 4 were adjusted to a solid content concentration of 60 g / L using ion-exchanged water to obtain a magnesium hydroxide slurry.

[0091] Next, the slurry of magnesium hydroxide obtained was heated to 80°C while stirring 6.7L, and 268ml of No. 3 water glass (Na2O·3.14SiO2, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) of 0.57mol / L was added thereto over 10 minutes. Then, 1340ml of No. 3 water glass and 3.25L of 0.5N hydrochloric acid were added simultaneously. Here, No. 3 water glass was added over 50 minutes, and hydrochloric acid was added over 60 minutes. After aging the slurry thus obtained for 30 minutes, it was dehydrated and washed with water to obtain a filter cake of the core-shell particle precursor.

[0092] Next, the obtained filter cake of the core-shell particle precursor was adjusted to a solid content concentration of 60 g / L with ion exchange water, heated to 80°C while stirring, and 268 ml of No. 3 water glass of 0.57 mol / L was added thereto over a period of 10 minutes. Then, 670 ml of No. 3 water glass and 1.9 L of 0.5 N hydrochloric acid were added simultaneously. Here, No. 3 water glass was added over a period of 25 minutes, and hydrochloric acid was added over a period of 35 minutes. After aging the slurry thus obtained for 30 minutes, it was dehydrated and washed with water to obtain a filter cake of core-shell particles.

[0093] Here, the obtained core-shell particles were measured by the ATR method using FT-IR ("FT / IR-4100" manufactured by JASCO). As a result, it was confirmed that not only the 3500 to 3800 cm -1 The OH-derived peaks were also confirmed at 1000-1300 cm -1 The nearby peaks are from Si-O-Si.

[0094] Next, 21.6 L of 0.7 N hydrochloric acid was added to the obtained core-shell particles, and the particles were resuspended under stirring at room temperature. After adjusting the solid content concentration of the core-shell particles to 25 g / L, the particles were heated to 60° C. and aged for 1 hour to dissolve the core particles, thereby obtaining a slurry of hollow silica.

[0095] The obtained hollow silica slurry was dehydrated and washed with water to prepare a filter cake of hollow silica, and the filter cake of hollow silica was dried at 60° C. for 28 hours to obtain hollow silica particles (long diameter: 0.86 μm, thickness: 0.26 μm, aspect ratio: 3.3, shell thickness: 30 nm, hollow ratio: 66%, particle size: 0.95 μm, pore volume: 0.67 cm 3 / g, BET specific surface area: 123m 2 / g).

[0096] The obtained hollow silica particles were measured by the ATR method using FT-IR ("FT / IR-4100" manufactured by JASCO). As a result, no spectral distribution of 3500 to 3800 cm-1 of the magnesium hydroxide particles was confirmed. -1 The peaks derived from OH are only confirmed at 1000-1300 cm -1 In addition, the hollow silica particles were analyzed by X-ray diffraction ("EMPYRIAN" manufactured by PANalytical), and the peak of magnesium hydroxide was not confirmed, indicating that it was amorphous silica. Furthermore, based on the weight of the obtained hollow silica particles, the proportion of silica in the core-shell particles was 26% by weight.

[0097] [Example 2]

[0098] When forming core-shell particles, the concentration of hydrochloric acid was changed from 0.5N to 0.52N. Hollow particles (major diameter: 0.88 μm, thickness: 0.28 μm, aspect ratio: 3.1, shell thickness: 40 nm, hollow ratio: 59%, particle size: 1.20 μm, pore volume: 0.50 cm) were obtained in the same manner as in Example 1. 3 / g, BET specific surface area: 81m 2 / g).

[0099] [Example 3]

[0100] Hollow particles (long diameter: 0.246 μm, thickness: 0.116 μm, aspect ratio: 2.1, shell thickness: 23 nm, hollow ratio: 53%, particle size: 0.94 μm, pore volume: 0.85 cm) were obtained in the same manner as in Example 1 except that plate-shaped hydrotalcite ("DHT4" manufactured by Kyowa Chemical Industry Co., Ltd.) with a long diameter of 0.2 μm, a thickness of 0.07 μm, and an aspect ratio of 2.9 was used instead of plate-shaped magnesium hydroxide particles with a long diameter of 0.8 μm, a thickness of 0.2 μm, and an aspect ratio of 4, and that the concentration of hydrochloric acid was changed from 0.5 N to 0.49 N when forming core-shell particles. 3 / g, BET specific surface area: 135m 2 / g).

[0101] <TEM Observation>

[0102] Regarding the hollow particles of Example 1, the observation results obtained using a transmission electron microscope ("JEM-2100PLUS" manufactured by JEOL Ltd.) are shown in Fig. 3. It was confirmed from Fig. 3 that the particles are plate-shaped hollow particles with a shell (silica layer) thickness of 30 nm. Further, in Figure 4 the SEM photograph of the magnesium hydroxide particles used as the core particles is shown, and from Fig. 3 and Figure 4 it was confirmed that the particles are hollow particles maintaining the plate shape of the core particles.

[0103] <Resin Composition>

[0104] (1) Mixing by ultrasonic treatment

[0105] 1 g of bisphenol F type epoxy resin ("JER806" manufactured by Mitsubishi Chemical Corporation), 0.38 g of a curing agent ("LV11" manufactured by Mitsubishi Chemical Corporation), and 0.04 g of the hollow silica particles obtained in Example 1 were mixed to obtain Resin Composition 1. Regarding the mixing, it was carried out by performing ultrasonic treatment for 1 minute using "NS-200-60" manufactured by Nippon Seiki Co., Ltd.

