A metal-doped nano-TiO 2 Preparation method of coating material and catalyst

Through anionic surfactant modification and polycarboxylic acid treatment, the uniform doping and stability of metal-doped nano-titanium dioxide coating materials are achieved, which solves the problems of complexity and insufficient performance of catalyst coating methods, and improves the coating performance of catalysts. layer strength and catalytic activity.

CN115178259BActive Publication Date: 2024-10-29PETROCHINA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202110363777.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-04-02
Publication Date
2024-10-29
Estimated Expiration
2041-04-02

AI Technical Summary

Technical Problem

The existing catalyst coating methods are complex and have poor performance, resulting in the catalyst's coating strength and catalytic activity not being optimal. Especially in nanomaterial applications, hydrophobic modification makes it difficult to coat and load nanotitanium dioxide on the carrier, and Nano-microcrystalline cellulose decomposes during high-temperature roasting, causing nano-titanium dioxide to fall off.

Method used

An anionic surfactant is used to modify the nano-titanium dioxide sol, and the metal nitrate is treated with polycarboxylic acid or polyol to form an unsaturated metal carboxylate solution to achieve uniform metal doping, avoid polymerization of nano-titanium dioxide, and improve the uniformity of the coating film and catalytic performance.

Benefits of technology

It improves the coating strength, thermal stability and catalytic activity of the catalyst, reduces the coating shedding rate, enhances the performance and stability of the catalyst, and ensures the uniformity of metal doping and the maintenance of the nanostate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115178259B_ABST
    Figure CN115178259B_ABST
Patent Text Reader

Abstract

The present invention relates to the preparation of a nano-sol coating material for the treatment of volatile organic waste gas, in particular to a metal-doped nano-TiO 2 The preparation method of the coating material comprises dissolving a titanate with a monohydric alcohol to form a solution ①, mixing a chelating agent, water and a monohydric alcohol to form a solution ②, slowly dropping the solution ② into the solution ① to form a transparent sol, adding an anionic surfactant to form a sol ③; adding a doped metal salt to a polycarboxylic acid or a polyol to form an unsaturated carboxylate or unsaturated alcohol salt solution to form a solution ④; finally slowly dropping the solution ④ into the sol ③, heating and stirring, evaporating and concentrating until the TiO in the solution is 2 The content reaches 10% to 20% to form a coating material. At the same time, the present invention further prepares TiO 2 Coated catalyst, nano-TiO prepared by this method 2 The coating material has good uniformity, strength, and catalytic performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a method for preparing a nano-sol coating material for treating volatile organic waste gas (VOC). Background Art

[0002] Catalytic oxidation is one of the most effective methods for treating volatile organic compounds (VOCs). So far, the catalysts for VOCs treatment are mainly Pt, Pd, and Rh precious metal catalysts. Most of these catalysts use cordierite honeycomb ceramics as the first carrier, and a γ-Al2O3 coating is coated on the surface of its pores as the second carrier. Functional additives such as those that improve activity, thermal stability, and sulfur resistance are usually added to the second carrier to improve the catalyst performance, and finally the precious metal active components are impregnated on the second carrier. The second carrier coating method not only affects the coating strength and process difficulty, but also directly affects the various properties of the catalyst. Therefore, the research on the carrier coating method has become one of the research focuses of this type of catalyst.

[0003] The existing coating method is to first make γ-Al2O3 into powder, then make slurry with water and additives, apply it on the carrier, and finally impregnate various auxiliary components into the carrier. Not only is the process complicated, the catalyst preparation cycle is long, but also the catalyst coating performance and catalytic activity cannot reach the best. In order to improve the performance of the second carrier, researchers have adopted nanotechnology to mix γ-Al2O3 nanopowder and auxiliary nanopowder to make coating slurry. Since nanomaterials are composed of extremely fine microscopic particles less than 100nm, the strength and catalytic performance of the coating can be improved. However, due to the agglomeration between nanopowder particles, although the particles can be made very small after grinding, they can generally only reach the micron level, resulting in microscopic uneven distribution of auxiliary agents and carriers, so as to affect the strength and catalytic performance of the coating.

[0004] CN200810156937.2 A method for preparing hydrophobic nano titanium dioxide powder discloses a method for preparing hydrophobic nano titanium dioxide powder, wherein the nano titanium dioxide is first subjected to inorganic surface treatment in the liquid phase of the nano titanium dioxide aqueous dispersion, and then subjected to organic surface treatment, and finally the nano titanium dioxide slurry is filtered and washed until the conductivity of the filtrate is less than 500 μS / cm, and then dried and crushed to obtain the hydrophobic nano titanium dioxide powder. The invention combines the inorganic surface treatment and the organic surface treatment of nano titanium dioxide into one, changes the surface properties of nano titanium dioxide, increases the filtration speed of nano titanium dioxide during the solid-liquid separation process, reduces the loss rate of nano titanium dioxide, has a short process flow, is convenient to operate, and is easy to control. The prepared nano titanium dioxide powder not only has good hydrophobicity, but also has excellent light stability. However, the patent adopts hydrophobic modification for nano titanium dioxide, and the hydrophobic modification will make it more difficult to coat and load nano titanium dioxide on the cordierite carrier.

