Low voltage resistors, circuit substrates, semiconductor component packaging and interposers
By using a resin composition of carbon nanotubes and carbon aerogels, combined with epoxy resin and acrylic resin, the demand for high-performance varistors under low voltage is solved, achieving high nonlinear coefficient and low electrostatic capacitance effects, and is suitable for high-voltage applications. frequency application.
Patent Information
- Application Number
- CN202180010589.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-01
AI Technical Summary
Existing technology is difficult to provide high-performance varistors at low voltages, and lacks solutions with excellent overvoltage protection characteristics and low electrostatic capacitance. Especially in high-frequency areas, the electrostatic capacitance of varistors used is relatively high.
A resin composition containing carbon nanotubes and carbon aerogel is used as the cured body of the low-voltage varistor, combined with epoxy resin and acrylic resin, and through a specific manufacturing method and curing agent ratio, the nonlinear coefficient and electrostatic capacitance characteristics are optimized.
It achieves excellent performance of the rheostat operating at low voltage, has high nonlinear coefficient and low electrostatic capacitance, is suitable for high frequency areas, and provides better overvoltage protection characteristics and high frequency impedance.
Smart Images

Figure CN115210827B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a varistor including a cured product of a resin composition for forming a low-voltage varistor. Background Art
[0002] Patent Documents 1 to 4 describe technologies related to varistors.
[0003] Patent Document 1 describes a multilayer ceramic varistor. 3 In the sintered body, the ceramic layers as the main component and the internal electrodes are alternately stacked in multiple layers, wherein the ceramic layers are formed of ceramics having a pore volume occupancy of 1.35 to 4.85%. In addition, Patent Document 1 describes that the capacitance C of the examples is 5.5 to 32.0 nF.
[0004] Patent document 2 describes a voltage switchable dielectric (VSD) material composition. Patent document 2 describes that the VSD material composition includes: a binder, and high aspect ratio (HAR) particles including conductive particles and / or semiconductor particles. Figure 3 C describes that the resistance of the resistor changes within the range of 500 to 100 V.
[0005] Patent document 3 describes a paste for forming a varistor element, which contains a resin composition, wherein the resin composition is a resin composition containing (A) epoxy resin, (B) curing agent and (C) carbon nanotubes, and the semiconductor type single-layer carbon nanotubes in the carbon nanotubes account for more than 70 weight%.
[0006] Patent Document 4 describes a varistor-forming resin composition containing (A) an epoxy resin, (B) a curing agent, (C) carbon nanotubes, and (D) a dispersant.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2001-93706
[0010] Patent Document 2: U.S. Patent No. 7,695,644
[0011] Patent Document 3: U.S. Patent No. 10141090
[0012] Patent Document 4: International Publication No. 2019 / 116955 Summary of the invention
[0013] A varistor is an element (electronic component or electrical component) that has a property of high resistance when the voltage between a pair of electrodes is low, and a property of rapidly decreasing resistance when the voltage between the pair of electrodes exceeds a given value. Generally speaking, a varistor has a structure in which a material having nonlinear resistance characteristics is arranged between a pair of electrodes. Examples of materials having nonlinear resistance characteristics include silicon carbide, zinc oxide, and strontium titanate.
[0014] In order to improve the performance and reduce the cost of varistors, it is necessary to find new materials for varistors and continue to develop them.
[0015] In semiconductor devices and the like, there is a use for low-voltage varistors that can operate at a low voltage (for example, 10 V or less, preferably 8 V or less, and more preferably 7 V or less).
[0016] Furthermore, the varistor is required to have excellent overvoltage protection characteristics. That is, as a varistor with excellent performance, it is required that the resistance decreases more sharply with the increase of the applied voltage (the nonlinear coefficient α described later is high).
[0017] Furthermore, a varistor used in a high frequency region is required to have a low electrostatic capacitance.
[0018] An object of the present invention is to provide a varistor having excellent performance and capable of operating at a low voltage.
[0019] In order to solve the above-mentioned problems, the present invention has the following configuration.
