Application of a 3D photonic crystal metamaterial film in the preparation of time-temperature indicators
Through the combination of 3D photonic crystal metamaterial film and ionic liquid, using capillary action and microcapsule coating technology, the problems of small molecule leakage and photobleaching of existing time-temperature indicators are solved, and efficient, long-term visual temperature recording is achieved. , ensuring the accuracy and safety of the temperature change trajectory of transported items.
Patent Information
- Application Number
- CN202210824044.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-07-13
AI Technical Summary
Existing time-temperature indicators have problems such as the risk of leakage of small molecules and inconspicuous color changes, and cannot accurately record temperature changes. In particular, enzyme-type and polymerization-type indicators have the risk of chemical substance leakage, and diffusion-type indicators are prone to staining. Photobleaching.
A 3D photonic crystal metamaterial film is combined with an ionic liquid. By adjusting the composition and viscosity of the ionic liquid, capillary action is used to change the color of the photonic crystal metamaterial film to create a red-shift effect. The ionic liquid is coated with microcapsules to prevent leakage. Visual recording of temperature changes.
It achieves no small molecule leakage, efficient and long-term visual recording of the temperature change trajectory of cold chain transportation items, avoids photobleaching problems, and has relatively relaxed storage and preservation conditions.
Smart Images

Figure CN115183900B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of temperature monitoring visualization, and in particular to an application of a 3D photonic crystal metamaterial film in the preparation of a time-temperature indicator. Background Art
[0002] Time-Temperature Indicator (TTI) refers to a device that uses its own color changes to record the trajectory of temperature changes of items (medicine, fresh food, dairy products, fruits and vegetables, etc.) during cold chain transportation, so that end consumers can intuitively judge whether each item can be used later. Currently, the commonly used types of TTI are mainly diffusion type, enzyme type, polymerization type, photochromic type and microbial type, but these time-temperature indicators generally still have some problems. For example, enzyme type and polymerization type time-temperature indicators have the risk of small molecule leakage and are prone to contamination of the monitored substances; the dyes of the most commonly used diffusion type time-temperature indicators are prone to photobleaching problems, resulting in unclear color changes and inability to accurately record temperature changes. Therefore, there is an urgent need to develop more efficient time-temperature indicators.
[0003] 3D photonic crystal metamaterial film is an ordered film formed by periodically arranging materials of different refractive indexes through artificial reverse structural design. The photonic crystal metamaterial film itself does not contain any pigments and satisfies the Bragg equation through its own structure. ”, thus reflecting bright structural colors. The structural colors (i.e., the reflected wavelengths) of 3D photonic crystal metamaterials ) can be adjusted according to the Bragg formula by adjusting the observation angle ( ), the effective refractive index of the photonic crystal metamaterial ( ), lattice spacing ( ) can change the color of the photonic crystal metamaterial.
[0004] Therefore, under the premise of maintaining the structure of the 3D photonic crystal metamaterial film, the structural color it reflects can be maintained, and this material does not contain any small molecules and has no risk of chemical leakage; the color of the 3D photonic crystal metamaterial can be continuously adjusted by changing the lattice spacing, and infiltration with a liquid that matches the functional groups of the photonic crystal metamaterial matrix is one of the most effective ways to change the lattice spacing. As the "green solvent" of the 21st century, ionic liquids have the characteristics of being non-volatile and non-flammable. By changing the composition of ionic liquids, the melting temperature and viscosity of ionic liquids can be controlled. Therefore, the combination of ionic liquids and 3D photonic crystal metamaterials has great potential to become an efficient time-temperature indicator. Summary of the invention
[0005] In view of the deficiencies of the above-mentioned prior art, the object of the present invention is to provide an application of a 3D photonic crystal metamaterial film in the preparation of a time-temperature indicator; the present invention obtains a 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid response color change, which mainly consists of ionic liquid and a photonic crystal metamaterial film, and the two are connected by a liquid diffusion pad, wherein the 3D photonic crystal metamaterial film is completely placed above the liquid diffusion pad; the liquid diffusion pad is mainly composed of a material with capillary action, and can be composed of materials such as filter paper, non-woven fabric and melt-blown fabric. By designing and regulating the components of the ionic liquid, its melting temperature is matched with the storage temperature of the cold chain transported goods. When the critical temperature is exceeded, the ionic liquid melts and infiltrates the 3D photonic crystal metamaterial film by capillary action. Then, the anions of the ionic liquid match the functional groups of the 3D photonic crystal metamaterial film matrix, so that the infiltrated part is swollen by the ionic liquid, the lattice spacing between the photonic crystal building units becomes larger, and the color is red-shifted; the components of the ionic liquid are further adjusted to change the viscosity of the ionic liquid, thereby changing the capillary action speed and adjusting the indication time of the time-temperature indicator. When the temperature of the monitored item is lower than the critical temperature, the ionic liquid is solid and the color of the photonic crystal metamaterial film is maintained. The ionic liquid is encapsulated in a microcapsule. Before use, just press the microcapsule lightly to break the microcapsule to complete the activation of the time-temperature indicator, which can effectively prevent the ionic liquid from leaking during the transportation of the time-temperature indicator. This type of photonic crystal time-temperature indicator relies on the color change of the photonic crystal to record the temperature change trajectory. It is different from the pigment molecules used in the diffusion-type time-temperature indicator. It does not have the problem of small molecule leakage of polymerization-type, enzyme-type and other reaction-type time-temperature indicators. It is a greener and more efficient time-temperature indicator.