[0005] CN201610156546.5 A nano photocatalyst and a preparation method thereof, discloses a nano photocatalyst, comprising the following components in weight: 30-35 parts of nano titanium dioxide; 5-10 parts of nano microcrystalline cellulose colloid (nano microcrystalline cellulose is 2-3.5wt / %); 2-6 parts of adhesive; 1-3 parts of titanate silane coupling agent; 1-3 parts of anionic surfactant; 5-10 parts of dispersant; 80-85 parts of deionized water; the nano titanium dioxide is porous anatase nano titanium dioxide, the particle size of the nano titanium dioxide is 3-5nm, and the nano microcrystalline cellulose in the nano microcrystalline cellulose colloid is a network structure. The invention is green and pollution-free, the particle size of the porous anatase nano titanium dioxide is 3-5nm, the specific surface area is large, and the nano microcrystalline cellulose with a network structure connects the nano titanium dioxide to the surface, increases the distribution range of the nano titanium dioxide and the contact area with the substrate, and improves its purification effect. The harmful gases are degraded in newly built shopping malls, large office buildings, newly renovated residences, etc., and the harmful substances are converted into active substances such as [O] and [HO]. However, the nano-microcrystalline cellulose used in the patent will decompose when calcined at high temperature, which will inevitably cause the nano-titanium dioxide coated on the carrier to fall off.

[0006] CN201910740931.8 A high-efficiency nanomolecular photocatalyst and a preparation method thereof, provides a high-efficiency nanomolecular photocatalyst and a preparation method thereof, the nanomolecular photocatalyst comprises the following components in parts by weight: 30-35 parts of nano titanium dioxide TiO2; artificial zeolite Na1Al 12 Si 12 O 48·27H2O5-10 parts; semiconductor nanocrystal QDs5-10 parts; adhesive 2-6 parts; silane coupling agent 1-3 parts; anionic surfactant 1-3 parts; dispersant 5-10 parts; deionized water 80-85 parts; the preparation method comprises the following steps: S1, pretreatment; S2, film-forming agent preparation; S3, dispersion emulsion preparation; S4, mixed extract preparation; S5, final product preparation; S6, packaging. The present invention can minimize the agglomeration of nano ions in the photocatalyst, while breaking through some inorganic fillers and organic embedding, and can also achieve photocatalysis through self-luminescence, greatly improving the catalytic efficiency of the photocatalyst on harmful substances.

[0007] CN201410856336.8 A method for preparing a praseodymium-doped titanium dioxide composite nanofiber photocatalyst, discloses a method for preparing a praseodymium-doped titanium dioxide composite nanofiber photocatalyst, comprising: (a) placing tetrabutyl titanate in a mixed solution of anhydrous ethanol and acetic acid and mixing evenly, then sequentially adding praseodymium acetylacetonate and polyvinyl pyrrolidone thereto, and continuing stirring until a precursor solution is obtained; (b) adding the precursor solution to a syringe of an electrostatic spinning device, and obtaining a praseodymium-doped titanium dioxide nanofiber nonwoven fabric by controlling the process conditions of the electrostatic spinning; (c) arranging the nanofiber nonwoven fabric in a muffle furnace, and heating it from room temperature to 500°C in an air atmosphere to perform calcination, and then naturally cooling it to room temperature, to obtain the desired composite nanofiber photocatalyst product. Through the present invention, the efficiency and performance of mercury removal from coal-fired flue gas can be significantly improved, and at the same time, it has the advantages of easy control, low cost and low energy consumption, and is therefore particularly suitable for the application of mercury removal from flue gas in coal-fired power plants. This method uses non-ionic surfactants to separate titanium dioxide nanoparticles, which is a physical dispersion. There is no chemical bonding between the titanium dioxide nanoparticles and the cationic nanoparticles. However, the doped metals are still free in the solution in the form of ions. During the subsequent drying process, the ions migrate with the solution, resulting in uneven metal doping in the end.

