Shell, shell surface treatment method and electronic equipment
By drilling, printing and electroplating on the resin substrate, combined with the imprinting technology of ultraviolet coating, the complex and contaminated aluminum anode process is solved, and the low-cost and environmentally friendly metal texture treatment of the outer shell of electronic equipment is achieved.
Patent Information
- Application Number
- CN202210695926.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-06-20
AI Technical Summary
The existing aluminum anode process is complex in the processing of electronic equipment shells, high material costs and severe environmental pollution, making it difficult to apply on low-end products, and lacks low-cost and environmentally friendly alternatives to achieve metal texture.
Use resin substrate to drill and cut chamfer, print mirror ink layer and colored ink layer, and set up metal electroplating layer on the bottom surface. Finally, UV curing coating is printed on the surface of the resin substrate and imprinted to form concave and convex texture, replacing traditional aluminum Anode process.
The shell surface treatment similar to the appearance effect and texture of aluminum anode is achieved, while reducing environmental pollution and production costs, and is suitable for low-end electronic equipment.
Smart Images

Figure CN115178447B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of surface treatment, and in particular to a shell, a shell surface treatment method and an electronic device. Background Art
[0002] In the field of electronic devices such as notebooks, mobile phones, and tablet computers, aluminum anode technology is one of the most widely used electronic device shell processing technologies because of its good metal texture. However, aluminum anode cannot be used on relatively low-end products due to its complex process and high material cost, and aluminum anode technology seriously pollutes the environment. With the continuous advancement of the concept of green development, there is an urgent need for a low-cost and environmentally friendly shell surface treatment method that can give the shell of electronic devices a metal texture. Summary of the invention
[0003] The present invention provides a housing, a housing surface treatment method and an electronic device, so as to at least solve the above technical problems existing in the prior art.
[0004] In one aspect, the present invention provides a shell surface treatment method, the method comprising:
[0005] Drill and chamfer the edge of the top of the resin substrate to form a drilled surface;
[0006] Printing mirror ink on the edges of the bottom surface of the resin substrate to form a mirror ink layer, wherein the printing width of the mirror ink is equal to the projection width of the drilled surface on the bottom surface of the resin substrate; the drilled surface and the mirror ink layer form a high-gloss edge on the side wall of the resin substrate;
[0007] Printing a colored ink with an imitation anode texture on the bottom surface of the resin substrate to form a colored ink layer, wherein the printing thickness of the colored ink is equal to the printing thickness of the mirror ink;
[0008] Disposing a metal electroplating layer on the bottom surfaces of the colored ink layer and the mirror ink layer;
[0009] The ultraviolet curing coating is printed on the surface of the resin substrate and pre-cured to form an ultraviolet coating, and embossing is performed on the surface of the ultraviolet coating to form a concave-convex texture.
[0010] In one possible implementation manner, the resin substrate is a PET (polyethyleneterephthalate) material with a glossiness greater than 90 degrees, and the thickness of the resin substrate is 0.5-1.2 mm.
[0011] In one embodiment, the cutting and chamfering of the edge on the top of the resin substrate to form a drilled surface includes:
[0012] The edge line of the top of the resin substrate is drilled and chamfered at a drilling speed of 28000-36000 rpm to obtain a drilled surface, wherein the projection width of the drilled surface on the side of the resin substrate is 0.3-0.5 mm.
[0013] In one possible implementation manner, the projection width of the drilled surface on the bottom surface of the resin substrate is 0.3-0.6 mm.
[0014] In one possible implementation manner, the step of providing a metal electroplating layer on the bottom surfaces of the colored ink layer and the mirror ink layer comprises:
[0015] The aluminum material is placed in the vacuum coating machine with a 1×10 -4 -5×10 -4 Torr (1 Torr = 1 mmHg) for vacuum coating.
[0016] In one possible implementation manner, the thickness of the colored ink layer is 7-10 μm, and the thickness of the metal electroplating layer is 0.1-0.2 μm.
