A method and system for removing boron and concentrating lithium from high-boron lithium liquid

Through the acidification ultrafiltration, electrodialysis and deep boron deboration methods of high boron-containing lithium liquid, the problems of low boron removal rate and large water consumption in lithium extraction in salt lakes are solved, and efficient lithium resource recycling and boron recovery are achieved. Content control, suitable for large-scale applications.

CN115196655BActive Publication Date: 2024-11-22HANGZHOU CREATE ENVIRONMENTAL ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211009428.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-23
Publication Date
2024-11-22
Estimated Expiration
2042-08-23

AI Technical Summary

Technical Problem

The existing boron removal process has problems such as low boron removal rate, high consumption of water and acid and alkali resources, and is not suitable for large-scale applications in the treatment of high boron lithium. Especially in the process of lithium extraction in salt lakes, due to the complex nature of boron elements. Increases process difficulty and complexity.

Method used

After acidification and ultrafiltration of high boron-containing lithium liquid, the first and second stage electrodialysis treatments were carried out, combined with the boron removal resin to deeply deborate, and lithium carbonate was obtained through evaporation and concentration, which achieved high boron removal rate and lithium recovery rate. and methods that consume less acid and alkali resources.

Benefits of technology

The boron removal rate and lithium recovery rate of high boron-containing lithium liquid are improved, ensuring that the boron content of the final lithium product meets the battery level requirements, and reducing the consumption of water resources and acid and alkali resources, making it suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115196655B_ABST
    Figure CN115196655B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of boron-containing lithium liquid treatment, and provides a method and system for removing boron from a high-boron-containing lithium liquid and concentrating lithium. The present invention uses a first-stage electrodialysis to concentrate lithium in the solution while achieving boron removal, and uses a second-stage electrodialysis to recover lithium resources from the first-stage electrodialysis produced water, and further reduces the boron content in the recovered lithium; and the present invention further reduces the boron content in the solution to less than 5ppm through a resin boron removal process, ensuring that the boron content of the final lithium product meets the battery-grade requirements. In addition, the present invention can also use a bipolar membrane electrodialysis system to treat the lithium-rich refined liquid obtained after the resin boron removal, and then obtain a battery-grade lithium hydroxide solid by evaporation and crystallization. The method provided by the present invention has a high boron removal rate and lithium recovery rate, and boron enrichment will not occur in the lithium-rich refined liquid. The boron content of the lithium product finally obtained meets the battery-grade requirements, and the consumption of water resources and acid-base resources is small, which is suitable for large-scale application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of boron-containing lithium liquid treatment, and in particular to a method and system for removing boron and concentrating lithium in high-boron-containing lithium liquid. Background Art

[0002] With the rapid recovery of the new energy vehicle market, the demand for power batteries has continued to rise. At the same time, energy storage applications have further widened the gap between supply and demand of lithium resources. At present, salt lake brine-type lithium resources account for nearly 60% of the world's lithium resources. Salt lake lithium extraction technology will become an important part of the global lithium resource supply system.

[0003] Although China's lithium resources rank fourth in the world, 70% of them are salt lake lithium resources, which are mainly concentrated in the Qinghai-Tibet Plateau and Qinghai Salt Lake. They are characterized by a high magnesium-to-lithium ratio. Currently, large-scale potash fertilizer production capacity has been built, and lithium extraction capacity is in the growth stage. The lithium concentration in Tibet's salt lakes is generally higher, but due to weak infrastructure, harsh conditions at high altitudes and strict environmental protection requirements, they have not yet been fully developed.

[0004] Salt lake brine generally contains elements such as calcium, magnesium, boron, and lithium. Currently, in the process of lithium extraction, there are relatively mature and complete processes for the removal of calcium and magnesium. However, since the boron element exhibits different properties under different water quality conditions, the difficulty of lithium extraction and the complexity of the process are increased.

[0005] Existing boron removal processes include acid boron removal, extraction boron removal, reverse osmosis boron removal, nanofiltration boron removal, and reverse osmosis-secondary electrodialysis coupling process boron removal, etc. Among them, the acid boron removal method is to separate crude boric acid by adding hydrochloric acid to form a boric acid precipitate. The boron removal rate of this method is low and the acid consumption is large; although the boron removal rate of extraction boron removal is high, the organic solvent will enter the raffinate, which cannot meet the requirements of safety and environmental protection, and will bring great restrictions to the subsequent membrane process. Reverse osmosis boron removal and nanofiltration boron removal require a large amount of water resources and acid and alkali resources, which limit their large-scale application in places where water is scarce and acid and alkali transportation is extremely inconvenient. The reverse osmosis-secondary electrodialysis coupling process is to inject part of the reverse osmosis produced water into the concentration chamber of the first electrodialysis system, and at the same time inject the primary concentrated solution into the dilute chamber of the first electrodialysis. During the electrodialysis process, the solution concentration in the concentrated chamber increases, while the solution concentration in the dilute chamber decreases. In this way, after electrodialysis, a boron-rich solution is obtained in the dilute chamber, and a boron-lithium separation mother liquor is obtained in the concentrated chamber, realizing the separation of boron and lithium. Although the boron removal rate of the reverse osmosis-secondary electrodialysis coupling process can reach more than 85%, since reverse osmosis will enrich boron, it cannot solve the problem of high boron content in lithium-rich solution.