[0008] CN201310502913.9 Iron phosphate coated photocatalytic nano titanium dioxide powder and its application, providing a photocatalytic yellow powder that can be used for environmental purification, by coating each titanium dioxide particle with iron phosphate particles, selectively shielding or weakening the degradation function of titanium dioxide on macromolecular organic matter. Its operation steps are: (1) mixing nano titanium dioxide with pH buffer solution, and then adding anionic surfactant; (2) dissolving iron salt and phosphate in distilled water and stirring, and then adding anionic surfactant; (3) adding the mixed solution obtained in step (1) to the mixed solution obtained in step (2), adjusting the pH value to alkaline with ammonia water, stirring and heating, and drying to obtain a gel. This patent forms a gel by adjusting the pH to alkaline, and the final powder material can be widely used in various organic polymer shaped products, especially organic fibers or plastic products or color coatings.

[0009] CN201410666696.1 A method for preparing anatase-type nano titanium dioxide powder modified by co-doping iron element and two non-metallic elements, discloses a method for preparing anatase-type nano titanium dioxide powder modified by co-doping iron element and two non-metallic elements, (1) mixing an organic titanium source, alkylphenol polyoxyethylene ether, C4-7 monohydric alcohol, C5-8 alkane or cycloalkane to obtain a mixed solution A; (2) mixing alkylphenol polyoxyethylene ether, C4-7 monohydric alcohol, C5-8 alkane or cycloalkane with a dilute acid solution (dilute hydrochloric acid or dilute nitric acid) containing iron, nitrogen and sulfur to obtain a mixed solution B; (3) dropping B into the mixed solution A to obtain a mixed solution C; (4) reacting the mixed solution C in a hydrothermal reaction vessel at 120-180°C for 1-12 hours, cooling, washing and drying. This patent only adds non-ionic surfactants during the hydrolysis of titanium salt, and dilute hydrochloric acid or dilute nitric acid is used when doping iron, nitrogen and sulfur. Its main purpose is to prepare nanopowder materials.

[0010] CN201710984878.7 A mesoporous silica photocatalytic net and preparation method, the patent relates to the preparation of a titanium-based sol coating liquid doped with Tb, Fe and N, the steps comprising: (1) mixing tetrabutyl titanate, n-butanol and diethanolamine to obtain liquid A; (2) dissolving urea, hydrated terbium nitrate and hydrated ferric nitrate in anhydrous ethanol and deionized water, mixing and stirring to obtain liquid B; (3) slowly adding liquid A to liquid B placed in an ice water bath, stirring continuously, and continuing to stir for 1 to 2 hours after the addition to obtain a doped titanium-based sol coating liquid. This patent uses ethanol as a dispersant, and the metal ions and nano-titanium dioxide are physically dispersed. Summary of the invention

[0011] The object of the present invention is to provide a method for preparing a metal-doped nano titanium dioxide coating material to improve the coating strength, thermal stability and activity of a catalytic oxidation catalyst.

[0012] The method for preparing a metal-doped nano-titanium dioxide coating material of the present invention specifically comprises the following steps:

[0013] (1) Dissolve titanate in monohydric alcohol to form a solution ①,

[0014] (2) Mixing a chelating agent, water and a monohydric alcohol to form a solution②,

[0015] (3) Slowly add solution ② to solution ① to form a transparent sol, and add anionic surfactant to form sol ③;

[0016] (4) adding the doped metal salt to a polycarboxylic acid or a polyol to form an unsaturated carboxylate or unsaturated alcohol salt solution to form solution ④;

[0017] (5) Slowly drop solution ④ into sol ③, heat and stir, evaporate and concentrate until the TiO2 content in the solution reaches 10% to 20%, thereby forming a coating material.

[0018] In the above preparation method, the anionic surfactant in step (3) is sodium dodecyl sulfate or sodium polyacrylate, and its added amount is 0.01 to 1 times the amount of the titanium substance, preferably 0.02 to 0.2 times.

[0019] In the above step (4), the polycarboxylic acid is citric acid, butanetetracarboxylic acid, itaconic acid or oligomeric maleic acid, and the added amount is 0.1 to 5 times the amount of the total amount of the doped metal substance.

[0020] In the above step (4), the polyol is propylene glycol or ethylene glycol, and the amount of the polyol added is 0.1 to 5 times the amount of the total amount of the doped metal substance.

[0021] In the above step (4), the doping metal is selected from Group VIII or rare earth, and the amount of the doping metal is 0 to 1 times, preferably 0.02 to 0.2 times, the amount of the titanium substance.

[0022] In the above steps (1) and (2), the monohydric alcohol is ethanol, isopropanol, butanol, etc., and the amount thereof added is 5 to 50 times, preferably 10 to 20 times, the amount of the titanium substance.

[0023] In the above step (2), the chelating agent is acetylacetone or alcoholamines, and the alcoholamines are ethanolamine, diethanolamine or triethanolamine. The amount of acetylacetone or alcoholamines added is 0.1 to 10 times the amount of the titanium substance, preferably 1 to 3 times.