[0017] In one embodiment, the step of embossing the surface of the UV coating comprises:
[0018] A structure with a concave and convex texture is prepared on a metal master;
[0019] The structure of the concavo-convex texture on the metal master is transferred to the ultraviolet coating to form a concavo-convex texture on the ultraviolet coating.
[0020] In one possible implementation manner, after the concavo-convex texture is formed on the UV coating, the glossiness of the UV coating is 10-20 degrees.
[0021] Another aspect of the present invention provides a housing, which is manufactured according to the housing surface treatment method described above, and comprises:
[0022] A resin substrate, wherein the edge line at the top of the resin substrate is drilled and chamfered to form a drilled surface;
[0023] A mirror ink layer, wherein the mirror ink layer is located around the edges of the bottom surface of the resin substrate, and the width of the mirror ink layer is equal to the projection width of the drilled surface on the bottom surface of the resin substrate;
[0024] A colored ink layer, wherein the colored ink layer is disposed on the bottom surface of the resin substrate;
[0025] a metal electroplating layer, the metal electroplating layer being arranged on the bottom surface of the mirror ink layer; and
[0026] The UV coating is arranged on the surface of the resin substrate and has a concave-convex texture on the surface of the UV coating.
[0027] Another aspect of the present invention provides an electronic device having the above-mentioned housing.
[0028] In the above scheme of the present invention, the edge line on the top of the resin substrate is drilled and cut, and then the mirror ink layer, the colored ink layer, and the electroplated metal electroplated layer are layered and printed on the bottom of the resin substrate, and finally the UV coating is printed on the surface of the resin substrate, and the concave-convex texture is set on the surface of the UV coating. The shell surface is treated by the above process to replace the aluminum metal anode process, on the one hand, the shell has an excellent appearance and texture similar to the metal aluminum anode; on the other hand, the surface treatment method of the present invention greatly reduces environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A schematic diagram of an exploded structure of a shell provided by an embodiment of the present invention is shown;
[0030] Figure 2 A schematic cross-sectional view of a housing provided by an embodiment of the present invention is shown;
[0031] Figure 3 A schematic diagram showing a process of a shell surface treatment method provided by an embodiment of the present invention;
[0032] Figure 4 A schematic diagram of a shell sample provided by an embodiment of the present invention is shown.
[0033] Explanation of the reference numerals: 1. resin substrate; 11. drilled surface; 2. mirror ink layer; 3. colored ink layer; 4. metal electroplating layer; 5. ultraviolet coating. DETAILED DESCRIPTION
[0034] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0035] like Figure 1-Figure 2 The figure shows a schematic diagram of the structure of a housing provided by the present invention, and the housing comprises, from top to bottom:
[0036] A resin substrate 1 , a mirror ink layer 2 , a colored ink layer 3 and a metal electroplating layer 4 , and an ultraviolet coating 5 is also arranged on the surface of the resin substrate 1 .
[0037] The resin substrate 1 is transparent PET (polyethylene terephthalate), and the thickness of the resin substrate 1 is 0.5-1.2 mm. The edge line position of the top of the resin substrate 1 is drilled and chamfered to form a drilled surface 11; the projection width T1 of the drilled surface 11 on the bottom surface of the resin substrate 1 is 0.3-0.6 mm, and the projection width T3 of the drilled surface 11 on the side surface of the resin substrate 1 is 0.3-0.5 mm.
[0038] The mirror ink layer 2 is located at the edges of the bottom surface of the resin substrate 1 , and the width T2 of the mirror ink layer 2 is equal to the projection width T1 of the drilled surface 11 on the bottom surface of the resin substrate 1 .
[0039] The colored ink layer 3 is evenly printed on the bottom surface of the resin substrate 1, the total area of the colored ink layer 3 and the mirror ink layer 2 is equal to the total area of the bottom surface of the resin substrate 1, and there is no overlapping area between the colored ink layer 3 and the mirror ink layer 2; the thickness of the colored ink layer 3 is equal to the thickness of the mirror ink layer 2, and the thickness is 7-10μm.