[0006] Therefore, there is an urgent need to provide a method for removing boron and concentrating lithium in a high-boron-containing lithium solution that has a high boron removal rate and lithium recovery rate, consumes less water and acid and alkali resources, and is suitable for large-scale application. Summary of the invention

[0007] The object of the present invention is to provide a method and system for removing boron from a high-boron-containing lithium liquid and concentrating lithium. The method for removing boron from a high-boron-containing lithium liquid and concentrating lithium provided by the present invention has a high boron removal rate and a lithium recovery rate, and no boron enrichment will occur in the obtained lithium-rich refined liquid. The boron content of the lithium product finally obtained meets the battery-grade requirements, and the method of the present invention consumes less water and acid-base resources and is suitable for large-scale application.

[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0009] A method for removing boron from a high-boron lithium liquid and concentrating lithium, comprising the following steps:

[0010] (1) acidifying the high-boron lithium liquid and then ultrafiltering to obtain a purified high-boron lithium liquid; the high-boron lithium liquid has a Li content of 1.5 to 7 g / L and a B content of 1.2 to 5 g / L;

[0011] (2) subjecting the purified high-boron-containing lithium liquid to a first-stage electrodialysis treatment to obtain a first-stage deborated concentrated liquid and a first-stage boron-rich desalinated liquid;

[0012] (3) subjecting the primary boron-rich desalinated liquid to a second-stage electrodialysis treatment to obtain a secondary deboronized concentrated liquid and a secondary boron-rich desalinated liquid; the secondary deboronized concentrated liquid is returned to step (2) for the first-stage electrodialysis treatment;

[0013] (4) adjusting the pH value of the primary deboronized concentrated solution to 8 to 14, and then performing deep deboronization using a boron removal resin to obtain a lithium-rich refined solution;

[0014] (5) adjusting the pH value of the lithium-rich refined solution to 6 to 8 and then evaporating and concentrating it to obtain a solution to be precipitated with lithium; mixing the solution to be precipitated with a sodium carbonate solution to precipitate lithium to obtain lithium carbonate;

[0015] There is no time limit for the steps (3) and (4).

[0016] Preferably, the content of high-valent metal ions in the high-boron lithium liquid is less than 1 ppm, the Na content is 1.25-10 g / L, the K content is 1-3 g / L, and the mass ratio of Li to Na is greater than 0.8; the valence of the high-valent metal ions is +2 or above.

[0017] Preferably, the acidification is based on adjusting the pH value of the high-boron lithium liquid to 1-6.5; the pore size of the ultrafiltration filter membrane is 0.01-0.05 μm; before the ultrafiltration, the acidified high-boron lithium liquid is filtered; the pore size of the filtration filter membrane is 50-100 μm.

[0018] Preferably, the receiving liquid on the concentrated water side of the first-stage electrodialysis treatment is one or more of lithium chloride solution, sodium chloride solution, potassium chloride solution and pure water; the current density of the first-stage electrodialysis treatment is 300-450A / m 2 , the membrane voltage is 0.7~1.2V;

[0019] The first deboronized concentrated solution has a Li content of 12 to 18 g / L, a Na content of 8 to 12 g / L, a K content of 5 to 8 g / L, and a B content of 0.1 to 1.8 g / L.

[0020] Preferably, the current density of the second stage electrodialysis treatment is 100-400 A / m 2 , the membrane voltage is 0.7~1.2V;

[0021] The content of Li in the secondary boron-rich desalinated liquid is 0.02-0.1 g / L, the content of Na is 0.01-0.2 g / L, the content of K is 0.01-0.3 g / L, and the content of B is 1.3 g-5.2 g / L; the secondary boron-rich desalinated liquid is subjected to boron extraction treatment.

[0022] Preferably, the boron removal resin is a macroporous boron removal adsorption resin; and the content of B in the lithium-rich refined liquid is less than 0.01 g / L.

[0023] Preferably, step (5) is replaced by:

[0024] The lithium-rich solution is subjected to bipolar membrane electrodialysis treatment to obtain a lithium hydroxide solution and a dilute lithium solution; the dilute lithium solution and the purified high-boron lithium solution are mixed and returned to the first-stage electrodialysis treatment step; the lithium hydroxide solution is evaporated and crystallized to obtain lithium hydroxide.

[0025] Preferably, the condensed water produced by the evaporative crystallization is used as system replenishment water for the first-stage electrodialysis treatment and the second-stage electrodialysis treatment.

[0026] The present invention also provides a system for removing boron and concentrating lithium from a high-boron lithium liquid, comprising:

[0027] Security filters;

[0028] an ultrafiltration system connected to the outlet of the security filter;

[0029] a primary electrodialysis system connected to the filtrate outlet of the ultrafiltration system;

[0030] A secondary electrodialysis system connected to the fresh water outlet of the primary electrodialysis system; the concentrated water outlet of the secondary electrodialysis system is connected to the inlet of the primary electrodialysis system;

[0031] a boron removal resin system connected to the concentrate outlet of the primary electrodialysis system;

[0032] an MVR system in communication with an outlet of the boron removal resin;

[0033] A lithium sinking unit is connected to the outlet of the MVR system.