[0024] In the above step (3), when solution ② is added dropwise to solution ①, stirring or ultrasonic oscillation must be performed, and the dropping speed should not be too fast.

[0025] In the above step (5), solution ④ is slowly added dropwise to sol ③ under constant temperature stirring at 70-90°C.

[0026] The viscosity of the coating material formed by the above preparation method at room temperature is 5 to 20 centipoise, preferably 10 to 18 centipoise. If the viscosity of the coating material formed is too high, it can be diluted with deionized water to adjust the viscosity.

[0027] Furthermore, the present invention also discloses a method for preparing a metal-doped nano-titanium dioxide film-coated catalyst, comprising the following steps:

[0028] (1) Dissolve titanate in monohydric alcohol to form a solution ①,

[0029] (2) Mixing a chelating agent, water and a monohydric alcohol to form a solution②,

[0030] (3) Slowly adding solution ② to solution ① to form a transparent sol, and adding anionic surfactant to modify it to form sol ③;

[0031] (4) adding the doped metal salt to a polycarboxylic acid or a polyol to form an unsaturated carboxylate or unsaturated alcohol salt solution to form solution ④;

[0032] (5) Slowly drop solution ④ into sol ③, heat and stir, evaporate and concentrate until the TiO2 content in the solution reaches 10% to 20%, thereby forming a coating material;

[0033] (6) dipping the coating material obtained in step (5) into the base material;

[0034] (7) Aging, drying and calcining to form a coating catalyst.

[0035] The substrate material in the above step (6) is selected from honeycomb ceramics, foam ceramics, honeycomb metal or foam metal.

[0036] Furthermore, the above-mentioned film-coated catalyst can also be used as a carrier to further introduce precious metals to improve its activity.

[0037] The present invention provides a method for preparing a metal-doped nano titanium dioxide coating material, which comprises the following steps: modifying a nano titanium dioxide sol by adding an anionic surfactant, and then adding an unsaturated metal carboxylate solution formed by treating a metal nitrate with a polycarboxylic acid, thereby achieving the effect of uniform metal doping while preventing the nano titanium dioxide from polymerizing, thereby maintaining the nano state and improving the uniformity, strength, and catalytic performance of the coating.

[0038] The present invention is under the effect of monohydric alcohol dispersant, and titanium salt is hydrolyzed and polycondensed to form cationic nano particles with positive charge on the surface, and because the nano particle size is less, a sol is formed. In the sol, metal is doped, the performance of nano titanium dioxide can be improved, and its thermal stability and catalytic activity are improved. However, if metal salt is directly added, because metal ion is also positively charged, metal ion can not be adsorbed on the titanium dioxide nano particle surface, and in the drying process, along with solvent volatilization, metal ion migrates along with solvent, and finally will be separated out to the surface, causing doping unevenness. Therefore, metal ion can be chemically bonded to the nano titanium dioxide particle surface by carboxyl or hydroxyl by adding polycarboxylic acid or polyol in the metal salt doping process, but if directly added, although metal ion may be adsorbed to the titanium dioxide particle surface by carboxylic acid under the effect of polycarboxylic acid or polyol negative charge, other nano particles can also be attracted by carboxyl, causing nano particle polymerization precipitation. Therefore, the present invention adopts a special process to modify the nano titanium dioxide and metal nitrate solution before mixing, that is, first add anionic surfactant to modify the nano titanium dioxide sol, so that the anionic surfactant occupies part of the positive position of titanium dioxide, dope metal and polycarboxylic acid to form unsaturated metal carboxylate, and then mix the two liquids, the carboxyl group not combined with metal ions is combined with the positive charge on the surface of cationic nano titanium dioxide. This specific addition order and method has two advantages. On the one hand, Figure 1 As shown, the surface of each nanoparticle is covered by a surfactant, forming a spatial barrier, which prevents the nanoparticles from contacting each other, thereby achieving a dispersion effect; on the other hand, the excess positive charge on the surface of the nanoparticles can attract unsaturated polycarboxylates, making the metal particles evenly distributed on all the nanoparticles in the sol, thereby achieving atomic-level doping. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 Schematic diagram of the metal doping process.

[0040] Figure 2 This is the SEM picture of the catalyst surface.

[0041] Figure 3 This is a SEM photo of the catalyst coating.

[0042] Figure 4 The following are the evaluation results of the embodiments and comparative examples. DETAILED DESCRIPTION

[0043] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0044] The following examples and comparative examples are listed to illustrate the effects of the present invention, but the protection scope of the present invention is not limited to these examples. The "parts" described in the examples refer to mol parts.