[0020] (Structure 1)
[0021] Structure 1 of the present invention is a low-voltage resistor, comprising a cured body of a resin composition for forming a low-voltage resistor, characterized in that the resin composition for forming a low-voltage resistor comprises (A) at least one selected from carbon nanotubes and carbon aerogels; and (B) at least one selected from epoxy resins and acrylic resins.
[0022] (Structure 2)
[0023] Structure 2 of the present invention is based on the low-voltage varistor of structure 1, and the varistor voltage is 0.3-10V when the inflow current of the low-voltage varistor is 0.1mA.
[0024] (Structure 3)
[0025] Structure 3 of the present invention is based on the low-voltage resistor of structure 1 or 2, and the current-voltage characteristic of the low-voltage resistor is changed to I=KV α When characterized (where V is the applied voltage, I is the inflow current, K is a constant, and α is the nonlinear coefficient), the nonlinear coefficient α is 7 to 20.
[0026] (Structure 4)
[0027] Structure 4 of the present invention is based on any low-voltage varistor of structures 1 to 3, and the static capacitance is 0.5 to 200 pF.
[0028] (Structure 5)
[0029] Structure 5 of the present invention is a circuit substrate on which any low-voltage varistor of Structures 1 to 4 is mounted.
[0030] (Structure 6)
[0031] Structure 6 of the present invention is a semiconductor component package equipped with any low-voltage varistor of Structures 1 to 4.
[0032] (Structure 7)
[0033] The structure 7 of the present invention is an interposer equipped with any low-voltage resistor of the structures 1 to 4.
[0034] According to the present invention, a varistor having excellent performance and capable of operating at a low voltage can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 1 is a schematic top view of electrodes used in a varistor according to an embodiment of the present invention.
[0036] Figure 2 4 is a schematic top view of a varistor according to an embodiment of the present invention.
[0037] Figure 3 3 is a graph showing the current-voltage characteristics of the varistor of Example 1.
[0038] Figure 4 This is a graph showing the current-voltage characteristics of the varistor of Example 2.
[0039] Figure 5 3 is a graph showing the current-voltage characteristics of the varistor of Comparative Example 1.
[0040] Figure 6 3 is a graph showing the current-voltage characteristics of the varistor of Comparative Example 2.
[0041] Figure 7 This is a SEM photograph of the porous carbon of Reference Example 1 of the present invention (magnification: 10,000 times).
[0042] Figure 8 This is a SEM photograph of the porous carbon of Reference Example 1 of the present invention (magnification: 100,000 times).
[0043] Fig. 9 This is a SEM photograph of the porous carbon of Reference Example 2 (magnification: 10,000 times).
[0044] Fig.10This is a SEM photograph of the porous carbon of Reference Example 2 (magnification: 100,000 times).
[0045] Fig.11 This is a SEM photograph of the porous carbon of Reference Comparative Example 2 (magnification: 10,000 times).
[0046] Fig.12 This is a SEM photograph of the porous carbon of Reference Comparative Example 2 (magnification: 100,000 times).
[0047] Fig.13 This is the Raman spectrum of the porous carbon of Reference Example 1.
[0048] Fig.14 This is the Raman spectrum of the porous carbon of Reference Example 2.
[0049] Fig.15 This is the Raman spectrum of the porous carbon of Reference Comparative Example 2. DETAILED DESCRIPTION
[0050] The following embodiments of the present invention are specifically described with reference to the drawings. Note that the following embodiments are forms for embodying the present invention, and the present invention is not limited to the scope thereof.
[0051] <Low Voltage Varistor>
[0052] First, the low voltage varistor of the present invention is described. The low voltage varistor of the present embodiment includes a cured product of a resin composition for forming a low voltage varistor. The resin composition for forming a low voltage varistor will be described later.
[0053] exist Figure 2 A schematic diagram showing an example of a varistor. Figure 2 The varistor shown has Figure 1 As shown in FIG. 1 , a cured body 16 of a material having varistor characteristics (a resin composition for forming a low-voltage varistor) is arranged on a pair of electrodes 14a and 14b. Figure 2 The structure of the varistor shown is a simple example, and any structure can be used as long as a material having varistor characteristics is arranged between a pair of electrodes. For example, a structure in which a material having varistor characteristics is arranged between electrodes arranged in parallel, a structure in which a pair of electrodes are arranged three-dimensionally in a comb shape, etc. can be used.