[0034] Preferably, the lithium precipitation unit is replaced with a bipolar membrane system, the lithium hydroxide solution outlet of the bipolar membrane system is connected to the inlet of the MVR system, the dilute acid outlet of the bipolar membrane system is connected to the boron removal resin system, and the dilute lithium solution outlet of the bipolar membrane system is connected to the inlet of the primary electrodialysis system.

[0035] The invention provides a method for removing boron and concentrating lithium from a high-boron lithium liquid. The method comprises the following steps: acidifying and ultrafiltering the high-boron lithium liquid to obtain a purified high-boron lithium liquid; then subjecting the purified high-boron lithium liquid to a first-stage electrodialysis treatment to obtain a first-stage deborated concentrated liquid and a first-stage boron-rich desalinated liquid; subjecting the boron-rich desalinated liquid to a second-stage electrodialysis treatment to obtain a second-stage deborated concentrated liquid and a second-stage boron-rich desalinated liquid; mixing the second-stage deborated concentrated liquid with the purified high-boron lithium liquid and returning to the first-stage electrodialysis treatment step; deeply deborating the first-stage deborated concentrated liquid by using a boron removal resin to obtain a lithium-rich refined liquid; and evaporating and concentrating the lithium-rich refined liquid and using sodium carbonate to precipitate lithium to obtain lithium carbonate. The present invention uses a first-stage electrodialysis to remove boron and concentrate lithium in the solution, and uses a second-stage electrodialysis to recover lithium resources from the first-stage electrodialysis produced water, and further reduce the boron content in the recovered lithium. Finally, through two-stage electrodialysis, a lithium resource recovery rate of more than 95% is achieved; and the present invention further reduces the boron content in the solution to less than 5ppm through a resin boron removal process, ensuring that the boron content of the final lithium product meets battery-grade requirements.

[0036] Furthermore, the present invention can also use a bipolar membrane electrodialysis system to treat the lithium-rich refined liquid obtained after the resin removes boron, and then obtain battery-grade lithium hydroxide solid by evaporation and crystallization.

[0037] The method for removing boron and concentrating lithium from a high-boron-containing lithium liquid provided by the present invention has high boron removal rate and lithium recovery rate, and no boron enrichment will occur in the obtained lithium-rich refined liquid. The boron content of the lithium product finally obtained meets the battery-grade requirements, and the consumption of water resources and acid-base resources is small, so the lithium product is suitable for large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 A schematic diagram of the structure of a system for removing boron from high-boron lithium liquid and concentrating lithium (excluding a bipolar membrane electrodialysis system);

[0039] Figure 2 A schematic diagram of the structure of a system for removing boron from high-boron lithium liquid and concentrating lithium (including a bipolar membrane electrodialysis system);

[0040] Figures 1-2 In: 1-security filter, 2-ultrafiltration system, 3-primary electrodialysis system, 4-secondary electrodialysis system, 5-boron removal resin system, 6-MVR system, 7-lithium precipitation unit, 8-bipolar membrane electrodialysis system. DETAILED DESCRIPTION

[0041] The present invention provides a method for removing boron and concentrating lithium from a high-boron lithium liquid, comprising the following steps:

[0042] (1) acidifying the high-boron lithium liquid and then ultrafiltering to obtain a purified high-boron lithium liquid; the high-boron lithium liquid has a Li content of 1.5 to 7 g / L and a B content of 1.2 to 5 g / L;

[0043] (2) subjecting the purified high-boron-containing lithium liquid to a first-stage electrodialysis treatment to obtain a first-stage deborated concentrated liquid and a first-stage boron-rich desalinated liquid;

[0044] (3) subjecting the primary boron-rich desalinated liquid to a second-stage electrodialysis treatment to obtain a secondary deboronized concentrated liquid and a secondary boron-rich desalinated liquid; the secondary deboronized concentrated liquid is returned to step (2) for the first-stage electrodialysis treatment;

[0045] (4) adjusting the pH value of the primary deboronized concentrated solution to 8 to 14, and then performing deep deboronization using a boron removal resin to obtain a lithium-rich refined solution;

[0046] (5) adjusting the pH value of the lithium-rich refined solution to 6 to 8 and then evaporating and concentrating it to obtain a solution to be precipitated with lithium; mixing the solution to be precipitated with a sodium carbonate solution to precipitate lithium to obtain lithium carbonate;

[0047] There is no time limit for the steps (3) and (4).

[0048] The present invention acidifies the high-boron lithium liquid and then performs ultrafiltration to obtain a purified high-boron lithium liquid. In the present invention, the content of Li in the high-boron lithium liquid is 1.5-7g / L, preferably 2-6g / L, and the content of B is 1.2-5g / L, preferably 1.5-4.5g / L; the content of high-valent metal ions in the high-boron lithium liquid is preferably <1ppm, the content of Na is preferably 1.25-10g / L, the content of K is preferably 1-3g / L, and the mass ratio of Li and Na is preferably greater than 0.8; the high-valent metal ions are preferably divalent and above metal ions, specifically calcium ions and / or magnesium ions; the high-boron lithium liquid in the present invention is specifically a magnesium-removing high-boron lithium liquid, and the present invention has no restrictions on the source of the magnesium-removing high-boron lithium liquid, which can be prepared from sodium chloride, lithium chloride, and boron oxide, or can be an enriched liquid obtained by removing impurities and hardness from salt lake brine and enriching lithium, sodium, potassium, boron and other elements in a known manner (nanofiltration, reverse osmosis).

