3D-printed concrete structure with stretchable ropes
By using high carbon content slender steel wire ropes as reinforcements in concrete 3D printing, the problems of structural brittleness and insufficient adhesion are solved, higher ductility and impact resistance are achieved, suitable for load-bearing structures, and the reinforcement process is simplified .
Patent Information
- Application Number
- CN202180018768.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-04
- Filing Date
- 2021-02-16
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-02-16
AI Technical Summary
In the existing concrete 3D printing technology, the brittleness of the structure and insufficient adhesion of the reinforcements result in poor ductility and impact resistance, making it difficult to be used for load-bearing structures. Moreover, traditional reinforcement methods are labor-intensive, error-prone, and conflict with the purpose of automated printing.
Slender high-carbon content steel wire ropes are used as reinforcements, and the tensile strength is increased through quenching and cold working, and the elastic and plastic elongation at break is greater than 4% to enhance the ductility and impact resistance of the structure, and during printing It is transported simultaneously with the cementitious material during the process.
The ductility and impact resistance of concrete 3D printed structures are significantly improved, making them suitable for load-bearing structures. At the same time, the reinforcement process is simplified, manual work is reduced, and printing efficiency is improved.
Smart Images

Figure CN115210070B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a concrete building manufactured by concrete 3D printing. Background Art
[0002] The so-called "concrete 3D printing" in this article refers to the additive manufacturing of concrete or cementitious materials, which has developed rapidly in the past few years. According to the concrete 3D printing technology, a pump supplies cementitious mortar to the printing nozzle through a hose, and the printing nozzle extrude the cementitious mortar in a stacked manner. The gantry robot guides and moves the entirety, that is, the hose and the printing nozzle.
[0003] Generally speaking, cementitious matrix structures, especially concrete structures, are brittle and have poor resistance to tensile or bending stresses. Adding fasteners to these structures can increase their ductility.
[0004] Brittleness is also a problem for structures made using 3D printing of concrete.
[0005] Traditional reinforcements, such as rebar, can be inserted into the printed concrete layer while the concrete is still not solidified. However, this approach has serious disadvantages. It is labor-intensive, prone to errors, and the adhesion between the rebar and the concrete is insufficient. In addition, this method is contrary to the ultimate goal of concrete 3D printing, which is to minimize manual work.
[0006] It is possible to add reinforcing fibers to cementitious mortar. However, experience has shown that it is difficult to deliver a mixture of cementitious mortar and concrete through a hose and a printing nozzle.
[0007] Another solution to the reinforcement problem is to install a reinforcement grid or mesh in advance and extrude the cementitious mortar around it. Here, as before, the installation of the reinforcement in advance requires manual work, which one would like to avoid. In addition, the presence of the reinforcement makes the extrusion process and the operation of the print head more complicated.
[0008] The Technical University of Eindhoven, in cooperation with Bekaert, has come up with an excellent solution that allows the simultaneous laying of concrete and reinforcements. A reinforcement delivery device is added to the print head, which has a reel with a flexible steel wire. The reinforcement delivery device moves with the gantry robot, pays out the flexible steel wire from the reel and introduces it into the laid concrete layer. In this way, the simultaneous laying of concrete and reinforcements is achieved.
[0009] Although the steel cables used have many advantages, such as light weight, high tensile strength and good flexibility, their reinforcement effect is not enough to provide the required ductility and impact resistance. Therefore, 3D printed concrete structures are not often used in load-bearing situations. Summary of the invention
[0010] A general object of the present invention is to overcome the disadvantages of the prior art.
[0011] A specific object of the present invention is to provide a reinforcement with better ductility for concrete 3D printed buildings.
[0012] Another object of the present invention is to provide a more impact-resistant concrete 3D printed building.
[0013] According to the present invention, there is provided a concrete building manufactured by concrete 3D printing. The building comprises two or more layers of cementitious material extruded in a stacked manner. The building further comprises at least one elongated steel element, which reinforces at least one layer of cementitious material in the two or more layers of cementitious material, and preferably reinforces all layers of cementitious material in the two or more layers of cementitious material.