[0040] The metal electroplating layer 4 is uniformly electroplated on the bottom surface of the mirror ink layer 2, and the thickness of the metal electroplating layer 4 is 0.1-0.2 μm.
[0041] The UV coating 5 is printed on the surface of the resin substrate 1, and the thickness of the UV coating 5 is 15-35 μm. In order to improve the surface texture of the shell, a concave-convex texture is embossed on the surface of the UV coating 5, and the cross-section of the embossed concave-convex structure in the embossing direction is rectangular or triangular.
[0042] like Figure 3 A schematic flow chart of a shell surface treatment method provided by an embodiment of the present invention is shown, and the method comprises:
[0043] Step S1, drilling and chamfering the edge of the top of the resin substrate to form a drilled surface;
[0044] The shell of the present invention is mainly used for the shell of electronic devices such as consumer electronic products and information technology products or the shell of internal parts of electronic devices, such as the shell of a laptop computer, the shell of a keyboard, the shell of a mobile phone back cover, the pen body shell of a stylus or the shell of a mouse, etc., and the present invention does not limit this. The shell material is resin, because the resin substrate has a lower cost than the aluminum shell, which is conducive to reducing production costs. The edge line on the top of the resin substrate is drilled and chamfered to form a drilled surface, which can bring the texture of a bright metal edge.
[0045] Step S2, printing mirror ink on the edges of the bottom surface of the resin substrate to form a mirror ink layer, wherein the printing width of the mirror ink is equal to the projection width of the drilled surface on the bottom surface of the resin substrate; the drilled surface and the mirror ink layer form a high-gloss edge on the side wall of the resin substrate;
[0046] Mirror ink is printed on the edges of the bottom surface of the resin substrate, and the printing width of the mirror ink is equal to the projection width of the drilled surface on the bottom surface of the resin substrate to ensure that the high-gloss edge effect is real, thereby improving the appearance of the shell aluminum anode.
[0047] Step S3, printing a colored ink with an imitation anode texture on the bottom surface of the resin substrate to form a colored ink layer, wherein the printing thickness of the colored ink is equal to the printing thickness of the mirror ink;
[0048] A colored ink layer is provided to enrich the color of the shell and meet the personalized color requirements of different electronic devices.
[0049] Step S4, providing a metal electroplating layer on the bottom surfaces of the colored ink layer and the mirror ink layer;
[0050] Providing a metal plating layer can increase the metallic texture of the shell and further enhance the appearance of the shell aluminum anode.
[0051] Step S5, printing a UV-curable coating on the surface of the resin substrate and pre-curing it to form a UV coating, and embossing on the surface of the UV coating to form a concave-convex texture.
[0052] Since the resin is easy to age, printing a UV-curable coating on the surface of the resin substrate can delay the aging of the resin, thereby extending the service life of the shell. The present invention further performs embossing on the surface of the pre-cured UV coating to form a concave-convex texture, thereby achieving the appearance of sandblasting or hairline on the surface of the aluminum anode. Compared with the process conditions and process costs of sandblasting or hairline, the production cost is lower and the process conditions are easier to control by embossing on the surface of the UV coating to form a concave-convex texture while ensuring the appearance of sandblasting or hairline.
[0053] In the above scheme of the present invention, the edge line on the top of the resin substrate is drilled and cut, and then the mirror ink layer, the colored ink layer, and the electroplated metal electroplated layer are layered and printed on the bottom of the resin substrate, and finally the UV coating is printed on the surface of the resin substrate, and the concave-convex texture is set on the surface of the UV coating. The shell surface is treated by the above process to replace the aluminum metal anode process. On the one hand, the shell can maintain the excellent appearance and texture of the metal aluminum anode; on the other hand, the surface treatment method of the present invention greatly reduces environmental pollution.