[0049] In the present invention, the acidification is preferably based on adjusting the pH value of the high boron-containing lithium solution to 1-6.5, preferably to 2-6, and the acidification reagent is preferably one or both of hydrochloric acid and sulfuric acid, and the mass fractions of the hydrochloric acid and sulfuric acid are independently preferably 3-30%.

[0050] In the present invention, the pore size of the ultrafiltration membrane is preferably 0.01-0.05 μm; before the ultrafiltration, the acidified high-boron lithium liquid is preferably filtered; the pore size of the filtration membrane is preferably 50-100 μm; the filtration is preferably filtered using a security filter. The present invention reduces the content of suspended matter and macromolecular dissolved matter in the high-boron lithium liquid through ultrafiltration, preventing contamination of subsequent membrane systems and resin units.

[0051] After obtaining the purified high-boron lithium liquid, the present invention performs a first-stage electrodialysis treatment on the purified high-boron lithium liquid to obtain a first-stage deboronized concentrated liquid and a first-stage boron-rich desalinated liquid. In the present invention, the receiving liquid on the concentrated water side of the first-stage electrodialysis treatment is preferably one or more of lithium chloride, sodium chloride, potassium chloride and pure water, and the content of B in the receiving liquid is preferably less than 0.1ppm; the current density of the first-stage electrodialysis treatment is preferably 300-450A / m 2 , more preferably 350 to 400 A / cm 2 The membrane pair voltage of the first-stage electrodialysis treatment is preferably 0.7-1.2V, more preferably 0.7-1V; the dialysis membrane used in the first-stage electrodialysis treatment is preferably a styrene divinylphenyl anion and cation exchange membrane, or a styrene-based anion and cation exchange membrane. In the present invention, the content of Li in the first deboronated concentrated solution is preferably 12-18g / L, the content of Na is preferably 8-12g / L, the content of K is preferably 5-8g / L, and the content of B is preferably 0.1-1.8g / L.

[0052] After obtaining the primary boron-rich desalinated liquid, the present invention subjects the primary boron-rich desalinated liquid to a second-stage electrodialysis treatment to obtain a secondary deborated concentrated liquid and a secondary boron-rich desalinated liquid; the secondary deborated concentrated liquid is returned to step (2) for the first-stage electrodialysis. In a specific embodiment of the present invention, the secondary deborated concentrated liquid is preferably mixed with the purified high-boron lithium liquid, and then the first-stage electrodialysis treatment is performed together. In the present invention, the receiving liquid on the concentrated water side of the second-stage electrodialysis treatment is preferably one or more of lithium chloride, sodium chloride, potassium chloride and pure water, and the content of B in the receiving liquid is preferably less than 0.1ppm; the current density of the second-stage electrodialysis treatment is preferably 100-400A / m 2 , more preferably 100 to 300 A / cm 2, the membrane pair voltage of the first-stage electrodialysis treatment is preferably 0.7-1.2V, more preferably 0.7-1V; the type of dialysis membrane used in the second-stage electrodialysis treatment is consistent with that of the first-stage electrodialysis treatment, which will not be repeated here. The first-stage boron-rich desalination liquid contains a small amount of Li, Na, K, Cl, sulfate ions, etc. The present invention desalinates the first-stage boron-rich desalination liquid through the second-stage electrodialysis, and migrates the Li, Na, K, Cl, sulfate ions, etc. in the first-stage boron-rich desalination liquid to the concentrated water side to obtain a second-stage deboronized concentrated liquid, and the second-stage deboronized concentrated liquid is mixed with the purified high-boron lithium liquid, and then enters the first-stage electrodialysis for re-concentration and deboronization treatment, thereby recovering lithium resources. In the present invention, the content of Li in the secondary boron-rich desalinated liquid is preferably 0.02-0.1 g / L, the content of Na is preferably 0.01-0.2 g / L, the content of K is preferably 0.01-0.3 g / L, and the content of B is preferably 1.3 g-5.2 g / L; the secondary boron-rich desalinated liquid is preferably subjected to boron extraction treatment; the present invention has no special requirements on the specific operating conditions of the boron extraction treatment, and the operating conditions familiar to those skilled in the art can be adopted. The present invention recovers fresh water resources and boron resources through boron extraction treatment.