[0054] A varistor is an electronic component (or electrical component) having nonlinear resistance characteristics. The relationship between the voltage V (applied voltage) applied between a pair of electrodes 14a and 14b of a varistor and the current I (inflow current) flowing between the two terminals at this time (current-voltage characteristics) can be expressed as I=K·V, with K being a constant. αThe approximation of the approximation is called the nonlinear coefficient. In the case of a normal ohmic resistor, α=1, but in the case of a varistor, α>1. When the nonlinear coefficient α of the varistor is greater than 7, specifically when α is 7 to 20, it can be said that it has an overvoltage protection characteristic with excellent performance.
[0055] By using the resin composition for forming a low-voltage varistor of this embodiment, a varistor having excellent overvoltage protection characteristics, that is, a varistor having a nonlinear coefficient α of 7 or more, specifically α of 7 to 20, can be manufactured.
[0056] The low-voltage varistor of the present embodiment preferably has a varistor voltage of 0.3 to 10V when the current flowing into the low-voltage varistor is 0.1mA, more preferably 0.3 to 8V, and further preferably 0.3 to 7V. The low-voltage varistor of the present embodiment is particularly preferably used in the case where the varistor voltage is about 6V when the current flowing into the low-voltage varistor is 0.1mA. The low-voltage varistor of the present embodiment can operate at a relatively low voltage compared to the existing varistor. Therefore, it can be said that the varistor of the present embodiment has excellent characteristics as a low-voltage varistor.
[0057] The low-voltage varistor of the present embodiment preferably has an electrostatic capacitance of 0.5 to 200 pF, preferably 0.5 to 180 pF, and preferably 0.5 to 160 pF. The electrostatic capacitance in this case can be measured using an oscillator frequency of 1 kHz. Compared with the existing varistor, the low-voltage varistor of the present embodiment has a low impedance at high frequencies due to its relatively low electrostatic capacitance. For this reason, the varistor of the present embodiment can be said to have excellent characteristics as a low-voltage varistor in the high-frequency region.
[0058] This embodiment is a circuit substrate equipped with the above-mentioned low-voltage varistor. The varistor of this embodiment can be preferably used as a low-voltage varistor in a high-frequency region. Therefore, by mounting the varistor of this embodiment on a given circuit substrate, a desired electronic circuit can be obtained.
[0059] The present embodiment is a semiconductor component package equipped with the above-mentioned low-voltage varistor. The varistor of the present embodiment can be preferably used as a low-voltage varistor in a high-frequency region. For this reason, a semiconductor component package capable of performing a desired operation can be obtained by mounting the varistor of the present embodiment on a given semiconductor component package.
[0060] This embodiment is an interposer equipped with the above-mentioned low-voltage varistor. The interposer is a substrate having through electrodes for achieving conduction of the circuit on the surface and back of the substrate for the purpose of high integration of the circuit. The varistor of this embodiment can preferably be used as a low-voltage varistor in a high-frequency region. For this reason, by mounting the varistor of this embodiment on a given interposer, a highly integrated electronic circuit capable of performing the desired operation can be obtained.
[0061] <Resin composition for forming low voltage varistor>
[0062] Next, the low-voltage varistor forming resin composition used to form the cured body of the low-voltage varistor of the present embodiment is specifically described. In addition, in this specification, the low-voltage varistor forming resin composition is simply referred to as "resin composition" (or sometimes referred to as "resin composition of the present embodiment")).
[0063] <(A)Component>
[0064] The low voltage varistor forming resin composition of the present embodiment includes, as the component (A), at least one selected from (A1) carbon nanotubes and (A2) carbon aerogel.
[0065] The carbon nanotubes (A1) contained in the resin composition for forming a low voltage varistor are described.