[0054] In one example, the resin substrate is a PET material with a glossiness greater than 90 degrees, and the thickness of the resin substrate is 0.5-1.2 mm.
[0055] PET has excellent mechanical properties, high transparency, corrosion resistance and other excellent properties. Selecting transparent PET with a glossiness greater than 90 degrees as the base material of the shell is conducive to improving the quality of the shell. The thickness of the resin substrate is controlled at 0.5-1.2mm. If the thickness of the resin substrate is less than 0.5mm, the strength of the substrate will be very low, which is not conducive to drilling and cutting around it. In order to avoid sharp edges, the drilling and cutting width needs to be controlled within 0.3, which is not conducive to the effect. If the thickness of the resin substrate is higher than 1.2mm, the strength of the substrate is too high, which is not conducive to the subsequent 3D hot pressing of the substrate, and it will also increase the overall thickness of the product.
[0056] In one example, the cutting of the edge of the top of the resin substrate by drilling and chamfering to form a drilled surface includes:
[0057] The edge line on the top of the resin substrate is drilled and chamfered at a drilling speed of 28000-36000 rpm to obtain a drilled surface with a drilling width of 0.3-0.5 mm.
[0058] The drilling width is the projection width of the drilling surface on the side of the resin substrate, for example Figure 2 T3 is the drilling width, and the T3 width is 0.3-0.5mm.
[0059] Using CNC (Computer Numerical Control) and PCD (Polycrystalline Diamond) or MCD (Manual Crystal Diamond) high-gloss cutter head, the edge of the top of the resin substrate is drilled and cut at a speed of 28,000 to 36,000 rpm to obtain a drilled surface with a smooth cross section.
[0060] In one example, the projection width of the drilled surface on the bottom surface of the resin substrate is 0.3-0.6 mm.
[0061] In one example, a metal electroplating layer is provided on the bottom surface of the colored ink layer and the mirror ink layer, comprising:
[0062] The aluminum material is placed in the vacuum coating machine with a 1×10 -4 -5×10 -4 Torr for vacuum coating.
[0063] The aluminum material is hung on the tungsten wire and placed in the vacuum coating machine. The tungsten wire is heated to melt the aluminum material hung on the tungsten wire. The aluminum material evaporates and scatters. The molten aluminum is aluminum atoms, which exist in an amorphous or liquid state and adhere to the plated object. After cooling and crystallization, it becomes an aluminum film.
[0064] The vacuum coating machine is set at 1×10 -4 -5×10-4 Torr range, 1Torr is 1mmHg. When the vacuum is too low, the evaporating aluminum encounters residual gas or the gas generated when the tungsten wire is heated, and the collision occurs and cools down. The formed aluminum particles (a collection of very small aluminum particles) will adhere to the coated part. At this time, the formed coating may still contain residual gas in the fine aluminum particles, which will make it lose its luster and greatly reduce the adhesion between the coating and the primer.
[0065] As the vacuum degree increases and the temperature of the tungsten filament increases, the kinetic energy of the evaporated aluminum will also increase. Pure aluminum (without residual gas) will adhere to the surface of the coated part, and the density will be very high, so the coating performance will be improved (including adhesion, etc.).
[0066] In one example, the thickness of the colored ink layer is 7-10 μm, and the thickness of the metal electroplating layer is 0.1-0.2 μm.
[0067] If the thickness of the metal electroplating layer is less than 0.1μm, the subsequent electronic products will be corroded and chemical changes (such as surface atomization, etc.) will be caused when other topcoats are sprayed; if the thickness of the metal electroplating layer is greater than 0.2μm, the electroplating layer will become white, affecting the appearance.
[0068] In one example, in step S5, imprinting is performed on the surface of the UV coating, including:
[0069] A structure with a concave and convex texture is prepared on a metal master;
[0070] The structure of the concavo-convex texture on the metal master is transferred to the ultraviolet coating to form a concavo-convex texture on the ultraviolet coating.