[0053] After obtaining the primary deboronized concentrated solution, the present invention adjusts the pH value of the primary deboronized concentrated solution to 8-14, and then uses a boron removal resin for deep deboronization to obtain a lithium-rich refined solution. In the present invention, the reagent used to adjust the pH value of the primary deboronized concentrated solution is preferably a sodium hydroxide solution, a potassium hydroxide solution or a lithium hydroxide solution, and the mass fraction of the sodium hydroxide solution, the potassium hydroxide solution or the lithium hydroxide solution is independently preferably 3-10%; the boron removal resin is preferably a macroporous boron removal adsorption resin. The present invention has no special requirements for the macroporous boron removal adsorption resin, and the commercially available resin known to those skilled in the art can be used. In a specific embodiment of the present invention, a polystyrylamine polyhydroxy type boron removal resin is used, and the total exchange capacity of the resin is ≥0.5meq / mL; the content of B in the lithium-rich refined solution is preferably less than 0.01g / L.

[0054] After obtaining the lithium-rich refined liquid, the present invention adjusts the pH value of the lithium-rich refined liquid to 6 to 8 and then evaporates and concentrates it to obtain a solution to be precipitated with lithium; the solution to be precipitated with lithium is mixed with a sodium carbonate solution to precipitate lithium to obtain lithium carbonate. In the present invention, the reagent used to adjust the pH value of the lithium-rich refined liquid is preferably hydrochloric acid and / or sulfuric acid, and the mass fraction of the hydrochloric acid and sulfuric acid is preferably 3 to 30% independently; the content of Li in the solution to be precipitated with lithium is preferably 22 to 28 g / L; the present invention has no special requirements for the specific conditions of the evaporation and concentration, and the conditions familiar to those skilled in the art can be used; the condensed water generated during the evaporation and concentration process is preferably used as process water for the first-stage electrodialysis treatment and the second-stage electrodialysis treatment.

[0055] The present invention has no special requirements on the amount and concentration of the sodium carbonate solution, and it can be added according to conditions familiar to those skilled in the art. The present invention converts lithium in the solution into lithium carbonate by adding sodium carbonate, and the obtained lithium carbonate precipitate is filtered and dried to obtain a finished lithium carbonate product, and the obtained finished lithium carbonate product meets battery grade requirements.

[0056] In the present invention, after obtaining the lithium-rich solution, the lithium-rich solution may be further subjected to the following treatment to obtain a lithium hydroxide product, the specific steps being as follows:

[0057] The lithium-rich solution is subjected to bipolar membrane electrodialysis treatment to obtain a lithium hydroxide solution and a dilute lithium solution; the dilute lithium solution and the purified high-boron lithium solution are mixed and returned to the first-stage electrodialysis treatment step; the lithium hydroxide solution is evaporated and crystallized to obtain lithium hydroxide.

[0058] In the present invention, the bipolar membrane electrodialysis treatment system (i.e., bipolar membrane electrodialysis system) preferably includes an anode, an anode membrane, a plurality of repeated membrane units, a cathode membrane, and a cathode arranged in sequence from left to right; a membrane unit preferably includes a bipolar membrane, an anion exchange membrane, a cation exchange membrane, and a bipolar membrane arranged in sequence, a salt chamber is provided between the anion exchange membrane and the cation exchange membrane, an acid chamber is provided between the bipolar membrane and the anion exchange membrane, and an alkali chamber is provided between the bipolar membrane and the cation exchange membrane; the lithium-rich refined liquid is introduced into the salt chamber, the initial solution in the acid chamber is water, after electrolysis, the anions in the lithium-rich refined liquid migrate to the acid chamber, and combine with the hydrogen ions decomposed from the bipolar membrane cation surface to generate acid, and the Li, Na, and K ions in the lithium-rich refined liquid migrate to the alkali chamber, and combine with the hydroxide ions decomposed from the bipolar membrane anion surface to generate LiOH, NaOH, and KOH. The alkaline solution obtained in the alkali chamber is the lithium hydroxide solution, which also contains a small amount of sodium hydroxide and potassium hydroxide, and battery-grade lithium hydroxide solid can be obtained by evaporation and crystallization. In the present invention, the operating voltage of the bipolar membrane electrodialysis treatment is preferably 1.0 to 3.0 V per membrane pair, and the current density is preferably 300 to 800 A / m 2 . In the present invention, a dilute acid solution with a concentration of about 0.1 to 2 mol / L is obtained in the acid chamber of the bipolar membrane electrodialysis system; the present invention preferably uses the dilute acid solution for the regeneration of the macroporous boron removal adsorption resin to achieve internal recycling of resources. In the present invention, the solution remaining after the bipolar membrane electrodialysis treatment is a dilute lithium solution, wherein the Li content is about 3 to 5 g / L; the present invention preferably mixes the dilute lithium solution with the purified high-boron lithium solution and returns it to the first electrodialysis treatment step to achieve lithium recovery. The present invention has no special requirements for the specific conditions of the evaporation and crystallization of the lithium hydroxide solution, and the conditions familiar to those skilled in the art can be used; the condensed water generated during the evaporation and crystallization process is preferably used as process water for the first-stage electrodialysis treatment and the second-stage electrodialysis treatment.

[0059] The present invention also provides a system for removing boron and concentrating lithium from a high-boron-containing lithium liquid, comprising:

[0060] Security filters;

[0061] an ultrafiltration system connected to the outlet of the security filter;

[0062] a primary electrodialysis system connected to the filtrate outlet of the ultrafiltration system;

[0063] A secondary electrodialysis system connected to the fresh water outlet of the primary electrodialysis system; the concentrated water outlet of the secondary electrodialysis system is connected to the inlet of the primary electrodialysis system;

[0064] a boron removal resin system connected to the concentrate outlet of the primary electrodialysis system;

[0065] an MVR system in communication with an outlet of the boron removal resin;

[0066] A lithium sinking unit is connected to the outlet of the MVR system.