[0006] The technical solution of the present invention is specifically described as follows.
[0007] A 3D photonic crystal metamaterial film is used in the preparation of a time-temperature indicator. The 3D photonic crystal metamaterial film and an ionic liquid are used in pairs; the anions in the ionic liquid are selected from one of methanesulfonate, trifluoromethanesulfonate, hydrogen sulfate, acetate, trifluoroacetate, and tetracyanoborate; the 3D photonic crystal metamaterial film is a self-supporting film obtained by constructing hard-core soft-shell microspheres with a monodispersity index of less than 0.05 and a size between 150 nanometers and 350 nanometers of photonic crystals, and is prepared by emulsion coating-bending induced regularization technology, as follows:
[0008] First, a coating liquid is prepared, and then the coating liquid is applied to a polyethylene terephthalate (PET) film, dried, and then composited with the PET film to obtain a "PET-photonic crystal metamaterial film-PET". Then, through the bending-induced regularization processing technology, the "PET-photonic crystal metamaterial film-PET" is continuously rolled around to bend the building units in a regular arrangement in the matrix; after the roll winding is completed, the composite film is UV-cured to obtain a photonic crystal metamaterial film; wherein, the coating liquid includes a monodisperse hard-core soft-shell microsphere emulsion and a hydroxyl-containing monomer of a functional acrylic or methacrylate type. The addition of the hydroxyl-containing monomer in the coating liquid causes a large number of hydroxyl groups in the matrix of the prepared 3D photonic crystal metamaterial film to react with the polar groups in the ionic liquid, thereby changing the crystal distance of the building units in the film, and causing swelling and discoloration.
[0009] In the present invention, the color of the 3D photonic crystal metamaterial film is determined by the size of the hard-core soft-shell microspheres, and the color can be continuously adjusted between blue and red. The hard-shell soft-shell microspheres for constructing photonic crystals are mainly synthesized by semi-continuous stepwise seed emulsion polymerization. Through seed emulsion polymerization, the microspheres can be grown simultaneously, so that the particle size of the microspheres is uniform. Hard-core soft-shell microspheres can be obtained by adding monomers in stages.
[0010] In the present invention, when synthesizing hard-shell and soft-shell microspheres, the temperature of semi-continuous stepwise seed emulsion polymerization is between 65 and 95° C., preferably between 75 and 85° C. The reaction time of the seed stage is 5 to 60 minutes, preferably 10 to 40 minutes; in the stage of generating hard-core microspheres, the dropwise reaction time is 100 to 450 minutes, preferably 150 to 300 minutes, and the insulation time after the dropwise addition is 10 to 90 minutes, preferably 15 to 75 minutes; in the stage of generating soft shells, the dropwise reaction time is 150 to 500 minutes, preferably 200 to 400 minutes, and the insulation time after the dropwise addition is 10 to 90 minutes, preferably 15 to 75 minutes.