[0014] The elongated steel element has a carbon content in the range of 0.60% to 1.20%.The elongated steel element is quenched and subsequently cold worked (eg rolled and wire drawn) until its tensile strength exceeds 2500 MPa, such as exceeds 2750 MPa.
[0015] The elongated steel element may be a steel wire or a steel rope.
[0016] In the case of a steel wire rope, the steel wire rope has steel wires or a steel strand consisting of steel wires.
[0017] In the case of a single steel wire, the wire diameter D is 0.20 mm to 2.0 mm, for example, 0.35 mm to 1.50 mm.
[0018] In the case of a steel wire rope, the wire diameter d of the steel wire is 0.03 mm to 0.65 mm, for example, 0.10 mm to 0.40 mm.
[0019] In case of a multi-strand steel wire rope, the diameter d' of the steel strand may be 0.25 mm to 0.75 mm, for example 0.30 mm to 0.75 mm.
[0020] The elastic and plastic elongation at break of the elongated steel element is greater than 4%, preferably greater than 4.5%, for example greater than 5% or 6% or more. As described below, this elongation value does not include the so-called structural elongation of the elongated steel element.
[0021] The term "cementitious material" refers to concrete, mortar, cement, etc.
[0022] The elastic elongation and plastic elongation of common steel wire ropes composed of quenched drawn steel wires with a high carbon content at break are up to 2%. The elastic elongation and plastic elongation of the steel wire rope to be used in the present invention at break exceed twice the above maximum values.
[0023] Due to its twisted nature, the steel wire rope has a wavy radial outer surface. These protrusions form possible anchorage points in the cementitious matrix when the structure is subjected to tensile or bending loads. The section of the steel wire rope between two anchorage points bridges the cracks that appear. The higher the elongation of this section of the steel wire rope, the better the ductility of the concrete structure. Therefore, the elongation of the steel wire rope to be used in the present invention is much higher, resulting in a much higher ductility of the 3D printed structure. Such a reinforced structure should have a higher impact resistance and may have more chances of being used as a load-bearing structure.
[0024] The elongated steel elements used in the present invention are preferably in a stress relieved state.
[0025] Generally speaking, all kinds of steel wires or cables are suitable as long as they are flexible enough to be able to move with and through the print head. The cable may be a single-strand cable or a multi-strand cable.
[0026] The elongated steel element may be provided with an anti-corrosion coating. The anti-corrosion coating may be a metallic coating, such as a zinc coating, a zinc alloy coating or a brass coating. The anti-corrosion coating may also be a polymer coating.
[0027] In case of a zinc coating or a zinc alloy coating, or in the absence of any coating, it is preferred to apply benzimidazole to the elongated steel element, for example by spraying or dipping.
[0028] According to another aspect of the present invention, there is also provided a method for manufacturing the above concrete building by 3D printing, wherein the elongated steel element and the cementitious material are simultaneously supplied through the same printing head or printing nozzle. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A schematic diagram of a method for manufacturing a building by concrete 3D printing.
[0030] Figure 2 The load-elongation curves of two types of wire ropes are shown. DETAILED DESCRIPTION
[0031] Figure 1It is shown how a building 100 is made by concrete 3D printing. The building 100 has a first layer 102 reinforced by steel cables 104. The building 100 also has a second layer 106 reinforced by steel cables 108, wherein the steel cables 106 may be the same steel cables as the steel cables 104 of the first layer. The second layer 106 is being extruded onto the first layer 102. This extrusion is achieved by a print head or print nozzle 110 that supplies cementitious mortar 112 and steel cables 108. The print head 110 moves in the direction indicated by arrow 114.
[0032] When the print head 110 supplies the cementitious mortar 112 and the steel wire 108, the steel wire and the concrete layer 106 follow the same path. Since the path may be curved and may have multiple turns, the steel wire 108 must be sufficiently flexible. This means that the wire diameter d of the steel wire is 0.03 mm to 0.65 mm, for example 0.10 mm to 0.40 mm. When using a multi-strand steel wire rope, the diameter d' of the steel strand can be 0.25 mm to 0.75 mm, for example 0.30 mm to 0.75 mm.