[0066] Carbon nanotubes are substances in which a six-membered ring network made of carbon is formed into a coaxial tube. Single-layer and multi-layer carbon nanotubes are known. Carbon nanotubes can be classified into metallic carbon nanotubes and semiconductor carbon nanotubes according to their electrical properties. The (A1) carbon nanotubes contained in the resin composition for forming a low-voltage varistor of this embodiment are single-layer carbon nanotubes.
[0067] The (A1) carbon nanotube is preferably a single-walled carbon nanotube. Specifically, single-walled carbon nanotubes (TUBALL SWCNT 93%) manufactured by OCSIAL can be used as the (A1) carbon nanotube. TUBALL SWCNT 93% is a single-walled carbon nanotube having an outer diameter of 1.6 nm ± 0.4 nm, a length of 5 μm or more, and a carbon nanotube content of 93% or more.
[0068] The content of (A1) carbon nanotubes in the resin composition for forming a low-voltage varistor is preferably 0.01 to 2 parts by weight, more preferably 0.015 to 1 part by weight, further preferably 0.02 to 0.1 part by weight, and particularly preferably 0.03 part by weight or more and less than 0.05 part by weight, relative to 100 parts by weight of the epoxy resin (B).
[0069] The carbon aerogel (A2) contained in the resin composition for forming a low voltage varistor will be described.
[0070] Carbon aerogel is a porous carbon composed of covalent bonds of nano-sized molecules and having a high porosity. Hereinafter, carbon aerogel is also referred to as porous carbon.
[0071] In this specification, the so-called carbon aerogel (porous carbon) is preferably a porous carbon obtained by replacing the solvent contained in a gel-like mixture containing a carbonaceous material as a raw material with a gas by supercritical drying and removing components other than carbon by thermal decomposition.
[0072] Carbon aerogel (porous carbon) has a large number of pores due to the manufacturing method. The size of the pores is less than 1 μm, and is a pore of nanometer size (nanopore). Generally speaking, the size of the nanopores of porous carbon is 200 to 300 nm. The size of the pores can be obtained by using a SEM photograph obtained by taking a cross-section of the porous carbon with a scanning electron microscope (SEM) as the average of the diameters of multiple pores in the SEM photograph. The diameters of all pores in the SEM photograph can be measured to find the average. In addition, for example, by measuring the diameters of 10 to 20 pores to find the average, it can be set as the size of the pores.
[0073] Such porous carbon can be preferably used as a material for producing a varistor. Specifically, as the (A2) carbon aerogel, carbon aerogel powder (model: PC16-151-10) manufactured by eM-TECH can be used.
[0074] Carbon aerogel powder PC16-151-10 can be manufactured by manufacturing method 1 described below. The specific manufacturing conditions of carbon aerogel powder PC16-151-10 are shown below. Furfural and phloroglucinol (molar ratio of furfural: phloroglucinol 3:1) are dissolved in ethanol. The amount of ethanol during the dissolution is adjusted so that the concentration of the total amount of furfural and phloroglucinol in the ethanol solution becomes 4 weight%. A gelled solid can be obtained by stirring the ethanol solution of furfural and phloroglucinol and then leaving it at room temperature. The gelled solid is replaced with air by supercritical carbon dioxide liquid to produce an aerogel as a precursor. Carbon aerogel PC16-151-10 is produced by calcining the aerogel at 1000°C under a nitrogen flow.
[0075] The content of the (A2) carbon aerogel in the resin composition for forming a low voltage varistor is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, further preferably 1 to 4.5 parts by weight, and particularly preferably 2 to 4 parts by weight, relative to 100 parts by weight of the (B) epoxy resin.
[0076] Next, porous carbon (carbon aerogel) that can be used in the present embodiment will be described in detail.
[0077] In the Raman spectrum of the porous carbon that can be used in the present embodiment measured by Raman spectroscopy, at 1590 cm -1 The integrated intensity of the peak of the G band near 1350 cm -1 When the integrated intensity of the peak of the D band near the substrate is ID, ID / IG is equal to or greater than 2.0. By using such porous carbon, a resin composition and a varistor forming paste for manufacturing a varistor having suitable varistor characteristics can be obtained.