[0011] In the present invention, the hard core soft shell microspheres for constructing photonic crystals are composed of seeds, hard core and soft shell from the inside to the outside. For the seeds, the main component can be one or a combination of two of polystyrene and polymethyl methacrylate; for the hard core, its material can be inorganic, organic polymer or inorganic-organic hybrid material, and when the hard core is made of organic polymer material, its glass transition temperature is higher than 50°C; more preferably, the main component of the hard core is one or a mixture of polystyrene, polymethyl acrylate, polymethyl methacrylate, polyisobutyl methacrylate, polybenzyl acrylate, polybenzyl methacrylate, polyisobornyl acrylate, polyisobornyl methacrylate, polyacrylonitrile, silicon dioxide and ferrosoferric oxide. The crosslinking agent used for the hard core microspheres is one or a mixture of divinylbenzene, 1,4-butanediol diacrylate, allyl methacrylate, ethylene glycol dimethacrylate, dipropylene glycol diacrylate, glycidyl methacrylate, acrylamide, N-hydroxymethyl acrylamide, diacetone acrylamide and ethyl acetoacetate methacrylate. For the soft shell, a copolymer of polyacrylate and polymethacrylate is generally used. The synthetic monomers are acrylic acid, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-propyl acrylate, n-propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl acrylate, tert-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, sec-butyl acrylate, sec-butyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, 2-ethylbutyl acrylate, 2-ethylbutyl methacrylate, n-octyl acrylate, n-octyl methacrylate, isooctyl acrylate, isooctyl methacrylate, dodecyl acrylate, dodecyl methacrylate, propylene The invention can be selected from the group consisting of tetradecyl acrylate, tetradecyl methacrylate, 2-phenoxyethyl acrylate, 2-phenoxyethyl methacrylate, lauryl acrylate, lauryl methacrylate, isodecyl acrylate, isodecyl methacrylate, isobornyl acrylate, isobornyl methacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, tripropylene glycol diacrylate, tripropylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, trimethylolpropane triacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxybutyl acrylate and hydroxybutyl methacrylate, or a mixture of any of the foregoing.
[0012] In the present invention, in the semi-continuous stepwise seed emulsion polymerization, the initiator selected is one or a mixture of benzoyl peroxide, lauroyl peroxide, tert-butyl hydroperoxide, tert-butyl perbenzoate, methyl ethyl ketone peroxide, dicyclohexyl peroxydicarbonate, potassium persulfate, sodium persulfate, ammonium persulfate, azobisisobutyronitrile, and azobisisoheptylonitrile.
[0013] In the present invention, when preparing a photonic crystal metamaterial film, when preparing a coating liquid, the solid content of the monodisperse hard-core soft-shell microsphere emulsion is between 30% and 60%. In addition, 10% to 60% by mass fraction of a functional acrylic or methacrylate hydroxyl-containing monomer is added to the coating liquid, mainly one or a mixture of acrylic acid, methacrylic acid, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, hydroxybutylphenyl methacrylate, and trimethylolpropane triacrylate.
[0014] In the present invention, when preparing the coating solution, corresponding photoinitiators and auxiliary agents need to be added. The photoinitiator is one or a mixture of diphenyl ketones, acetophenones, benzoins, thioxanthones, hexaaryl diimidazoles and anthraquinones. The additive is a mixture of a leveling agent and a wetting agent, wherein the leveling agent is mainly one or a mixture of BYK306, BYK325, BYK333, BYK341, N-2218, TEGO Glide 110, TEGO Glide 406, TEGO Glide 410, TEGO Glide 440, TEGO Glide 482, EASYTECHST-5050, TERIC 320; and the wetting agent is mainly one or a mixture of TEGO Twin4000, TEGO Twin 4100, CoatOSil 2400, CoatOSil 7604, TEGO Wet KL245, EGO Wet 250, TEGO Wet 260, TEGO Wet 270, TEGO Wet 280, TEGO Wet 500, TEGO Wet 510.
[0015] In the present invention, when preparing the photonic crystal metamaterial film, the coating liquid is dried by passing through 6 sections of an oven, and the oven temperature is controlled at 65-120°C.
[0016] In the present invention, the "PET-photonic crystal metamaterial film-PET" is continuously bent around the roller through the bending induced regularization technology, resulting in relative slip between the PET films, thereby driving the matrix of the photonic crystal metamaterial film to move, shearing the microspheres to arrange regularly, and producing bright structural colors. The number of bending times around the roller is 10-36 times, the temperature of the composite film is 25-120℃ when passing the roller, and the UV curing strength is 50-900 mJ / cm 2 .
[0017] In the present invention, the anion of the ionic liquid is selected from one of methanesulfonate, trifluoromethanesulfonate, hydrogen sulfate, acetate, trifluoroacetate, and tetracyanoborate; preferably, the ionic liquid is an imidazole ionic liquid; further preferably, the ionic liquid is selected from 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, 1-propyl-3-methylimidazolium trifluoromethanesulfonate, 1-butyl-3-methylimidazolium trifluoromethanesulfonate, 1-hexyl-3-methylimidazolium trifluoromethanesulfonate, 1-ethyl-3-methylimidazolium trifluoroacetate, 1-ethyl-3-methylimidazolium hydrogen sulfate, 1-propyl-3-methylimidazolium hydrogen sulfate, 1-butyl-3-methylimidazolium hydrogen sulfate, 1-hexyl-3-methyl Imidazole hydrogen sulfate, 1-ethyl-3-methylimidazolium acetate, 1-propyl-3-methylimidazolium acetate, 1-butyl-3-methylimidazolium acetate, 1-hexyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium methyl sulfate, 1-propyl-3-methylimidazolium methyl sulfate, 1-butyl-3-methylimidazolium methyl sulfate, 1-hexyl-3-methylimidazolium methyl sulfate, 1-ethyl-3-methylimidazolium tetracyanoborate, 1-butyl-3-methylimidazolium tetracyanoborate, 1-hexyl-3-methylimidazolium tetracyanoborate, 1-octyl-3-methylimidazolium tetracyanoborate, 1-decyl-3-methylimidazolium tetracyanoborate.
