A method for preparing an ellipsoidal nano-laser microcavity
By transforming ZnO nanorods into ZnO-MoOx nanoellipsoidal microcavity, the reflection mechanism of ellipsoidal boundary and focus is used to solve the problems of excitation mode light limitation and high order mode in nanolasers, achieving high Q value and directionality The nano-laser microcavity has simple process and low cost characteristics.
Patent Information
- Application Number
- CN202210670628.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-14
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-06-14
AI Technical Summary
Among existing nanolasers, the excitation mode light limiting factor of the echo corridor microcavity is small, and there are many high-order modes of spherical microcavity, making it difficult to study nano-scale ellipsoidal resonant cavity.
By transforming the ZnO nanorod into a ZnO-MoOx nanoellipsoidal microcavity, the total internal reflection mechanism of the ellipsoid boundary and focus is used to achieve the constraint and amplification of light, reduce the laser threshold, and improve the Q value and directionality.
It realizes a nanolaser microcavity with high Q value, single resonance mode and high directionality. It has simple process, mild conditions and low raw material cost, and is suitable for nanolasers and nanooptoelectronics.
Smart Images

Figure CN115189228B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nanometer semiconductor materials, and in particular relates to a method for preparing an ellipsoidal nanometer laser microcavity. Background Art
[0002] Laser theory and technology is one of the greatest achievements of mankind in history. It has been widely used in industrial processing, electronic information, biomedicine, national defense, basic research and other fields. As the foundation of laser theory and technology, the research and development of lasers is particularly important. The miniaturization of lasers is a very promising development direction, and related research has made great progress. At present, the size of lasers has been reduced to the nanometer level. Compared with traditional lasers, nanolasers are small in size, have excellent optoelectronic properties and rich and diverse structures, and have broad application prospects in light-matter coupling, sensing, communication, display, optical storage, nonlinear optics and other fields, creating conditions for improving the integration and transmission efficiency of optoelectronic devices and the construction of nano-optoelectronic circuits.
[0003] Semiconductor nanowire materials can be used not only as gain media for nanolasers, but also as resonant cavities, and are highly valued in the field of nanolasers. From the perspective of resonant cavities, lasers based on semiconductor nanowires mainly include Fabry-Perot and whispering gallery resonant cavities. The Fabry-Perot resonant cavity is composed of a nanowire body with a high refractive index and a flat end face. It uses the reflection of the two end faces of the nanowire to constrain the light, limiting the light energy to the axial direction of the nanowire, thereby satisfying the conditions for forming a laser. However, due to the low reflectivity of the end face, when the width of the nanowire is reduced to less than a few hundred nanometers, the end face has poor constraints on light, and due to the large surface area and the existence of Auger non-radiative recombination, the quality factor of the Fabry-Perot resonant cavity is low, and strong light excitation is required to observe the lasing phenomenon. The whispering gallery resonator allows light to propagate along the polygonal boundary of the nanowire cross section, and total internal reflection occurs at the boundary of the resonant cavity to form a resonant mode. Compared with the Fabry-Perot resonant cavity, it has a higher quality factor, a smaller resonant cavity size, high energy density, and a small mode volume. In addition, the whispering gallery microcavity is easy to prepare and has low cost. The problem with the whispering gallery microcavity is that the light confinement factor of the excitation mode is small, which means that the excitation mode is not effectively bound in the active material layer, and the light output mode is not suitable for waveguide coupling.