[0045] (1) Source of raw materials in the embodiment:

[0046] Citric acid Tianjin Kemeiou Chemical Reagent Co., Ltd.

[0047] Butanol Tianjin Komiou Chemical Reagent Co., Ltd.

[0048] Isopropyl alcohol Tianjin Komiou Chemical Reagent Co., Ltd.

[0049] Concentrated nitric acid Ruili Aolai Chemical Co., Ltd.

[0050] Concentrated hydrochloric acid Tianjin Komiou Chemical Reagent Co., Ltd.

[0051] Concentrated sulfuric acid Tianjin Komiou Chemical Reagent Co., Ltd.

[0052] Anhydrous ethanol Tianjin Kemeiou Chemical Reagent Co., Ltd.

[0053] Sodium Polyacrylate Tianjin Kemeiou Chemical Reagent Co., Ltd.

[0054] Sodium dodecane sulfate Tianjin Komiou Chemical Reagent Co., Ltd.

[0055] Cerium nitrate Chengdu Kelong Chemical Reagent Co., Ltd.

[0056] Manganese nitrate Chengdu Kelong Chemical Reagent Co., Ltd.

[0057] Lanthanum nitrate Chengdu Kelong Chemical Reagent Co., Ltd.

[0058] Ammonium Metavanadate Chengdu Kelong Chemical Reagent Co., Ltd.

[0059] Itaconic acid Tianjin Kemeiou Chemical Reagent Co., Ltd.

[0060] Oligomeric Maleic Acid Tianjin Kemeiou Chemical Reagent Co., Ltd.

[0061] Butane Tetracarboxylic Acid Tianjin Kemeiou Chemical Reagent Co., Ltd.

[0062] Cordierite Honeycomb Ceramics Jiangxi Pingxiang Yuanchuang

[0063] ⑵Analysis and testing methods:

[0064] Surface uniformity: direct observation, scanning electron microscopy analysis.

[0065] pH measurement of sample solution: The pH of the sample was dynamically measured using the pH analyzer S210 produced by Mettler.

[0066] Coating shedding rate test: Coating shedding rate is an important indicator for characterizing coating strength. The test method is as follows: the calcined carrier is placed in an ultrasonic water bath, ultrasonically shaken for 30 minutes, and dried at 110°C for 2 hours. The coating shedding rate L (%) is calculated according to the following formula:

[0067] L=[(W1-W2) / W0]×100%

[0068] Where:

[0069] W0—coating mass before the experiment, g;

[0070] W1—mass of carrier + coating before experiment, g;

[0071] W2—mass of carrier + coating after the experiment, g.

[0072] (3) Evaluation method:

[0073] Taking toluene as the object, the toluene is gasified and mixed with air to form a toluene content of 500-5000mg / m 3 The mixed gas is heated at 16000h under programmed temperature. -1 The fixed space velocity of toluene enters the fixed bed catalytic reactor, and the toluene removal rate at different temperatures is recorded. The temperature at which toluene is 98% converted (T98) is used to measure the catalyst activity. The lower the T98, the higher the catalyst activity.

[0074] Example 1

[0075] Dissolve 1 part of tetrabutyl titanate in 5 parts of ethanol, adjust the pH to 1 with concentrated nitric acid to form solution ①, mix 1 part of acetylacetone, 1 part of water and 5 parts of ethanol to form solution ②, slowly drop solution ② into solution ① under ultrasonic vibration to form transparent sol ③, i.e., complete hydrolysis, add 0.02 parts of sodium dodecyl sulfate to sol ③ to form sol ④.

[0076] Dissolve 1 part of lanthanum nitrate and cobalt nitrate in deionized water, and then add 0.1 part of butane tetracarboxylic acid solution to form solution ⑤.

[0077] Under constant temperature stirring at 70°C, slowly drop solution ⑤ into sol ④, continue heating and stirring to evaporate the solvent until the TiO2 content reaches 20%, and the sol viscosity measured at 20°C is 24.4 centipoise, thus forming a coating material.

[0078] The coating was dipped and pulled on 100-mesh cordierite honeycomb ceramics, aged at room temperature for 12 hours, dried at 105°C for 2 hours, and calcined at 500°C for 4 hours. The coating was repeated 3 times until the coating amount reached 18.3%. A precious metal solution with a mass ratio of Pt to Pd of 1:2 was used, and a certain amount of precious metal solution was taken for impregnation based on the total mass of the precious metal being 0.2% of the total mass of the carrier to form a catalyst.

[0079] Evaluation results:

[0080] The coating shedding rate was 0.35%.

[0081] Activity evaluation results: toluene 98% conversion temperature, T98 = 259°C.