[0018] In the present invention, the time-temperature indicator is a 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid response color change, which includes a cavity, a liquid diffusion pad with a porous structure is laid in the cavity, and microcapsules encapsulating ionic liquids through microfluidic technology and 3D photonic crystal metamaterial films are respectively arranged at the upper ends of the liquid diffusion pad; the liquid diffusion pad can be made of materials such as filter paper, non-woven fabrics or melt-blown fabrics. The ionic liquid is encapsulated in the microcapsule, and the time-temperature indicator can be activated by gently pressing the microcapsule before use, thereby effectively preventing the leakage of the ionic liquid during the transportation of the time-temperature indicator.
[0019] In the present invention, the monitoring temperature of the time-temperature indicator can be adjusted between -90 and 50°C by adjusting the type of ionic liquid; the monitoring time can be adjusted between 1 and 10 seconds by adjusting the type of anions combined with the parameter design of the device itself, or the complete color change time of the time-temperature indicator can be adjusted within 1 to 60 minutes, or the complete color change time can be adjusted within 1 to 72 hours. When the viscosity of the selected ionic liquid is between 1 and 100 cP and the length of the liquid diffusion pad is 0.5 cm to 2 cm, the complete color change time of the time-temperature indicator can be adjusted between 1 and 10 seconds; when the viscosity of the selected ionic liquid is between 100 and 200 cP and the length of the liquid diffusion pad is 3 to 5 cm, the complete color change time can be adjusted between 1 and 60 minutes; when the viscosity of the selected ionic liquid is between 100 cP and 600 cP and the length of the liquid diffusion pad is 8 to 12 cm, the complete color change time can be adjusted between 1 and 72 hours.
[0020] In the present invention, a time-temperature indicator is prepared by pairing a 3D photonic crystal metamaterial film containing a large number of hydroxyl groups in a matrix with an ionic liquid whose anions are selected from one of methanesulfonate, trifluoromethanesulfonate, bisulfate, acetate, trifluoroacetate, and tetracyanoborate. When the monitored ambient temperature is greater than the melting temperature of the corresponding ionic liquid, the 3D photonic crystal metamaterial film is gradually swollen by the ionic liquid as time increases, so that the lattice spacing between the photonic crystal building units becomes larger, and the color produces a red shift (color change), thereby realizing a visualized time-temperature visual indication.
[0021] The time-temperature indicator of the present invention can record the temperature change trajectory of cold chain transported items by designing the melting point of the ionic liquid to match the monitored temperature of the transported items and utilizing the swelling and discoloration effect of the ionic liquid on the photonic crystal metamaterial film; therefore, compared with the prior art, the time-temperature indicator has the following advantages:
[0022] (1) Visually record the temperature change trajectory of cold chain transportation items over a long period of time
[0023] The photonic crystal time-temperature indicator prepared by the present invention is different from the packaged time-temperature indicator. The latter relies on color pigments or dyes to produce color changes, so there are problems such as photobleaching, and it is impossible to accurately record the temperature change trajectory of the monitored object for a long time. In the present invention, the photonic crystal time-temperature indicator based on ionic liquid relies on the response of the photonic crystal metamaterial film to the ionic liquid to change color. It is a purely physical color-producing mechanism, so there is no need to worry about the photobleaching problem. In addition, the ionic liquid has extremely low volatility. After being infiltrated into the photonic crystal metamaterial film, it will be preserved for a long time, thereby recording the temperature change trajectory.
[0024] (2) Easy to store and preserve
[0025] Commonly used enzyme-type and polymer-type time-temperature indicators require harsh storage conditions to prevent them from being activated prematurely. The photonic crystal time-temperature indicator of the present invention has a stable photonic crystal metamaterial film structure, a stable developer ionic liquid, and is encapsulated in a microcapsule, so strict storage conditions are not required before activating the indicator. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the composition of a 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change.
[0027] Figure 2 Schematic diagram of the monitoring principle of 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change.