[0004] The performance of a whispering gallery microcavity is closely related to its shape. Compared with a disk-shaped microcavity, a spherical and ellipsoidal microcavity has a higher quality factor, but a spherical microcavity has many higher-order modes. An ellipsoidal microcavity can suppress higher-order modes and obtain a single-mode laser. In addition, an ellipsoidal microcavity can also improve the directionality of light. However, the size of the ellipsoidal microcavity currently obtained is on the order of several hundred micrometers, and there has been no research report on nanoscale ellipsoidal resonant cavities. Summary of the invention
[0005] The purpose of the present invention is to propose a method for preparing an ellipsoidal nano-laser microcavity in view of the shortcomings of the prior art. The principle of the present invention is to transform ZnO nanorods into ZnO-MoO x Nano-ellipsoidal microcavity, in addition to being able to constrain and amplify light by total internal reflection on the ellipsoidal boundary, the nano-ellipsoidal microcavity can also constrain and amplify light between the ellipsoidal interface and the ellipsoidal focus. The working principle of this method is: under the excitation of external laser, the working material located at the focus of the nano-ellipsoidal microcavity realizes particle number inversion, and the electrons at the high energy level spontaneously transition to the low energy level and spontaneously radiate photons in all directions. These photons converge to another focus after being reflected by the ellipsoidal interface. These light rays are reflected again by the ellipsoidal interface and return to the original focus. After multiple cycles between the ellipsoidal surface and the two focuses, the direction of the light rays tends to the direction of the ellipsoidal long axis, realizing the confinement and amplification of the laser in the microcavity; in addition, the ellipsoidal laser microcavity has an extremely high Q value, a single resonance mode and high directivity. The present invention has the characteristics of simple process flow, mild experimental conditions, cheap raw material price, and broad application prospects.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A method for preparing an ellipsoidal nano-laser microcavity comprises the following steps:
[0008] S1. Preparation of ZnO nanorod arrays;
[0009] S2. growing a PTCDA auxiliary layer;
[0010] The substrate with the ZnO nanorod array is immersed in a 3,4,9,10-tetracarboxylic anhydride (PTCDA) solution with a concentration of 5-15 mg / L, so that PTCDA is adsorbed on the surface of the ZnO nanorod array to obtain a PTCDA-ZnO nanorod array sample.
[0011] S3. Preparation of ZnO-MoO x Ellipsoidal nano-microcavity;
[0012] A sufficient amount of molybdenum trioxide powder is weighed; a PTCDA-ZnO nanorod array sample is placed face down directly above the molybdenum trioxide powder; and then heated in a protective gas environment by rapidly heating to 600-700°C within 10-15 minutes and maintaining the temperature for 5-30 minutes, so that the MoOx material evaporates and deposits on the PTCDA-ZnO nanorod array, and the weak parts of the ZnO nanorods are also evaporated; and finally, the sample is naturally cooled to room temperature to obtain a ZnO-MoOx ellipsoidal nano-microcavity.
[0013] The present invention utilizes the properties of the ellipsoidal reflector to make the laser working material into an ellipsoidal nano-microcavity, so that the light forms a circular amplification between the ellipsoidal surface and two focal points. When preparing the ellipsoidal nano-microcavity, the characteristic that the defective parts of the ZnO nanorods are easy to evaporate during the rapid heating process and the evaporation deposition characteristics of the MoOx material are cleverly utilized, and the ZnO-MoOx ellipsoidal nano-microcavity is obtained under a specific heating method.
[0014] The preparation method of the ellipsoidal nano-microcavity provided by the present invention has a scientific principle, a simple preparation process of the required ZnO nanorod array and MoOx materials, mild reaction conditions, and low costs of raw materials and equipment; compared with the ZnO nanorod material, the ZnO-MoOx ellipsoidal nano-microcavity has a lower lasing threshold. The principle and method of the present invention are expected to be applied to nano-lasers and nano-optoelectronics, and have great promotion and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 Schematic diagram of the principle of the ellipsoidal nano-micro cavity of the present invention;
[0016] Figure 2 ZnO nanorod arrays (a) and ZnO-MoO x Scanning electron microscopy image of the ellipsoidal nanocavity (b);
[0017] Figure 3 For ZnO nanorod arrays and ZnO-MoO x Emission spectra of ellipsoidal nanocavities, where the lasing phenomenon is from ZnO-MoO x Ellipsoidal nanocavity. DETAILED DESCRIPTION
[0018] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and drawings.
[0019] S1. Preparation of ZnO nanorod arrays; specifically comprising the following steps:
[0020] S11. Cleaning the substrate: ultrasonically clean a silicon substrate (1 cm×1 cm) in acetone, ethanol, and deionized water solution for 15 minutes, and then blow dry the substrate with air.
[0021] S12. Preparation of ZnO seed layer: prepare an ethanol solution of zinc acetate (15 mmol / L); then drop the ethanol solution of zinc acetate onto the front side (polished side) of the silicon substrate so that the solution covers the entire surface of the substrate, wait for 10 minutes and then blow the solution dry with air; repeat this process 10 times; then place the substrate in an air environment for heat treatment at 300°C for 1 hour to obtain a substrate with a ZnO seed layer.