[0067] In the present invention, the MVR system is preferably further provided with a condensate outlet, which is respectively connected to the primary electrodialysis system and the secondary electrodialysis system to provide process water replenishment for the primary electrodialysis system and the secondary electrodialysis system.

[0068] In the present invention, the lithium precipitation unit can also be replaced by a bipolar membrane system, the lithium hydroxide solution outlet of the bipolar membrane system is connected to the inlet of the MVR system, the dilute acid outlet of the bipolar membrane system is connected to the boron removal resin system, and the acid for resin regeneration is provided to the boron removal resin system, and the dilute lithium solution outlet of the bipolar membrane system is connected to the inlet of the primary electrodialysis system to realize the recovery of residual lithium.

[0069] In the present invention, the structural schematic diagram of the system for removing boron from high-boron lithium liquid and concentrating lithium is as follows Figures 1-2 As shown, Figure 1 It is a system for removing boron from high-boron lithium liquid and concentrating lithium, excluding a bipolar membrane electrodialysis system. Figure 2 The invention relates to a system for removing boron from a high-boron-containing lithium liquid and concentrating lithium, which comprises a bipolar membrane electrodialysis system.

[0070] The solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0071] Example 1

[0072] The magnesium-removing high-boron-containing lithium liquid used in this embodiment is prepared from sodium chloride, lithium chloride, potassium chloride and boron oxide, wherein the content of Li is 1.5 g / L, the content of Na is 1.25 g / L, the content of K is 1 g / L, the content of B element is 1.2 g / L, and the mass ratio of Li to Na is 1.2;

[0073] Pretreatment of high-boron lithium liquid: adding 30% hydrochloric acid to the high-boron lithium liquid, adjusting the pH value of the solution to 1, passing the acidified high-boron lithium liquid through a 50-100 μm security filter, filtering the obtained filtrate through an ultrafiltration system with a filter membrane pore size of 0.01-0.05 μm, and obtaining a purified high-boron lithium liquid;

[0074] Boron removal: The purified high-boron lithium liquid is subjected to a first-stage electrodialysis system for boron removal treatment to obtain a first-stage deboronized concentrated liquid and a first-stage boron-rich desalinated liquid. The content of Li in the first-stage deboronized concentrated liquid is 17.96 g / L, the content of Na is 14.97 g / L, and the content of K is 11.98 g / L; the content of B element is 1.28 g / L; the concentration ratio is 12.4:1, and the boron removal rate is 91.4% (the volume of the high-boron lithium liquid after magnesium removal is 12.4 times the volume of the first-stage deboronized concentrated liquid). The concentrated water side of the first-stage electrodialysis system uses a lithium chloride solution with a concentration of 0.5% as the receiving liquid, and the B content in the concentrated water receiving liquid is less than 0.1 ppm. The current density of the first-stage electrodialysis is 300 A / m 2 , the membrane voltage is 0.7V;

[0075] Recycling of lithium resources: The first-stage boron-rich desalinated liquid is passed into the second-stage electrodialysis system for secondary desalination and desalination to obtain a second-stage deboronized concentrated liquid. The second-stage deboronized concentrated liquid is diluted and mixed with the high-boron lithium liquid after intermediate purification, and then enters the first-stage electrodialysis for re-concentration and deboronization to recover lithium resources; at the same time, the second-stage electrodialysis also obtains a second-stage boron-rich desalinated liquid, in which the content of Li is 0.053g / L, the content of Na is 0.044g / L, the content of K is 0.035g / L, and the content of B is 1g / L; the second-stage boron-rich desalinated liquid enters the boron extraction process to recover fresh water resources and boron resources. The concentrated water side of the second-stage electrodialysis uses a lithium chloride solution with a concentration of 0.5% as the receiving liquid, and the B content in the concentrated water receiving liquid is less than 0.1ppm. The current density of the second-stage electrodialysis is 200A / m 2 , the membrane voltage is 0.7V;

[0076] Deep deboronization: adding 30% NaOH solution to the primary deboronized concentrated solution, adjusting the pH value of the primary deboronized concentrated solution to 9, and then using a boron removal resin to perform deep deboronization on the primary deboronized concentrated solution to obtain a lithium-rich refined solution, wherein the lithium-rich refined solution has a B content of 0.005 g / L, a Li content of 17.9 g / L, a Na content of 17.6 g / L, and a K content of 11.98 g / L; the resin is a macroporous boron removal adsorption resin;

[0077] Secondary concentration: After the pH value of the lithium-rich refined solution is adjusted to 7 with 30% hydrochloric acid, the solution to be precipitated is obtained by evaporation and concentration; the condensed water produced by evaporation is used as process water for the primary electrodialysis and secondary electrodialysis steps; the content of B in the solution to be precipitated is 0.007 g / L, the content of Li is 24.99 g / L, the content of Na is 24.56 g / L, and the content of K is 16.66 g / L;

[0078] Lithium precipitation: Add sodium carbonate solution to the lithium solution to be precipitated to convert lithium into lithium carbonate. The lithium carbonate precipitate can be filtered and dried to obtain the lithium carbonate product. The B content in the obtained lithium carbonate product meets the battery grade requirements.