[0028] Figure 3 Transmission electron microscopy (TEM) image of hard-core soft-shell particles.
[0029] Figure 4 Changes in the reflectance spectrum of photonic crystal metamaterial films before and after ionic liquid infiltration. DETAILED DESCRIPTION
[0030] The following is a clear and complete description of the technical solution of the present invention in conjunction with specific embodiments, so that relevant technical personnel in the field can have a more comprehensive understanding of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. It should be pointed out that the protection scope of the present invention cannot be limited by this. For professional and technical personnel, without departing from the implementation principle of the present invention, several improvements and changes can be made, and these improvements and changes should also be covered by the protection scope of the embodiments of the present invention.
[0031] Example 1
[0032] This embodiment provides a preparation and implementation process of a 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change ( Figure 1 ), where the synthesized photonic crystal metamaterial film is blue in color. If the critical storage temperature of the transported item is exceeded, the ionic liquid will gradually melt and infiltrate the photonic crystal metamaterial film, causing its color to redshift. Consumers can intuitively judge the temperature change trajectory experienced by each item during transportation based on the redshift position ( Figure 2 ). The specific implementation process includes the following steps:
[0033] Step 1: Through semi-continuous stepwise seed emulsion polymerization, the implementation temperature is 75°C, the total reaction time is 450 minutes, and a hard-core soft-shell microsphere building unit with a particle size of about 220 nanometers is obtained (the specific implementation process is referred to in Chinese invention patent CN103534079 A), and the monodispersity index is less than 0.05 ( Figure 3 ), wherein the seed composition is polystyrene, and the crosslinking agent is 1,4-butanediol diacrylate; the hard core composition is polystyrene, and the crosslinking agent is 1,4-butanediol diacrylate and allyl methacrylate; the soft shell composition is polyacrylic acid, polyisobutyl methacrylate, polybutyl acrylate and polyhydroxyethyl acrylate. The initiator used is sodium persulfate.
[0034] Step 2: Prepare the coating solution. Take 100 parts by weight of the monodisperse hard-core soft-shell microsphere emulsion prepared in step 1, add 25 parts by weight of hydroxyethyl acrylate, 1 part by weight of benzophenone and 1 part by weight of EDAP, 0.5 parts by weight of wetting agent TEGO Twin4000, and 0.5 parts by weight of leveling agent BYK306, and mix thoroughly for at least 1 hour.
[0035] Step 3: The prepared coating liquid is evenly coated on the polyethylene terephthalate (PET) film by micro-concave coating, and after drying in a 75°C oven, a layer of PET film is applied.
[0036] Step 4: The composite film is bent by continuous roller winding, thereby implementing the bending-induced regular shearing technology to arrange the building units regularly in the matrix. The processing temperature is room temperature. After the roller winding is completed, the composite film is UV-cured with a UV light intensity of 300 mJ / cm 2 After solidification, a 3D sub-crystal metamaterial film is obtained.
[0037] Step 5: Use a microfluidic instrument to make 1-ethyl-3-methylimidazolium acetate ionic liquid into microcapsules with a particle size of 1-10 microns, and put them into the chamber of the pre-designed time-temperature indicator. Cut the photonic crystal metamaterial film into a specific shape and put it into the device. The two are connected by a liquid diffusion pad, and the 3D photonic crystal metamaterial film is completely placed on the liquid diffusion pad. The liquid diffusion pad is 5 cm long. Before use, gently press the microcapsule to activate the 3D photonic crystal metamaterial time-temperature indicator.
[0038] If the ambient temperature of the transported items is always below -20°C, the photonic crystal time-temperature indicator will remain blue; if the ambient temperature exceeds -20°C, the 1-ethyl-3-methylimidazolium acetate ionic liquid will melt and gradually infiltrate the photonic crystal metamaterial film through capillary action, and the color of the infiltrated part will gradually shift to red ( Figure 4), the time it takes for the photonic crystal metamaterial film to completely turn green is 30 minutes.
[0039] Example 2
[0040] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that in step 1, the soft shell is composed of polybutyl acrylate, polyisooctyl acrylate and polyhydroxyethyl methacrylate.
[0041] The prepared photonic crystal time-temperature indicator will remain blue if the ambient temperature of the transported items is always below -20°C; if the ambient temperature exceeds -20°C, the 1-ethyl-3-methylimidazolium acetate ionic liquid will melt and gradually soak the photonic crystal, causing the color of the soaked part to shift red, and it will take 30 minutes for the photonic crystal metamaterial film to completely turn green.