[0078] In measuring the wavenumber (usually in cm) of Raman scattering (Raman shift) in Raman spectroscopy -1 ) corresponding to the intensity of Raman scattering, the porous carbon that can be used in this embodiment has a given Raman spectrum. Generally speaking, a substance composed of carbon has a Raman spectrum at 1590 cm due to the bonding state of carbon. -1 Nearby and 1350cm -1 There is a peak near 1590cm -1 The peak near the graphite is considered to be due to the sp 2 The peak of the G band of the hybrid orbital. 1350cm -1 The peak near the diamond is considered to be due to the sp 3 The peak of the D band of the hybrid orbital. The D band is believed to be based on diamond-like amorphous carbon, so the strong intensity of the D band is believed to be caused by the disorder of the bonding state of graphite. -1 The cumulative intensity of the peak value of the G band nearby is set to I G 、1350cm -1 The accumulated intensity of the peak value of the nearby D band is set to I D The porous carbon that can be used in this embodiment is characterized in that: D / I G is 2.0 or more. D / I G It is preferably 2.1 to 3.0, and more preferably 2.2 to 2.5.
[0079] The cumulative intensity of the peak of the G band refers to the area of the peak after subtracting the background as noise from the peak of the G band in the Raman spectrum that plots the intensity of Raman scattering corresponding to the wave number of Raman scattering. The same is true for the cumulative intensity of the peak of the D band. In addition, since the peak of the G band is close to the peak of the D band, the peak of the G band and the peak of the D band can be separated by performing peak fitting using an appropriate function such as a Lorentz function. Such a peak separation technique is well known.
[0080] The maximum intensity of the peak value of the G band is set to M G , set the maximum intensity of the peak value of the D band to M D The porous carbon that can be used in this embodiment is preferably M D / M G It is above 0.80.
[0081] In the Raman spectrum in which the intensity of Raman scattering corresponding to the wave number of Raman scattering is plotted, the maximum intensity of the peak of the G band is defined as M. G , set the maximum intensity of the peak value of the D band to M D The porous carbon that can be used in this embodiment is preferably M D / M G The maximum intensity M of the peak of the G band is 0.80 or more. G The maximum value of the peak intensity of Raman scattering in the G band after subtracting the background as noise from the measured value of the wave number range constituting the peak of the G band. D In addition, since the peak of the G band is close to the peak of the D band, the peak of the G band and the peak of the D band can be separated by peak fitting using an appropriate function such as the Lorentz function, and the maximum intensity M can be calculated. G In addition, M D / M G It is more preferably 0.80 to 3.0, and even more preferably 0.90 to 1.5. By using such porous carbon, a resin composition and a varistor forming paste for producing a varistor having suitable varistor characteristics can be obtained more reliably.
[0082] Next, a method for producing porous carbon (carbon aerogel) according to an embodiment of the present invention will be described.
[0083] [Manufacturing method 1]
[0084] In the method 1 for producing porous carbon that can be used in the present embodiment, porous carbon can be produced by thermal decomposition of a mixture of raw materials containing furfural and phloroglucinol.
[0085] (Process of preparing materials)
[0086] The method 1 for producing porous carbon that can be used in the present embodiment includes a process for preparing materials. In the process for preparing materials, first, a given amount of furfural and phloroglucinol is prepared. In the porous carbon that can be used in the present embodiment, in the raw material, furfural is preferably 100 to 500 parts by weight, more preferably 120 to 340 parts by weight, and further preferably 160 to 310 parts by weight, relative to 100 parts by weight of phloroglucinol.
[0087] (Pre-treatment process)
[0088] Manufacturing method 1 includes a pretreatment step for dissolving phloroglucinol and furfural in ethanol to obtain an ethanol solution. In the pretreatment step, phloroglucinol is first dissolved in ethanol. Next, furfural is dissolved in the ethanol solution of phloroglucinol. In addition, regarding the amount of ethanol during the dissolution, ethanol can be used in an amount that makes the concentration of the total amount of phloroglucinol and furfural in the ethanol solution become 1 to 45 weight %, preferably 1.5 to 30 weight %, and more preferably 2 to 25 weight %. In addition, in manufacturing method 1, the concentration of the total amount of phloroglucinol and furfural in the ethanol solution in the pretreatment step (raw material concentration in the solvent) is referred to as the initial concentration (weight %).