[0022] S13. Preparation of ZnO nanorod arrays;
[0023] A 50 mmol / L zinc nitrate aqueous solution and a hexamethylenetetramine aqueous solution were mixed in a 1:1 ratio and magnetically stirred for 20 minutes to obtain a uniformly mixed solution. A substrate with a ZnO seed layer was placed in the mixed solution, and the substrate floated face down on the surface of the mixed solution. Finally, the substrate was grown at a constant temperature of 80°C in a drying oven for 6 hours, the substrate was taken out and the surface was washed with deionized water, and the substrate with a ZnO nanorod array was obtained after drying.
[0024] S2. growing a PTCDA auxiliary layer;
[0025] The substrate with the ZnO nanorod array was immersed in a 10 mg / L 3,4,9,10-tetracarboxylic anhydride (PTCDA) solution for 5 minutes to allow PTCDA to adsorb on the surface of the ZnO nanorods. The substrate was taken out and dried to obtain a PTCDA-ZnO nanorod array sample with a PTCDA auxiliary layer.
[0026] S3. Preparation of ZnO-MoO x Ellipsoidal nano-microcavity;
[0027] 0.4 g of molybdenum trioxide (MoO3) powder was weighed and placed in a ceramic boat; the PTCDA-ZnO nanorod array sample was placed face down on the ceramic boat containing MoO3 powder without contacting the MoO3 powder; the ceramic boat was placed in the center of the heating zone of a quartz tube furnace; at room temperature, argon gas (99.99% high-purity argon gas) was introduced into the quartz tube furnace at a flow rate of 50 SCCM for more than 10 minutes to remove the air in the tube; while maintaining the ventilation condition, the quartz tube furnace was rapidly heated to 650°C within 10-15 minutes and maintained for 20 minutes; then naturally cooled to room temperature to obtain ZnO-MoO x Ellipsoidal nanocavity.
[0028] Figure 2 ZnO nanorod array (a) and ZnO-MoO prepared in this example x The scanning electron microscope image of the ellipsoidal nanocavity (b) shows that the ZnO nanorod is in the shape of a hexagonal prism with a side length of about 200 nm. x The sample is composed of ellipsoidal nanoparticles connected together, and the major axis size of the ellipsoid is about 500nm.
[0029] Figure 3 The ZnO nanorod array and the ZnO-MoO prepared in this example x Emission spectra of ellipsoidal nanocavities, where the lasing phenomenon is from ZnO-MoO xEllipsoidal nano-microcavity, ZnO nanorod sample only has fluorescence emission phenomenon, and its fluorescence spectrum is a very wide emission band. Different from ZnO nanorod sample, ZnO-MoO x The ellipsoidal nano-microcavity has multiple sharp laser emission peaks, and the half-width of the laser emission peak is only about 0.5nm. x The ellipsoidal nanolaser microcavity has lower laser excitation power than ZnO nanorod materials and has more application scenarios.
Claims
1. A method for preparing an ellipsoidal nano-laser microcavity, characterized in that: The following steps are involved: S1. Preparation of ZnO nanorod arrays; S2. growing a PTCDA auxiliary layer; The substrate having the ZnO nanorod array is immersed in a 3,4,9,10-tetracarboxylic anhydride solution to allow PTCDA to be adsorbed on the surface of the ZnO nanorod array to obtain a PTCDA-ZnO nanorod array sample; S3. Preparation of ZnO-MoO x Ellipsoidal nano-microcavity; A sufficient amount of molybdenum trioxide powder is weighed; a PTCDA-ZnO nanorod array sample is placed face down directly above the molybdenum trioxide powder; and then heated in a protective gas environment by rapidly heating to 600-700°C within 10-15 minutes and maintaining the temperature for 5-30 minutes, so that the MoOx material evaporates and deposits on the PTCDA-ZnO nanorod array, and at the same time, the weak parts of the ZnO nanorods are evaporated; and finally, the sample is naturally cooled to room temperature to obtain a ZnO-MoOx ellipsoidal nano-microcavity.
2. The method for preparing an ellipsoidal nano-laser microcavity according to claim 1, characterized in that: The concentration of the 3,4,9,10-tetracarboxylic anhydride solution is 5-15 mg / L.