[0042] Example 3
[0043] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that in step 1, the soft shell is composed of poly 2-ethylhexyl acrylate, poly (isooctyl methacrylate) and poly (isobutyl acrylate).
[0044] The performance of the prepared photonic crystal time-temperature indicator is the same as that of Examples 1 and 2.
[0045] Example 4
[0046] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that in step 1, the soft shell is composed of polymethyl methacrylate, polytert-butyl methacrylate and polylauryl acrylate.
[0047] The performance of the prepared photonic crystal time-temperature indicator is the same as that of Examples 1 and 2.
[0048] Example 5
[0049] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that in step 1, the soft shell is composed of polyisobornyl acrylate, polyisooctyl acrylate, polybutyl acrylate, polyhydroxyethyl methacrylate and poly2-ethylhexyl acrylate.
[0050] The performance of the prepared photonic crystal time-temperature indicator is the same as that of Examples 1 and 2.
[0051] Example 6
[0052] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that 100 parts by weight of the monodisperse hard-core soft-shell microsphere emulsion prepared in step 1 is taken, and 10 parts by weight of acrylic acid and 15 parts by weight of hydroxyethyl methacrylate are added thereto, and 2 parts by weight of α-hydroxyacetophenone, 0.5 parts by weight of wetting agent CoatOSil 2400, and 0.5 parts by weight of leveling agent BYK333 are added at the same time, and the mixture is thoroughly mixed for at least 1 hour.
[0053] The performance of the prepared photonic crystal time-temperature indicator is the same as that of Examples 1 and 2.
[0054] Example 7
[0055] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that the oven temperature used in step 3 is 85°C.
[0056] The performance of the prepared photonic crystal time-temperature indicator is the same as that of Examples 1 and 2.
[0057] Example 8
[0058] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that the intensity of the UV curing in step 4 is 800 mJ / cm 2 .
[0059] The color change of the prepared photonic crystal time-temperature indicator is the same as that of Examples 1 and 2, except that it takes 3 hours for the photonic crystal metamaterial to completely change from blue to green.
[0060] Example 9
[0061] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that of Example 1, except that the length of the liquid diffusion pad is 10 cm.
[0062] The color change of the prepared photonic crystal time-temperature indicator is the same as that of Examples 1 and 2, except that it takes 5 hours for the photonic crystal metamaterial to completely change from blue to green.
[0063] Example 10
[0064] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that in step 5, the ionic liquid added to the chamber of the time-temperature indicator is 1-ethyl-3-methylimidazole trifluoroacetate, and the length of the liquid diffusion pad is 1.5 cm.
[0065] The prepared photonic crystal time-temperature indicator, if the ambient temperature exceeds -14°C, the photonic crystal will gradually be soaked, the color of the soaked part will shift to red, and the time it takes for the photonic crystal metamaterial film to completely turn green is 45 seconds.
[0066] Embodiment 11
[0067] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that in step 5, the ionic liquid added to the chamber of the time-temperature indicator is 1-butyl-3-methylimidazolium trifluoromethanesulfonate.
[0068] The prepared photonic crystal time-temperature indicator will remain blue if the ambient temperature of the transported items is always below 16°C; if the ambient temperature exceeds 16°C, the 1-butyl-3-methylimidazolium methyl sulfate ionic liquid will melt and gradually infiltrate the photonic crystal, causing the color of the infiltrated part to shift to red.
[0069] Example 12
[0070] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that in step 1, the particle size of the synthesized microspheres is about 270 nanometers.
[0071] The prepared photonic crystal time-temperature indicator will remain green if the ambient temperature of the transported items is always below -20°C; if the ambient temperature exceeds -20°C, the 1-ethyl-3-methylimidazolium acetate ionic liquid will melt and gradually soak the photonic crystal, causing the color of the soaked part to shift to red. It takes 30 minutes for the photonic crystal metamaterial film to completely turn red.
[0072] Example 13
[0073] The preparation and implementation process of the 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid responsive color change provided in this embodiment is the same as that in Example 1, except that in step 1, the particle size of the synthesized microspheres is about 310 nanometers.
[0074] The prepared photonic crystal time-temperature indicator will remain red if the ambient temperature of the transported items is always below -20°C; if the ambient temperature exceeds -20°C, the 1-ethyl-3-methylimidazolium acetate ionic liquid will melt and gradually infiltrate the photonic crystal, causing the color of the infiltrated part to red-shift, and the photonic crystal metamaterial film will completely disappear in 30 minutes.