[0089] (Gelation process)
[0090] The production method 1 includes a gelling step for gelling the ethanol solution of phloroglucinol and furfural. In the gelling step, the ethanol solution of phloroglucinol and furfural obtained as described above is stirred and then left at room temperature to obtain a gelled solid.
[0091] (Cleaning process)
[0092] The manufacturing method 1 includes a washing step for washing the gelled solid. In the washing step, the gelled solid is washed. Ethanol can be used for washing, but it is not limited to this. Other alcohols can also be used. For example, the washing can be performed by repeatedly applying ethanol to the gelled product and discharging the applied ethanol to wash the gelled product. In addition, the washing step can be performed until the color of the discharged ethanol disappears.
[0093] (Supercritical drying process)
[0094] The manufacturing method 1 includes a supercritical drying step for the washed solid. The washed gelled solid is taken out and supercritically dried. Specifically, the gelled solid is placed in a sealed container and supercritical liquid CO is added at a given pressure. 2 Then, after maintaining this state, supercritical liquid CO 2 This process can be repeated as needed.
[0095] (Thermal Decomposition Process)
[0096] Manufacturing method 1 includes a thermal decomposition step of the supercritically dried solid. In the thermal decomposition step, the supercritically dried solid obtained as described above is placed in a furnace and heated to 800°C or above (e.g., 800°C to 1500°C, preferably 800°C to 1200°C, and more preferably 800°C to 1000°C) at a heating rate of 0.8 to 1.2°C / min in a nitrogen atmosphere. After the temperature is raised, the thermal decomposition is performed by maintaining the temperature for 5 to 60 minutes (preferably 20 to 30 minutes). As a result, components other than carbon are removed, and porous carbon can be obtained.
[0097] (Crushing process)
[0098] Manufacturing method 1 includes a pulverizing step for pulverizing and particle-forming the porous carbon obtained by the thermal decomposition step. In the pulverizing step, the heated porous carbon is returned to room temperature, and the porous carbon is pulverized to obtain a powdered porous carbon. In the pulverizing step, the porous carbon can be pulverized so that the porous carbon becomes a given particle size. In the pulverizing step, the average particle size of the porous carbon is preferably 0.01 to 50 μm, and more preferably 0.02 to 10 μm, for reasons of operability, etc. Regarding the average particle size, the particle size (average particle size: D50) at which the cumulative value of all particles is 50% can be set to be the above-mentioned particle size. The particle size distribution is measured by a laser diffraction / scattering particle size distribution measuring device LA-960 (laser diffraction scattering method) manufactured by Horiba, Ltd., and the D50 value is obtained based on the result of the particle size distribution measurement, thereby obtaining the average particle size D50.
[0099] As described above, porous carbon can be produced by production method 1.
[0100] [Manufacturing method 2]
[0101] In the method 2 for producing porous carbon that can be used in the present embodiment, porous carbon is produced by thermal decomposition of a raw material containing polyimide.
[0102] (Process of preparing materials)
[0103] The method 2 for producing porous carbon that can be used in the present embodiment includes a step of preparing materials. In the step of preparing materials, predetermined amounts of pyromellitic anhydride and p-phenylenediamine are prepared.