[0033] Figure 2 The load-elongation curve 20 of a conventional steel wire rope and the load-elongation curve 22 of a steel wire rope to be used in the present invention are shown. The abscissa is the elongation A expressed in percent and the ordinate is the tensile strength R in megapascals. The load-elongation curve is obtained in a tensile test according to standards ISO 6892 and DIN 51210.
[0034] At low loads, the load-elongation curves 20 and 22 may or may not have an initial large elongation. This elongation is called the structural elongation A. s , is a result of the twisted nature of the rope. By applying a small load, the wires or strands in the rope move slightly and come into closer contact with each other until the rope begins to behave as a single unit. This structure elongates s Depending on the type of wire rope structure, it can be small, large, or even absent.
[0035] The next elongation stage is the elastic elongation according to Hooke's law. The wire rope behaves as a whole and at the elastic elongation A e The range expands linearly according to the applied load.
[0036] The final elongation stage is plastic elongation. e After that, the wire begins to flow plastically until the wire rope finally breaks.
[0037] Plastic elongation A pThe size of A is the basic difference between ordinary steel wire ropes and the steel wire ropes to be used in the present invention. For the steel wire ropes to be used in the present invention, the value of plastic elongation is much larger. e and A p The sum is greater than 4%, such as greater than 4.5%, such as greater than 5%, greater than 6%.
[0038] The steel wire rope to be used in the present invention can be manufactured by the following method.
[0039] Original steel composition
[0040] The raw material is wire rod with the following steel composition:
[0041] The composition of ordinary carbon steel is as follows (all percentages are by weight):
[0042] A carbon content (%C) of 0.60% to 1.20%, such as 0.80% to 1.1%;
[0043] Manganese content (%Mn) is 0.10% to 1.0%, for example 0.20% to 0.80%;
[0044] Silicon content (%Si) is 0.10% to 1.50%, for example 0.15% to 0.70%;
[0045] The sulfur content (%S) is less than 0.03%, for example less than 0.01%;
[0046] The phosphorus content (%P) is less than 0.03%, for example less than 0.01%.
[0047] Alternatively, the following elements may be added to the composition:
[0048] Chromium (%Cr): content of 0.10% to 1.0%, for example, 0.10 to 0.50%;
[0049] Nickel (%Ni): content of 0.05% to 2.0%, for example, 0.10% to 0.60%;
[0050] Cobalt (%Co): content of 0.05% to 3.0%; for example, 0.10% to 0.60%;
[0051] Vanadium (%V): a content of 0.05% to 1.0%, for example 0.05% to 0.30%;
[0052] Molybdenum (%Mo): content of 0.05% to 0.60%, for example, 0.10% to 0.30%;
[0053] Copper (%Cu): content of 0.10% to 0.40%, for example, 0.15% to 0.30%;
[0054] Boron (%B): content of 0.001% to 0.010%, for example, 0.002% to 0.006%;
[0055] Niobium (%Nb): a content of 0.001% to 0.50%, for example, 0.02% to 0.05%;
[0056] Titanium (%Ti): a content of 0.001% to 0.50%, for example, 0.001% to 0.010%;
[0057] Antimony (%Sb): a content of 0.0005% to 0.08%, for example, 0.0005% to 0.05%;
[0058] Calcium (%Ca): a content of 0.001% to 0.05%, for example, 0.0001% to 0.01%;
[0059] Tungsten (%W): for example, a content of about 0.20%;
[0060] Zirconium (% Zr): for example, a content of 0.01% to 0.10%;
[0061] Aluminum (%Al): the content is preferably less than 0.035%, such as less than 0.015%, such as less than 0.005%;
[0062] Nitrogen (%N): content less than 0.005%;
[0063] Rare earth metals (%REM): content is 0.010% to 0.050%.
[0064] After some previous drawing operations and a final quenching treatment, it is best to provide the wire rope with a metal coating to improve its corrosion resistance.
[0065] Types of Metal Coatings
[0066] The metal coating is preferably a zinc coating or a zinc alloy coating.
[0067] The zinc alloy coating may be a zinc aluminum alloy coating having an aluminum content of 2 to 12% by weight, such as 3 to 11% by weight.