[0075] Comparative Example 1
[0076] In this comparative example, a 3D photonic crystal metamaterial time-temperature indicator is prepared by a method basically the same as that in Example 1, except that, in step one, when the hard-core soft-shell microspheres are synthesized by semi-continuous stepwise seed emulsion polymerization, the soft shell components are composed of polyisobutyl methacrylate, polybutyl acrylate, polyethyl acrylate and polyethyl methacrylate; in step two, when preparing the coating liquid, 25 parts by weight of ethyl acrylate are added to 100 parts by weight of the monodisperse hard-core soft-shell microsphere emulsion, and 1 part by weight of benzophenone and 1 part by weight of EDAP, 0.5 parts by weight of a wetting agent TEGO Twin4000, and 0.5 parts by weight of a leveling agent BYK306 are added at the same time, and the mixture is thoroughly mixed for at least 1 hour.
[0077] The prepared photonic crystal time-temperature indicator will remain blue if the ambient temperature of the transported items is always below -20°C; if the ambient temperature exceeds -20°C, the 1-ethyl-3-methylimidazolium acetate ionic liquid will melt and gradually infiltrate the photonic crystal, but the color of the infiltrated part will not change.
[0078] Comparative Example 2
[0079] This comparative example adopts a method substantially the same as that of Example 1 to prepare a photonic crystal time-temperature indicator, except that in step 5, 1-butyl-3-methylimidazolium iodide ionic liquid is made into microcapsules and then added into the chamber of the time-temperature indicator.
[0080] The prepared 3D photonic crystal metamaterial time-temperature indicator will remain blue if the ambient temperature of the transported items is always below -70°C; if the ambient temperature exceeds -70°C, the 1-butyl-3-methylimidazolium iodide ionic liquid will melt and gradually infiltrate the photonic crystal, but the color of the infiltrated part will not change.
Claims
1. Application of a 3D photonic crystal metamaterial film in the preparation of a time-temperature indicator, characterized in that: The main components of the time-temperature indicator are an ionic liquid and a 3D photonic crystal metamaterial film, which are connected by a liquid diffusion pad, wherein the 3D photonic crystal metamaterial film is completely placed above the liquid diffusion pad, and the liquid diffusion pad is mainly composed of a material with a capillary effect; when the critical temperature is exceeded, the ionic liquid melts, and the 3D photonic crystal metamaterial film is infiltrated by capillary action, and then the anions of the ionic liquid are matched with the functional groups of the 3D photonic crystal metamaterial film matrix, so that the infiltrated part is swollen by the ionic liquid, the lattice spacing between the photonic crystal building units becomes larger, and the color is red-shifted; the components of the ionic liquid are further adjusted to change the viscosity of the ionic liquid, thereby changing the capillary action speed and adjusting the indication time of the time-temperature indicator; The 3D photonic crystal metamaterial film and the ionic liquid are used in pairs; the anions in the ionic liquid are selected from one of methanesulfonate, trifluoromethanesulfonate, hydrogen sulfate, acetate, trifluoroacetate, and tetracyanoborate; the 3D photonic crystal metamaterial film is a self-supporting film obtained by constructing hard-core soft-shell microspheres with a monodispersity index of less than 0.05 and a size between 150 nanometers and 350 nanometers of photonic crystals, which is prepared by emulsion coating-bending induced regularization technology, as follows: First, a coating liquid is prepared, and then the coating liquid is applied to a polyethylene terephthalate (PET) film, dried, and then compounded with the PET film to obtain a "PET-photonic crystal metamaterial film-PET". Then, through a bending-induced regularization processing technology, the "PET-photonic crystal metamaterial film-PET" is continuously bent around a roller to make the building units regularly arranged in the matrix; after the roller winding is completed, the composite film is ultraviolet-cured to obtain a photonic crystal metamaterial film; wherein the coating liquid includes a monodisperse hard-core soft-shell microsphere emulsion and a hydroxyl-containing monomer of a functional acrylic or methacrylate type.
2. The use according to claim 1, characterized in that: The hard-core soft-shell microspheres are synthesized by semi-continuous stepwise seed emulsion polymerization. The hard core in the hard-core soft-shell microspheres is made of inorganic matter, organic polymer or inorganic-organic hybrid material. When the hard core is made of organic polymer material, its glass transition temperature is higher than 50°C; the soft shell material in the hard-core soft-shell microspheres is a copolymer of polyacrylates and polymethacrylates.
3. The use according to claim 1, characterized in that: In the coating liquid, the functional acrylic monomer is one or both of acrylic acid or methacrylic acid, and the hydroxyl-containing monomer is selected from one or a mixture of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, hydroxybutylphenyl methacrylate or trimethylolpropane triacrylate.