[0071] For example, a metal master with a hairline texture is engraved by laser engraving, and a concave-convex texture structure will appear on the metal master after engraving. An ultraviolet curing coating (UV coating) is sprayed on the surface of the resin substrate and pre-cured to form a UV coating. The thickness of the UV coating can be set according to demand. In this embodiment, the thickness of the UV coating is illustrated by taking 15-35 μm as an example. The metal master is then hot-pressed on the surface of the UV coating, and the embossing depth is 15-25 μm, so that the concave-convex texture on the surface of the metal master is transferred to the UV coating. In this way, a concave-convex texture structure can be presented on the surface of the UV coating, so that the surface of the shell presents a hairline effect and a concave-convex feel. After embossing, the glossiness of the UV coating surface is 10-20 degrees. The glossiness can be controlled by the depth of the texture engraved on the metal master. The deeper the texture embossing, the lower the glossiness; the shallower the texture embossing, the higher the glossiness. The shell sample obtained by the above-mentioned surface treatment method is as follows Figure 4 As shown, the sample surface has a clear hairline texture.
[0072] The present invention is further described in detail below with reference to specific embodiments.
[0073] Example 1
[0074] A shell surface treatment method, the method comprising:
[0075] Step S11, using a transparent PET with a thickness of 0.5 mm as a resin substrate, the glossiness of the transparent PET surface is greater than 90°, and using CNC and a PCD high-gloss cutter head to drill and chamfer the edge of the top of the resin substrate at a speed of 28000 rpm to form a drilled surface; the projection width T1 of the drilled surface on the bottom surface of the resin substrate is 0.3 mm, and the projection width T3 of the drilled surface on the side surface of the resin substrate is 0.3 mm;
[0076] Step S12, the resin substrate is precisely positioned by a film jig, and silver mirror ink is printed on the edges of the bottom surface of the resin substrate to form a mirror ink layer. The thickness of the mirror ink layer is 7 μm, and the printing width T2 of the silver mirror ink is equal to the projection width T1 of the drilled surface on the bottom surface of the resin substrate, that is, T2=0.3 mm; the drilled surface and the mirror ink layer form a high-gloss edge on the side wall of the resin substrate, presenting a more realistic appearance effect like a metal aluminum anode; specifically, the silver mirror ink used in this embodiment is a glossy water-based ink, and the color of the water-based ink on the Pantone color card is Pantone 877C.
[0077] Step S13, printing a semi-transparent colored ink imitating an anode texture on the bottom surface of the resin substrate to form a colored ink layer, the printing thickness of the colored ink is 7 μm; the colored ink in this embodiment is silver, which can achieve a silver metallic texture.
[0078] Step S14, electroplating a metal plating layer on the bottom surface of the colored ink layer and the mirror ink layer;
[0079] The aluminum sheet is hung on the tungsten wire and placed in a vacuum coating machine with a pressure of 10 –4 Torr, and then heat the tungsten wire to melt the aluminum flakes hanging on the tungsten wire, which evaporate and fly to all directions and adhere to the plated object. The molten aluminum is aluminum atoms, which exist in an amorphous or liquid state and adhere to the plated object. After cooling and crystallization, it becomes an aluminum film with a thickness of 0.1μm.
[0080] Step S15, printing UV-curing coating on the surface of the resin substrate and pre-curing it under 350nm ultraviolet rays, after the UV-curing coating is dried, a UV coating is formed on the surface of the resin substrate, and the thickness of the UV coating is 15μm; then, a hairline texture is engraved on the metal master by laser engraving, and then the metal master is hot-pressed on the surface of the UV coating, and the imprinting depth is 10μm. After hot pressing, a hairline texture is formed on the surface of the UV coating, and the concave-convex feeling of the hairline texture can further enhance the metal texture of the shell.