[0079] Example 2

[0080] The magnesium-removed high-boron lithium liquid used in this embodiment is salt lake brine that has been purified and initially concentrated, wherein the Li content is 4.5 g / L, the Na content is 3.25 g / L, the K content is 3 g / L, the B element content is 4.2 g / L, and the mass ratio of Li to Na is 1.38.

[0081] Pretreatment of high-boron lithium liquid: adding 30% hydrochloric acid to the high-boron lithium liquid, adjusting the pH value of the solution to 1, passing the acidified high-boron lithium liquid through a 50-100 μm security filter, filtering the obtained filtrate through an ultrafiltration system with a filter membrane pore size of 0.01-0.05 μm, and obtaining a purified high-boron lithium liquid;

[0082] Deboronization: The purified high-boron lithium liquid is subjected to a first-stage electrodialysis for deboronization to obtain a first-stage deboronized concentrated liquid and a first-stage boron-rich desalinated liquid, wherein the content of Li in the first-stage deboronized concentrated liquid is 16.33 g / L, the content of Na is 11.8 g / L, the content of K is 10.89 g / L, and the content of B element is 1.66 g / L; the concentration ratio is 3.67, and the boron removal rate is 92.4% (the volume of the high-boron lithium liquid after magnesium removal is 3.67 times that of the first-stage deboronized concentrated liquid); pure water is used as a receiving liquid on the concentrated water side of the first-stage electrodialysis, and the B content in the concentrated water receiving liquid is less than 0.1 ppm; the current density of the first-stage electrodialysis is 350 A / m 2 , the membrane voltage is 0.8V;

[0083] Recycling of lithium resources: The first-stage boron-rich desalination liquid enters the second-stage electrodialysis system for secondary desalination and desalination, and the Li, Na, K, Cl, sulfate ions and other ions in the first-stage boron-rich desalination liquid are transferred to the concentrated water side to obtain a second-stage deboronized concentrated liquid. The second-stage deboronized concentrated liquid is diluted and mixed with the purified high-boron lithium liquid, and enters the first-stage electrodialysis system for re-concentration and deboronization to recover lithium resources; at the same time, the second-stage electrodialysis desalination and desalination also obtains a second-stage boron-rich desalination liquid, in which the content of Li is 0.055g / L, the content of Na is 0.040g / L, the content of K is 0.037g / L, and the content of B is 4.08g / L; the second-stage boron-rich desalination liquid enters the boron extraction process to recover fresh water resources and boron resources. Pure water is used as the receiving liquid on the concentrated water side of the secondary electrodialysis, and the B content in the concentrated water receiving liquid is less than 0.1ppm. The current density of the secondary electrodialysis is 150A / m 2 , the membrane voltage is 0.8V;

[0084] Deep deboronization: adding 9% LiOH solution to the primary deboronized concentrated solution, adjusting the pH value of the primary deboronized concentrated solution to 14, and then using a boron removal resin to perform deep deboronization on the primary deboronized concentrated solution to obtain a lithium-rich refined solution, wherein the lithium-rich refined solution has a B content of 0.003 g / L, a Li content of 16.33 g / L, a Na content of 14.225 g / L, and a K content of 10.89 g / L; the resin is a macroporous boron removal adsorption resin;

[0085] Secondary concentration: 10% hydrochloric acid is used to adjust the pH value of the lithium-rich refined solution to 8, and then the solution to be precipitated is obtained by evaporation and concentration; the condensed water produced by evaporation is used as process water for the primary electrodialysis and secondary electrodialysis steps; the content of B in the solution to be precipitated is 0.005 g / L, the content of Li is 27.98 g / L; the content of Na is 24.367 g / L, and the content of K is 18.656 g / L;

[0086] Lithium precipitation: Add sodium carbonate solution to the lithium solution to be precipitated to convert lithium into lithium carbonate. The lithium carbonate precipitate can be filtered and dried to obtain the finished lithium carbonate product; the B content in the obtained lithium carbonate product meets the battery grade requirements.

[0087] Example 3

[0088] The other conditions are the same as those in Example 1, except that the steps after obtaining the lithium-rich refined solution are replaced by the following steps:

[0089] The lithium-rich refined solution was passed into the bipolar membrane electrodialysis system. The bipolar membrane operating voltage was 1.8V per membrane pair and the current density was 600A / m 2After the lithium-rich refined liquid is electrolyzed, the chloride ions migrate to the acid chamber and combine with the hydrogen ions decomposed from the bipolar membrane positive membrane surface to form hydrochloric acid. The Li, Na, and K ions in the lithium-rich refined liquid migrate to the alkaline chamber and combine with the hydroxide ions decomposed from the bipolar membrane negative membrane surface to form LiOH, NaOH, and KOH. The alkaline solution obtained in the alkaline chamber is passed into the MVR system for evaporation and crystallization to obtain battery-grade lithium hydroxide solid. The evaporated condensate is used as the system water replenishment for the primary and secondary electrodialysis. The dilute salt solution remaining after electrolysis in the bipolar membrane electrodialysis system is mixed with the purified high-boron lithium solution and enters the primary electrodialysis system for concentration to recover lithium resources. The dilute acid solution obtained after electrolysis in the bipolar membrane electrodialysis system is used for the regeneration of macroporous boron removal adsorption resin.