[0082] Example 2

[0083] Dissolve 1 part of tetrabutyl titanate in 20 parts of ethanol, adjust the pH to 2 with concentrated nitric acid to form solution ①, mix 5 parts of ethanolamine, 5 parts of water and 5 parts of ethanol to form solution ②, slowly add solution ② to solution ① under ultrasound or stirring to form transparent sol ③, thus completing the hydrolysis, add 0.01 parts of sodium dodecyl sulfate to sol ③ to form sol ④.

[0084] Dissolve 0.1 parts of lanthanum nitrate and cobalt nitrate in deionized water, and then add 1 part of citric acid solution to form solution ⑤.

[0085] Under constant temperature stirring at 70°C, slowly drop solution ⑤ into sol ④, continue heating and stirring to evaporate the solvent until the TiO2 content reaches 10%, and the sol viscosity is 8.2 centipoise at 20°C to form a coating material.

[0086] The coating was dipped and pulled on a 200-mesh cordierite honeycomb ceramic, aged at room temperature for 12 hours, dried at 105°C for 2 hours, and calcined at 500°C for 4 hours. The coating was repeated 3 times until the coating amount reached 8.8%. A precious metal solution with a mass ratio of Pt to Pd of 1:2 was used, and a certain amount of precious metal solution was taken for impregnation based on the total mass of the precious metal being 0.2% of the total mass of the carrier to form a catalyst.

[0087] Evaluation results:

[0088] The coating shedding rate was 0.22%.

[0089] Activity evaluation results: toluene 98% conversion temperature, T98 = 270°C.

[0090] Example 3

[0091] Dissolve 1 part of tetrabutyl titanate in 10 parts of isopropanol, adjust the pH to 3 with concentrated hydrochloric acid to form solution ①, mix 5 parts of diethanolamine, 1 part of water and 10 parts of isopropanol to form solution ②, slowly add solution ② to solution ① under ultrasound or stirring to form transparent sol ③, thus completing the hydrolysis, add 0.2 parts of sodium dodecyl sulfate to sol ③ to form sol ④.

[0092] Dissolve 1 part of cerium nitrate, lanthanum nitrate and manganese nitrate in deionized water, and then add 5 parts of itaconic acid solution to form solution ⑤.

[0093] Under constant temperature and stirring at 90°C, slowly drop solution ⑤ into sol ④, continue heating and stirring to evaporate the solvent until the TiO2 content reaches 20%, and the sol viscosity measured at 20°C is 29.8 centipoise, thus forming a coating material.

[0094] The coating was dipped and pulled on a 60-mesh cordierite honeycomb ceramic, aged at room temperature for 12 hours, dried at 105°C for 2 hours, and calcined at 500°C for 4 hours. The coating was repeated 3 times. A precious metal solution with a mass ratio of Pt to Pd of 1:2 was used. A certain amount of precious metal solution was taken for impregnation based on the total mass of the precious metal being 0.2% of the total mass of the carrier to form a catalyst.

[0095] Evaluation results:

[0096] The coating shedding rate was 0.39%.

[0097] Activity evaluation results: toluene 98% conversion temperature, T98 = 253°C.

[0098] Example 4

[0099] Dissolve 1 part of tetrabutyl titanate in 50 parts of ethanol, adjust the pH to 1 with concentrated nitric acid to form solution ①, mix 5 parts of triethanolamine, 1 part of water and 50 parts of ethanol to form solution ②, slowly add solution ② to solution ① under ultrasound or stirring to form transparent sol ③, thus completing hydrolysis, add 1 part of sodium polyacrylate to sol ③ to form sol ④.

[0100] A total of 0.1 parts of cerium nitrate and ammonium metavanadate were dissolved in deionized water, and then 0.1 parts of oligomeric maleic acid solution was added to form solution ⑤.

[0101] Under constant temperature and stirring at 90°C, slowly drop solution ⑤ into sol ④, continue heating and stirring to evaporate the solvent until the TiO2 content reaches 20%, and the sol viscosity measured at 20°C is 31.4 centipoise, thus forming a coating material.

[0102] The coating was dipped and pulled on a 60-mesh cordierite honeycomb ceramic, aged at room temperature for 12 hours, dried at 105°C for 2 hours, and calcined at 500°C for 4 hours. The coating was repeated 3 times until the coating amount reached 19.9%. A precious metal solution with a mass ratio of Pt to Pd of 1:2 was used, and a certain amount of precious metal solution was taken for impregnation based on the total mass of the precious metal being 0.2% of the total mass of the carrier to form a catalyst.

[0103] Evaluation results:

[0104] The coating shedding rate was 0.49%.

[0105] Activity evaluation results: toluene 98% conversion temperature, T98 = 300°C.