[0081] Example 2
[0082] A shell surface treatment method, the method comprising:
[0083] Step S21, using a transparent PET with a thickness of 0.9 mm as the resin substrate, the glossiness of the transparent PET surface is greater than 90°, and using CNC and a PCD high-gloss cutter head to drill and chamfer the edge of the top of the resin substrate at a speed of 32000 rpm to form a drilled surface; the projection width T1 of the drilled surface on the bottom surface of the resin substrate is 0.6 mm, and the projection width T3 of the drilled surface on the side surface of the resin substrate is 0.4 mm;
[0084] Step S22, accurately positioning the resin substrate by a film jig, printing silver mirror ink on the edges of the bottom surface of the resin substrate to form a mirror ink layer, the thickness of the mirror ink layer is 8 μm, and the printing width T2 of the silver mirror ink is equal to the projection width T1 of the drilled surface on the bottom surface of the resin substrate, that is, T2 = 0.6 mm; the drilled surface and the mirror ink layer form a high-gloss edge on the side wall of the resin substrate, presenting a more realistic metal aluminum anode-like appearance; specifically, the silver mirror ink used in this embodiment is produced by Deligao Paint Company, model number Deligao877C-F17279.
[0085] Step S23, printing a semi-transparent colored ink imitating an anode texture on the bottom surface of the resin substrate to form a colored ink layer, the printing thickness of the colored ink is 8 μm; the colored ink in this embodiment is silver, which can achieve a silver metallic texture.
[0086] Step S24, electroplating a metal plating layer on the bottom surface of the colored ink layer and the mirror ink layer;
[0087] The aluminum wire is hung on the tungsten wire and placed in a vacuum coating machine with a pressure of 3×10 -4 Torr, then heat the tungsten wire to melt the aluminum wire hanging on the tungsten wire, and the aluminum wire evaporates, scatters in all directions and adheres to the plated object. The molten aluminum is aluminum atoms, which exist in an amorphous or liquid state and adhere to the plated object. After cooling and crystallization, it becomes an aluminum film with a thickness of 0.15μm.
[0088] Step S25, printing UV-curing coating on the surface of the resin substrate and pre-curing it under 380nm ultraviolet light, after the UV-curing coating is dried, a UV coating is formed on the surface of the resin substrate, and the thickness of the UV coating is 25μm; then, a hairline texture is engraved on the metal master by laser engraving, and then the metal master is hot-pressed on the surface of the UV coating, and the imprinting depth is 15μm. After hot pressing, a hairline texture is formed on the surface of the UV coating, and the concave-convex feeling of the hairline texture can further enhance the metal texture of the shell.
[0089] Example 3
[0090] A shell surface treatment method, the method comprising:
[0091] Step S31, using a transparent PET with a thickness of 1.2 mm as the resin substrate, the glossiness of the transparent PET surface is greater than 90°, and using CNC and a PCD high-gloss cutter head to drill and chamfer the edge of the top of the resin substrate at a speed of 36000 rpm to form a drilled surface; the projection width T1 of the drilled surface on the bottom surface of the resin substrate is 0.5 mm, and the projection width T3 of the drilled surface on the side surface of the resin substrate is 0.5 mm;
[0092] Step S32, accurately positioning the resin substrate by a film jig, printing silver mirror ink on the edges of the bottom surface of the resin substrate to form a mirror ink layer, the thickness of the mirror ink layer is 10 μm, and the printing width T2 of the silver mirror ink is equal to the projection width T1 of the drilled surface on the bottom surface of the resin substrate, that is, T2 = 0.5 mm; the drilled surface and the mirror ink layer form a high-gloss edge on the side wall of the resin substrate, presenting a more realistic metal aluminum anode-like appearance; specifically, the silver mirror ink used in this embodiment is produced by Deligao Paint Company, model number Deligao877C-F17279.
[0093] Step S33, printing a semi-transparent colored ink imitating an anode texture on the bottom surface of the resin substrate to form a colored ink layer, the printing thickness of the colored ink is 10 μm; the colored ink in this embodiment is silver, which can achieve a silver metallic texture.