4. The use according to claim 1, characterized in that: Photoinitiator and auxiliary agent are also added to the coating liquid; wherein the photoinitiator is one or a mixture of diphenyl ketone, acetophenone, benzoin, thioxanthone, hexaaryldiimidazole and anthraquinone; and the auxiliary agent includes a leveling agent and a wetting agent.
5. The use according to claim 1, characterized in that: In the coating liquid, the solid content of the monodisperse hard-core soft-shell microsphere emulsion is between 30% and 60%, and the hydroxyl-containing monomer of the functional acrylic acid or methacrylate ester accounts for 10% to 60% of the total mass of the coating liquid.
6. The use according to claim 1, characterized in that: The ionic liquid is an imidazolium ionic liquid.
7. The use according to claim 1, characterized in that: The ionic liquid is selected from 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, 1-propyl-3-methylimidazolium trifluoromethanesulfonate, 1-butyl-3-methylimidazolium trifluoromethanesulfonate, 1-hexyl-3-methylimidazolium trifluoromethanesulfonate, 1-ethyl-3-methylimidazolium trifluoroacetate, 1-ethyl-3-methylimidazolium hydrogen sulfate, 1-propyl-3-methylimidazolium hydrogen sulfate, 1-butyl-3-methylimidazolium hydrogen sulfate, 1-hexyl-3-methylimidazolium hydrogen sulfate, 1-ethyl-3-methylimidazolium acetate, 1-propyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, 1-propyl-3-methylimidazolium trifluoroacetate, 1-ethyl-3-methylimidazolium hydrogen sulfate, 1-propyl-3-methylimidazolium hydrogen sulfate, 1-butyl-3-methylimidazolium hydrogen sulfate, 1-hexyl-3-methylimidazolium hydrogen sulfate, 1-ethyl-3-methylimidazolium acetate, 1-propyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium trifluoromethanesulfonate, 1-ethyl-3-methylimidazolium trifluoroacetate, 1-ethyl-3-methylimidazolium hydrogen sulfate, 1-propyl-3-methylimidazolium hydrogen sulfate, 1-butyl-3-methylimidazolium hydrogen sulfate, 1-hexyl-3-methylimidazolium hydrogen sulfate, 1-ethyl-3-methylimidazolium acetate, 1-propyl-3-methylimidazolium acetate, 1-ethyl-3-methylimida One or a mixture of butyl-3-methylimidazolium acetate, 1-hexyl-3-methylimidazolium acetate, 1-ethyl-3-methylimidazolium methyl sulfate, 1-propyl-3-methylimidazolium methyl sulfate, 1-butyl-3-methylimidazolium methyl sulfate, 1-hexyl-3-methylimidazolium methyl sulfate, 1-ethyl-3-methylimidazolium tetracyanoborate, 1-butyl-3-methylimidazolium tetracyanoborate, 1-hexyl-3-methylimidazolium tetracyanoborate, 1-octyl-3-methylimidazolium tetracyanoborate, and 1-decyl-3-methylimidazolium tetracyanoborate.
8. The use according to claim 1, characterized in that: During bending induced regularization processing, the number of bending times around the roller is 10-36 times, and the temperature of the composite film when passing the roller is 25-120℃; during UV curing, the UV curing intensity is 50-900 mJ / cm 2 .
9. The use according to claim 1, characterized in that: The time-temperature indicator is a 3D photonic crystal metamaterial time-temperature indicator based on ionic liquid response color change, which includes a cavity, a liquid diffusion pad with a porous structure is laid in the cavity, and microcapsules encapsulated with ionic liquid by microfluidic technology and a 3D photonic crystal metamaterial film are respectively arranged at the two ends above the liquid diffusion pad; the microcapsule is pressed before using the time-temperature indicator to activate the time-temperature indicator; when the monitored object is below the melting temperature of the ionic liquid, the ionic liquid is solid, and the color of the photonic crystal metamaterial film does not change at this time; when the ambient temperature exceeds the melting temperature of the ionic liquid, the ionic liquid melts, and the ionic liquid uses capillary action to infiltrate the 3D photonic crystal metamaterial film, and the temperature change trajectory is recorded by observing the position of the red shift of the color of the 3D photonic crystal metamaterial film.
10. The use according to claim 9, characterized in that: The monitoring temperature of the time-temperature indicator is adjusted between -90 and 50°C, and the complete color change time range of the time-temperature indicator is adjusted between 1 and 10 seconds, or the complete color change time range is adjusted within 1 to 60 minutes, or the complete color change time range is adjusted between 1 to 72 hours.
Citation Information
Cited By
Preparation method of high-performance 3D photonic crystal structural color paint
CN119931487A
A method for preparing high-performance 3D photonic crystal structured color coatings
CN119931487B