[0106] Example 5

[0107] Dissolve 1 part of tetrabutyl titanate in 5 parts of butanol, adjust the pH to 2 with concentrated nitric acid to form solution ①, mix 10 parts of diethanolamine, 10 parts of water and 50 parts of butanol to form solution ②, slowly add solution ② to solution ① under ultrasound or stirring to form transparent sol ③, thus completing the hydrolysis, add 0.1 parts of sodium polyacrylate to sol ③ to form sol ④.

[0108] Dissolve 0.1 parts of cerium nitrate, manganese nitrate and lanthanum nitrate in deionized water, and then add 1 part of citric acid solution to form solution ⑤.

[0109] Under constant temperature and stirring at 90°C, slowly drop solution ⑤ into sol ④, continue heating and stirring to evaporate the solvent until the TiO2 content reaches 15%, and the sol viscosity is 15.6 centipoise at 20°C to form a coating material.

[0110] The coating was dipped and pulled on a 60-mesh honeycomb ceramic, aged at room temperature for 12 hours, dried at 105°C for 2 hours, and calcined at 500°C for 4 hours. The coating was repeated 3 times until the coating amount reached 14.3%. A precious metal solution with a mass ratio of Pt to Pd of 1:2 was used, and a certain amount of precious metal solution was taken for impregnation based on the total mass of the precious metal being 0.2% of the total mass of the carrier to form a catalyst.

[0111] Evaluation results:

[0112] The coating shedding rate was 0.16%.

[0113] Activity evaluation results: toluene 98% conversion temperature, T98 = 240°C.

[0114] Comparative Example 1

[0115] Dissolve 1 part of tetrabutyl titanate in 5 parts of butanol, adjust the pH to 2 with concentrated nitric acid to form solution ①, mix 10 parts of diethanolamine, 10 parts of water and 50 parts of butanol to form solution ②, slowly drop solution ② into solution ① under ultrasound or stirring to form transparent sol ③, thus completing hydrolysis, add 1 part of polyvinyl pyrrolidone to sol ③ to form sol ④.

[0116] Dissolve 0.1 parts of cerium nitrate, manganese nitrate and lanthanum nitrate in deionized water, and then add 1 part of citric acid solution to form solution ⑤.

[0117] Under constant temperature and stirring at 90℃, solution ⑤ is slowly added dropwise to sol ④ to produce flocculent precipitation, which becomes turbid liquid under stirring. Continue heating and stirring to evaporate the solvent until the TiO2 content reaches 15%, and the sol viscosity is 16.4 centipoise at 20℃. A coating material is formed.

[0118] The coating was dipped and pulled on a 60-mesh honeycomb ceramic, aged at room temperature for 12 hours, dried at 105°C for 2 hours, and calcined at 500°C for 4 hours. The coating was repeated 3 times until the coating amount reached 13.1%. A precious metal solution with a mass ratio of Pt to Pd of 1:2 was used, and a certain amount of precious metal solution was taken for impregnation based on the total mass of the precious metal being 0.2% of the total mass of the carrier to form a catalyst.

[0119] Evaluation results:

[0120] The coating shedding rate was 1.32%. The large coating shedding rate was mainly due to the agglomeration after the addition of citric acid.

[0121] The activity evaluation results show that the 98% conversion temperature of toluene is T98>360℃, and the catalytic effect is obviously poor, which is mainly caused by the uneven doping of metals.

[0122] Comparative Example 2

[0123] Dissolve 1 part of tetrabutyl titanate in 5 parts of butanol, adjust the pH to 2 with concentrated nitric acid to form solution ①, mix 10 parts of diethanolamine, 10 parts of water and 50 parts of butanol to form solution ②, slowly drop solution ② into solution ① under ultrasound or stirring to form transparent sol ③, and complete the hydrolysis.

[0124] Dissolve 0.1 parts of cerium nitrate, manganese nitrate and lanthanum nitrate in deionized water, and then add 1 part of citric acid solution to form solution ④.

[0125] Under constant temperature and stirring at 90℃, solution ④ is slowly added dropwise to sol ③ to produce flocculent precipitation, which becomes turbid liquid under stirring, and then 1 part of sodium polyacrylate is added, and heating and stirring are continued to evaporate the solvent until the TiO2 content reaches 15%, and the sol viscosity measured at 20℃ is 12.4 centipoise. A coating material is formed.

[0126] The coating was dipped and pulled on a 60-mesh honeycomb ceramic, aged at room temperature for 12 hours, dried at 105°C for 2 hours, and calcined at 500°C for 4 hours. The coating was repeated 3 times until the coating amount reached 13.5%. A precious metal solution with a mass ratio of Pt to Pd of 1:2 was used, and a certain amount of precious metal solution was taken for impregnation based on the total mass of the precious metal being 0.2% of the total mass of the carrier to form a catalyst.