[0090] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for removing boron from a high-boron lithium solution and concentrating lithium, characterized in that: The following steps are involved: (1) acidifying the high-boron lithium liquid and then ultrafiltering to obtain a purified high-boron lithium liquid; The content of Li in the high-boron lithium solution is 1.5-7 g / L, and the content of B is 1.2-5 g / L; the content of high-valent metal ions in the high-boron lithium solution is less than 1 ppm; the valence of the high-valent metal ions is +2 or above; (2) subjecting the purified high-boron lithium liquid to a first-stage electrodialysis treatment to obtain a first-stage deboronized concentrated liquid and a first-stage boron-rich desalinated liquid; the receiving liquid on the concentrated water side of the first-stage electrodialysis treatment is one or more of a lithium chloride solution, a sodium chloride solution, a potassium chloride solution and pure water; the current density of the first-stage electrodialysis treatment is 300 to 450 A / m 2 , the membrane voltage is 0.7-1.2V; the content of Li in the primary deboronation concentrated solution is 12-18g / L, the content of Na is 8-12g / L, the content of K is 5-8g / L, and the content of B is 0.1-1.8g / L; (3) subjecting the primary boron-rich desalinated liquid to a second-stage electrodialysis treatment to obtain a secondary deboronized concentrated liquid and a secondary boron-rich desalinated liquid; the secondary deboronized concentrated liquid is returned to step (2) for the first-stage electrodialysis treatment; (4) after adjusting the pH value of the primary deboronized concentrated solution to 8 to 14, deep deboronization is performed using a boron removal resin to obtain a lithium-rich refined solution; (5) adjusting the pH value of the lithium-rich refined solution to 6 to 8 and then evaporating and concentrating the solution to obtain a lithium precipitation solution; The lithium solution to be precipitated is mixed with a sodium carbonate solution to precipitate lithium, thereby obtaining lithium carbonate; There is no time limit for the steps (3) and (4).

2. The method according to claim 1, characterized in that The high-boron lithium liquid has a Na content of 1.25-10 g / L, a K content of 1-3 g / L, and a mass ratio of Li to Na greater than 0.

8.

3. The method according to claim 1, characterized in that The acidification is based on adjusting the pH value of the high-boron lithium liquid to 1-6.5; the pore size of the ultrafiltration filter membrane is 0.01-0.05 μm; before the ultrafiltration, the acidified high-boron lithium liquid is filtered; the pore size of the filtration filter membrane is 50-100 μm.

4. The method according to claim 1, characterized in that: The current density of the second stage electrodialysis treatment is 100-400A / m 2 , the membrane voltage is 0.7~1.2V; The content of Li in the secondary boron-rich desalinated liquid is 0.02-0.1 g / L, the content of Na is 0.01-0.2 g / L, the content of K is 0.01-0.3 g / L, and the content of B is 1.3 g-5.2 g / L; the secondary boron-rich desalinated liquid is subjected to boron extraction treatment.

5. The method according to claim 1, characterized in that The boron removal resin is a macroporous boron removal adsorption resin; the content of B in the lithium-rich refined liquid is less than 0.01 g / L.

6. The method according to claim 1, characterized in that The step (5) is replaced by: The lithium-rich refined liquid is subjected to bipolar membrane electrodialysis treatment to obtain a lithium hydroxide solution and a dilute lithium solution; the dilute lithium solution and the purified high-boron lithium solution are mixed and returned to the first-stage electrodialysis treatment step; The lithium hydroxide solution is evaporated and crystallized to obtain lithium hydroxide.

7. The method according to claim 6, characterized in that The condensed water produced by the evaporative crystallization is used as system water for the first-stage electrodialysis treatment and the second-stage electrodialysis treatment.

8. A system used in the method for removing boron and concentrating lithium from a high-boron lithium solution according to any one of claims 1 to 7, characterized in that: include: Security filters; an ultrafiltration system connected to the outlet of the security filter; a primary electrodialysis system connected to the filtrate outlet of the ultrafiltration system; a secondary electrodialysis system in communication with the fresh water outlet of the primary electrodialysis system; The concentrated water outlet of the secondary electrodialysis system is connected to the inlet of the primary electrodialysis system; a boron removal resin system connected to the concentrate outlet of the primary electrodialysis system; an MVR system in communication with an outlet of the boron removal resin; A lithium sinking unit is connected to the outlet of the MVR system.

9. The system according to claim 8, characterized in that The lithium precipitation unit is replaced with a bipolar membrane system, the lithium hydroxide solution outlet of the bipolar membrane system is connected to the inlet of the MVR system, the dilute acid outlet of the bipolar membrane system is connected to the boron removal resin system, and the dilute lithium solution outlet of the bipolar membrane system is connected to the inlet of the primary electrodialysis system.