[0106] (2) Mixing using a homogenizer

[0107] 5 g of bisphenol F type epoxy resin ("JER806" manufactured by Mitsubishi Chemical Corporation), 1.9 g of a curing agent ("LV11" manufactured by Mitsubishi Chemical Corporation), and 0.2 g of the hollow silica particles obtained in Example 1 were mixed to obtain Resin Composition 2. Regarding the mixing, it was carried out using a portable homogenizer ("T10 Basic" manufactured by IKA Japan Co., Ltd.) under the conditions of 8000 rpm for 5 minutes.

[0108] (3) Mixing using a rotation-revolution mixer

[0109] 5 g of bisphenol F type epoxy resin ("JER806" manufactured by Mitsubishi Chemical Corporation), 2.5 g of a curing agent ("LV11" manufactured by Mitsubishi Chemical Corporation), and 0.875 g of the hollow silica particles obtained in Example 1 were mixed to obtain Resin Composition 3. Regarding the mixing, it was carried out using a rotation-revolution mixer ("Kakuhunter SK-300SVII" manufactured by Shashin Kagaku Co., Ltd.) under the conditions of 1700 rpm for 3 minutes.

[0110] <Resin Molded Body>

[0111] The resin compositions 1-3 were poured into a silicone resin mold having a thickness of 2 mm, and cured at 80° C. for 3 hours to obtain resin molded bodies 1-3.

[0112] The obtained molded body was cut with a cross-section polisher ("IB-09010CP" manufactured by JEOL), and the cross-section was observed with a SEM ("JSM-7600F" manufactured by JEOL). As a result, no destruction of the hollow particles was confirmed in any of the resin molded bodies 1-3. In addition, no intrusion of the resin into the interior of the hollow particles was confirmed in any of the resin molded bodies 1-3.

[0113] Industrial Applicability

[0114] The hollow particles of the present invention can be preferably used in electronic materials, for example, heat insulating materials, sound insulating materials, impact buffering materials, stress buffering materials, optical materials, and lightweight materials.

[0115] Description of Reference Numerals

[0116] L Long diameter

[0117] T Thickness

[0118] 10 Laminated body

[0119] 11 Resin layer

[0120] 12 metal foil

Claims

1. A resin composition comprising a resin and plate-like hollow particles, wherein: The hollow particles contain silicon dioxide, have an aspect ratio of 2 or more and 100 or less, a shell thickness of 10 nm or more and 100 nm or less, and a pore volume of 1.5 cm 3 / g or less, Among them, the aspect ratio is a value calculated by dividing the long diameter of the hollow particle by the thickness of the hollow particle, the long diameter of the hollow particle is a value measured by observation using a scanning electron microscope (SEM) or a transmission electron microscope (TEM), and is the average value of the long diameters of 100 randomly selected primary particles, and the thickness of the hollow particle is a value measured by observation using a scanning electron microscope (SEM) or a transmission electron microscope (TEM), and is the average value of the thicknesses of 100 randomly selected primary particles.

2. The resin composition according to claim 1, wherein The major diameter of the hollow particles is 0.1 μm or more and 10 μm or less.

3. The resin composition according to claim 1 or 2, wherein The thickness of the hollow particles is 0.01 μm or more and 5 μm or less.

4. The resin composition according to claim 1 or 2, wherein The hollow particles have a hollow ratio of 20% to 95%.

5. A method for producing a resin composition, the resin composition comprising a resin and plate-like hollow particles, wherein: The hollow particles contain silicon dioxide, have an aspect ratio of 2 or more and 100 or less, a shell thickness of 10 nm or more and 100 nm or less, and a pore volume of 1.5 cm 3 / g or less, the manufacturing method comprises: obtaining core-shell particles by coating core particles with a shell-forming material, and removing the core particles from the core-shell particles to obtain the hollow particles, wherein the core particles are magnesium hydroxide or hydrotalcite, Among them, the aspect ratio is a value calculated by dividing the long diameter of the hollow particle by the thickness of the hollow particle, the long diameter of the hollow particle is a value measured by observation using a scanning electron microscope (SEM) or a transmission electron microscope (TEM), and is the average value of the long diameters of 100 randomly selected primary particles, and the thickness of the hollow particle is a value measured by observation using a scanning electron microscope (SEM) or a transmission electron microscope (TEM), and is the average value of the thicknesses of 100 randomly selected primary particles.

6. The method for producing a resin composition according to claim 5, wherein The removal of the core particles is performed by dissolving the core particles in an acidic solution.

7. The method for producing a resin composition according to claim 5 or 6, wherein: The shell forming material is water glass or tetraethoxysilane.

8. The method for producing a resin composition according to claim 5 or 6, wherein: After the core particles are removed, the hollow particles are fired.

Citation Information

Patent Citations

  • Resin composition and wiring circuit board using the same

    JP2007056158A

  • Preparation method of hollow micro / nano material

    CN108483451A

  • Method for producing hollow silica particle from sodium silicate using zno inorganic template particle

    WO2018135685A1

  • Resin composition, prepreg, metal foil-clad laminate board, resin composite sheet, and, printed circuit board

    WO2019230661A1