[0127] Evaluation results:

[0128] The coating shedding rate was 1.05%. The large coating shedding rate was mainly due to the agglomeration after the addition of citric acid.

[0129] The activity evaluation results show that the 98% conversion temperature of toluene is T98>300℃, and the catalytic effect is poor, mainly because the nano-titanium dioxide agglomerates, the particles increase, and the specific surface area decreases.

[0130] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a metal-doped nano titanium dioxide coating material, characterized in that: The following steps are involved: (1) Dissolve titanate in monohydric alcohol to form a solution①, (2) Mix the chelating agent, water and monohydric alcohol to form a solution②, (3) Slowly add solution ② to solution ① to form a transparent sol, and add anionic surfactant to form sol ③; (4) adding the doped metal salt to a polycarboxylic acid or a polyol to form an unsaturated carboxylate or unsaturated alcohol salt solution to form solution ④; (5) Slowly add solution ④ to sol ③, heat and stir, evaporate and concentrate until the TiO2 content in the solution reaches 10%~20%, forming a coating material; The anionic surfactant in step (3) is sodium dodecyl sulfate or sodium polyacrylate; The polycarboxylic acid in step (4) is citric acid, butanetetracarboxylic acid, itaconic acid or oligomeric maleic acid; The polyol in step (4) is propylene glycol or ethylene glycol.

2. The method for preparing a metal-doped nano-titanium dioxide coating material according to claim 1, characterized in that: The amount of the anionic surfactant added in step (3) is 0.01 to 1 times the amount of the titanium substance.

3. The method for preparing a metal-doped nano titanium dioxide coating material according to claim 1, characterized in that: The amount of the anionic surfactant added in step (3) is 0.02 to 0.2 times the amount of the titanium substance.

4. The method for preparing a metal-doped nano-titanium dioxide coating material according to claim 1, characterized in that: The doping metal is selected from Group VIII or rare earth, and the total amount of the doping metal is 0.02 to 1 times the amount of the titanium substance.

5. The method for preparing a metal-doped nano titanium dioxide coating material according to claim 1, characterized in that: The monohydric alcohol in steps (1) and (2) is ethanol, isopropanol or butanol, and the amount added is 5 to 50 times the amount of the titanium substance.

6. The method for preparing a metal-doped nano-titanium dioxide coating material according to claim 1, characterized in that: The chelating agent in step (2) is acetylacetone or alcohol amine, and the amount added is 0.1 to 10 times the amount of the titanium substance.

7. The method for preparing a metal-doped nano titanium dioxide coating material according to claim 6, characterized in that: The alcoholamines are ethanolamine, diethanolamine or triethanolamine.

8. A method for preparing a metal-doped nano-titanium dioxide film-coated catalyst, characterized in that: The following steps are involved: (1) Dissolve titanate in monohydric alcohol to form a solution①, (2) Mix the chelating agent, water and monohydric alcohol to form a solution②, (3) Slowly add solution ② to solution ① to form a transparent sol, and add anionic surfactant to modify it to form sol ③; (4) adding the doped metal salt to a polycarboxylic acid or a polyol to form an unsaturated carboxylate or unsaturated alcohol salt solution to form solution ④; (5) Slowly add solution ④ to sol ③, heat and stir, evaporate and concentrate until the TiO2 content in the solution reaches 10%~20%, forming a coating material; (6) dipping the coating material obtained in step (5) into the base material; (7) Aging, drying and calcining to form a coating catalyst; The anionic surfactant in step (3) is sodium dodecyl sulfate or sodium polyacrylate; The polycarboxylic acid in step (4) is citric acid, butanetetracarboxylic acid, itaconic acid or oligomeric maleic acid; The polyol in step (4) is propylene glycol or ethylene glycol.

9. The method for preparing a metal-doped nano-titanium dioxide film-coated catalyst according to claim 8, characterized in that: The substrate material in step (6) is selected from honeycomb ceramics, foam ceramics, honeycomb metal or foam metal.

10. The method for preparing a metal-doped nano-titanium dioxide film-coated catalyst according to claim 8, characterized in that: The precious metal is introduced using the film-coated catalyst as a carrier.

Citation Information

Patent Citations

  • Method of preparing hydrophobic nano-titanium dioxide powder

    CN101367548A

  • Iron phosphate-wrapped photocatalytic nano titanium dioxide powder and application thereof

    CN103551174A

  • Preparation method of anatase nano-titanium dioxide powder modified via codoping of iron element with other two non-metallic elements

    CN104525232A

  • Preparation method of praseodymium-doped titanium dioxide composite nanofiber photocatalyst

    CN104607171A

  • A nano-photocatalyst and its preparation method

    CN105689006B