[0094] Step S34, electroplating a metal plating layer on the bottom surface of the colored ink layer and the mirror ink layer;
[0095] The aluminum wire is hung on the tungsten wire and placed in a vacuum coating machine with a pressure of 5×10 -4 Torr, then heat the tungsten wire to melt the aluminum wire hanging on the tungsten wire, and the aluminum wire evaporates, scatters in all directions and adheres to the plated object. The molten aluminum is aluminum atoms, which exist in an amorphous or liquid state and adhere to the plated object. After cooling and crystallization, it becomes an aluminum film with a thickness of 0.2μm.
[0096] Step S35, printing UV-curing coating on the surface of the resin substrate and pre-curing it under 400nm ultraviolet light, after the UV-curing coating is dried, a UV coating is formed on the surface of the resin substrate, and the thickness of the UV coating is 35μm; then, a hairline texture is engraved on the metal master by laser engraving, and then the metal master is hot-pressed on the surface of the UV coating, and the imprinting depth is 25μm. After hot pressing, a hairline texture is formed on the surface of the UV coating, and the convexity and concavity of the hairline texture can further enhance the metal texture of the shell.
[0097] Performance Testing
[0098] The shells prepared in Examples 1 to 3 were subjected to the following performance tests. The tests were conducted after the samples were processed and cooled and allowed to stand at room temperature for 24 hours.
[0099] Glossiness test: Use a gloss meter to test the glossiness of the standard sample (i.e., the aluminum anode shell) and the shell surface prepared in this embodiment. The qualified product condition is: glossiness difference △ = ± 5°;
[0100] Color difference test: The color difference instrument is calibrated in black and white, and the CIELAB value method is used to first test the L, a, and b values of the standard sample (i.e., the aluminum anode shell) as the standard sample, and then the L', a', and b' of the shell prepared in the embodiment are tested, and finally ΔL, Δa, Δb, and ΔE are calculated; product qualification conditions: ΔL = ±1.2, Δa = ±0.5, Δb = ±0.5, ΔE ≤1.5.
[0101] RCA wear resistance: 150 times of friction; Product qualification conditions: The surface film should have no bubbles or wrinkles, and there should be obvious different colors except for the test points, and the bottom should not be exposed at the test points.
[0102] Resistance to rubber friction: Number of times of rubber friction: 1000 times; Product qualification conditions: The surface film should have no bubbles, wrinkles, cracks, and no obvious visible discoloration.
[0103] Solvent abrasion resistance: Use 100% pure cotton white gauze stacked in 5 layers (30*30mm) at room temperature, soaked in 95% ethanol, and conduct abrasion test: 500g / cm 2 force, distance 6cm, speed 60 back and forth / min, wipe the tested area back and forth, one back and forth counts as 1 time, a total of 800 cycles, clean up after wiping, and leave it for 2 hours; Product qualification conditions: the surface film should have no bubbles, wrinkles, cracks, no obvious visible discoloration, and no color on the gauze.
[0104] Wool felt test: Use an abrasion tester at room temperature, with a load of 200g and a distance of 5CM. Use wool felt to wipe the tested area back and forth at 30 times / min. One back and forth counts as 1 time, with a total of 200,000 cycles. Clean it up after wiping. Product qualification conditions: The surface must not be damaged, and there is no obvious change in surface gloss.
[0105] Table 1 shows the performance test results.
[0106]
[0107]
[0108] The basic principles of the present application are described above in conjunction with specific embodiments. However, it should be noted that the advantages, strengths, effects, etc. mentioned in the present application are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. are required by each embodiment of the present application. In addition, the specific details disclosed above are only for the purpose of illustration and ease of understanding, not for limitation, and the above details do not limit the present application to being implemented by adopting the above specific details.