[0068] The preferred composition is near the eutectoid position: the aluminum content is about 5%. The zinc alloy coating may also have wetting agents such as lanthanum and cerium, which are less than 0.1% of the zinc alloy. The rest of the coating is zinc and unavoidable impurities. Another preferred composition includes about 10% aluminum. The increase in aluminum content provides better corrosion resistance compared to the eutectoid composition with an aluminum content of about 5%.
[0069] Other elements such as silicon (Si) and magnesium (Mg) may be added to the zinc-aluminum alloy. For optimum corrosion resistance, a particularly good alloy includes 2% to 10% aluminum and 0.2% to 3.0% magnesium, with the remainder being zinc.
[0070] For example, 5% aluminum, 0.5% magnesium, and the rest zinc.
[0071] The zinc coating or zinc alloy coating is preferably applied to the steel wire by a hot-dip operation. The average thickness of the metal coating is preferably limited to 4 micrometers, for example to 3 micrometers.
[0072] The coated steel wire is then subjected to a final diameter reduction treatment, for example by wet drawing, until a final wire diameter is obtained. The final wire diameter is 0.10 mm to 0.80 mm, for example 0.15 mm to 0.60 mm, for example 0.20 mm to 0.40 mm.
[0073] Then, the steel wires are twisted into a wire rope.
[0074] For example, a wire rope thus twisted may be stress relieved by passing it through a high-frequency or medium-frequency induction coil, the length of which is matched to the speed of movement of the wire rope; it has in fact been observed that at a specific temperature of about 300 degrees Celsius, after a period of heat treatment, the tensile strength decreases by about 10%, without any increase in the plastic elongation at break; however, by raising the temperature slightly to above 400 degrees Celsius, a further decrease in the tensile strength is observed, while the plastic elongation at break increases; in this way, the plastic elongation can be increased to more than 6%, while the tensile strength decreases by 10% to 15%.
[0075] In order to prevent the concrete reinforced by the zinc-coated metal elements from evolving hydrogen during hardening, the steel wire ropes may be treated with benzimidazole (eg by spraying benzimidazole on the steel wire rope or dipping the steel wire rope in benzimidazole).
[0076] List of reference numerals:
[0077] 100 Buildings made with concrete 3D printing
[0078] 102 First Floor
[0079] 104 Wire Rope
[0080] 106 Second Floor
[0081] 108 Wire Rope
[0082] 110 Print head or print nozzle
[0083] 112 Cementitious mortar
[0084] 114 Moving direction
Claims
1. A concrete building manufactured by concrete 3D printing, the concrete building comprising: - two or more layers of cementitious material extruded in a layered manner, - at least one elongated steel element reinforcing at least one of said two or more layers of cementitious material, The carbon content of the elongated steel element is in the range of 0.60% to 1.20%, The elongated steel element is cold worked and has a tensile strength in excess of 2500 MPa, It is characterized in that The elongated steel element has an elastic elongation and a plastic elongation at break greater than 4%.
2. The concrete building according to claim 1, wherein: The elongated steel element is in a stress-relieved state.
3. The concrete building according to claim 1 or 2, wherein: The elongated steel element is a steel wire.
4. The concrete building according to claim 1 or 2, wherein: The elongated steel element is a steel wire rope.
5. The concrete building according to claim 4, wherein: The steel wire rope includes two or more strands of steel wires.
6. The concrete building according to claim 4, wherein: The steel wire rope is a single-strand steel wire rope.
7. The concrete building according to claim 1, wherein: The elongated steel element is provided with an anti-corrosion coating.
8. The concrete building according to claim 7, wherein: The anti-corrosion coating is a zinc alloy coating.
9. The concrete building according to claim 1, wherein: The elongated steel element contains benzimidazole.
10. A method for manufacturing the concrete building according to claim 1 by 3D printing, wherein: The elongated steel element is fed simultaneously with the gelling material through the same print head or print nozzle.
Citation Information
Patent Citations
High corrosion resistant electric arc spraying pure zinc coating hole sealing agent, preparation technology and application thereof
CN104498856A
Zinc-coated steel cord with improved fatigue resistance
CN1427911A
Method for strengthening or repairing an existing reinforced concrete structural element
US20040154263A1
Steel fiber for reinforcement of high-performance concrete
US6235108B1
An apparatus and a method for constructing a construction element or a building
WO2015197910A1