[0109] The block diagrams of the devices, apparatuses, equipment, and systems involved in this application are only illustrative examples and are not intended to require or imply that they must be connected, arranged, and configured in the manner shown in the block diagram. As will be appreciated by those skilled in the art, these devices, apparatuses, equipment, and systems can be connected, arranged, and configured in any manner. Words such as "including", "comprising", "having", etc. are open words, referring to "including but not limited to", and can be used interchangeably with them. The words "or" and "and" used here refer to the words "and / or" and can be used interchangeably with them, unless the context clearly indicates otherwise. The words "such as" used here refer to the phrase "such as but not limited to", and can be used interchangeably with them.
[0110] It should also be noted that in the apparatus, device and method of the present application, each component or each step can be decomposed and / or recombined. Such decomposition and / or recombination should be regarded as equivalent solutions of the present application.
[0111] The above description of the disclosed aspects is provided to enable any person skilled in the art to make or use the present application. Various modifications to these aspects will be readily apparent to those skilled in the art, and the general principles defined herein may be applied to other aspects without departing from the scope of the present application. Therefore, the present application is not intended to be limited to the aspects shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
[0112] The above description has been given for the purpose of illustration and description. In addition, this description is not intended to limit the embodiments of the present application to the forms disclosed herein. Although multiple example aspects and embodiments have been discussed above, those skilled in the art will recognize certain variations, modifications, changes, additions and sub-combinations thereof.
Claims
1. A shell surface treatment method, characterized in that: The method includes: Drilling and chamfering the edge of the top of the resin substrate to form a drilled surface, including: drilling and chamfering the edge of the top of the resin substrate at a drilling speed of 28000-36000 rpm to obtain a drilled surface, wherein the projection width of the drilled surface on the side of the resin substrate is 0.3-0.5 mm; the projection width of the drilled surface on the bottom of the resin substrate is 0.3-0.6 mm; the resin substrate is a PET material with a glossiness greater than 90 degrees, and the thickness of the resin substrate is 0.5-1.2 mm; printing mirror ink on the edges of the bottom of the resin substrate to form a mirror ink layer, wherein the printing width of the mirror ink is equal to the projection width of the drilled surface on the bottom of the resin substrate; the drilled surface and the mirror ink layer form a high-gloss edge on the side wall of the resin substrate; Printing a colored ink with an imitation anode texture on the bottom surface of the resin substrate to form a colored ink layer, wherein the printing thickness of the colored ink is equal to the printing thickness of the mirror ink; The metal electroplating layer is provided on the bottom surface of the colored ink layer and the mirror ink layer, including: placing the aluminum material in a vacuum coating machine, -4 -5×10 -4 Torr vacuum coating; the thickness of the colored ink layer is 7-10 μm, and the thickness of the metal electroplating layer is 0.1-0.2 μm; A UV-curable coating is printed on the surface of the resin substrate and pre-cured to form a UV coating, and embossing is performed on the surface of the UV coating to form a concave-convex texture, including: preparing a concave-convex texture structure on a metal master; transferring the concave-convex texture structure on the metal master to the UV coating to form a concave-convex texture on the UV coating; after the concave-convex texture is formed on the UV coating, the glossiness of the UV coating is 10-20 degrees.
2. A housing, characterized in that: The shell surface treatment method according to claim 1 is manufactured, and the shell comprises: A resin substrate, wherein the edge line at the top of the resin substrate is drilled and chamfered to form a drilled surface; A mirror ink layer, wherein the mirror ink layer is located around the edges of the bottom surface of the resin substrate, and the width of the mirror ink layer is equal to the projection width of the drilled surface on the bottom surface of the resin substrate; A colored ink layer, wherein the colored ink layer is disposed on the bottom surface of the resin substrate; a metal electroplating layer, the metal electroplating layer being arranged on the bottom surface of the mirror ink layer; and The UV coating is arranged on the surface of the resin substrate and has a concave-convex texture on the surface of the UV coating.
3. An electronic device, characterized in that: The invention comprises the housing as claimed in claim 2.