[0104] (Pre-treatment process)
[0105] Manufacturing method 2 includes a pretreatment process for synthesizing a polyimide solution. In the pretreatment process of manufacturing method 2, pyromellitic anhydride and p-phenylenediamine can be used as materials to synthesize a polyamic acid solution. In addition, dimethylacetamide and toluene can be used as solvents during the synthesis. The total weight of the solvent (dimethylacetamide and toluene) corresponding to the total weight of pyromellitic anhydride and p-phenylenediamine can be selected so that the initial concentration of the synthesized polyamic acid solution becomes a given range. In manufacturing method 2, the so-called initial concentration (weight %) refers to the concentration of polyamic acid in the polyamic acid solution in the pretreatment process (the ratio of the total weight of pyromellitic anhydride and p-phenylenediamine as raw materials to the weight of the synthesized polyamic acid solution). The initial concentration is 1 to 45 weight%, preferably 1.5 to 30 weight%, more preferably 2 to 25 weight, and further preferably 10 to 15 weight%. The synthesis of the polyamic acid solution can be carried out by mixing pyromellitic anhydride and p-phenylenediamine and heating. As a result, a polyamic acid solution can be synthesized. Next, a polyimide solution can be synthesized by adding predetermined amounts of pyridine and acetic anhydride to the polyamic acid solution obtained as described above.
[0106] (Gelation process)
[0107] The production method 2 includes a gelation step for gelling the polyimide solution. In the gelation step, the polyimide solution obtained as described above is stirred and then left to stand at room temperature to obtain a gelled solid.
[0108] (Washing process, supercritical drying process, heating process and pulverizing process)
[0109] Production method 2 includes a washing step, a supercritical drying step, a heating step, and a pulverizing step. In production method 2, after the gelation step, the washing step, supercritical drying step, heating step, and pulverizing step are performed in the same manner as production method 1, thereby producing porous carbon.
[0110] In the pyrolysis step of the manufacturing methods 1 and 2, the peak temperature of pyrolysis of the porous carbon that can be used in the present embodiment is 800° C. or higher, preferably 800° C. to 1500° C., more preferably 800° C. to 1200° C., and even more preferably 800° C. to 1000° C. When the peak temperature of pyrolysis is a given temperature, the porous carbon contained in the resin composition or the like for manufacturing a varistor having suitable varistor characteristics can be obtained more reliably.
[0111] The outline of the porous carbon described above is as follows.
[0112] (Structure of porous carbon 1)
[0113] The structure of porous carbon 1 is porous carbon. In a Raman spectrum obtained by measuring the porous carbon by Raman spectroscopy, at 1590 cm -1 The integrated intensity of the peak of the G band near 1350 cm -1 When the integrated intensity of the peak of the D band in the vicinity is defined as ID, ID / IG is equal to or greater than 2.0, the porous carbon has pores with a size of less than 1 μm, and the porous carbon is porous carbon for a varistor element.
[0114] By using the porous carbon of Structure 1, a resin composition for producing a varistor element having suitable varistor characteristics and a varistor element forming paste can be obtained.
[0115] (Structure of porous carbon 2)
[0116] The porous carbon structure 2 is the porous carbon based on the structure 1, and when the maximum intensity of the peak of the G band is MG and the maximum intensity of the peak of the D band is MD, MD / MG is 0.80 or more.
[0117] By using the porous carbon of Structure 2, it is possible to more reliably obtain a resin composition and a varistor element forming paste for producing a varistor element having suitable varistor characteristics.
[0118] (Structure of porous carbon 3)
[0119] The porous carbon having Structure 3 is a porous carbon based on Structure 1 or 2, and the peak temperature of thermal decomposition during the production of the porous carbon is 800° C. or higher and 1500° C. or lower.
[0120] By using the porous carbon of Structure 3, it is possible to more reliably obtain the porous carbon contained in the resin composition or the like for producing a varistor element having suitable varistor characteristics.
[0121] (Structure of porous carbon 4)
[0122] The porous carbon structure 4 is a porous carbon according to any one of structures 1 to 3, and is produced by thermal decomposition of a mixture of raw materials including furfural and phloroglucinol.
[0123] By using the porous carbon of Structure 4, it is possible to more reliably obtain the porous carbon contained in the resin composition or the like for producing a varistor element having suitable varistor characteristics.
[0124] (Structure of porous carbon 5)
[0125] The porous carbon of Structure 5 is a porous carbon based on Structure 4, wherein the raw material contains 100 to 500 parts by weight of furfural per 100 parts by weight of phloroglucinol.
[0126] In the porous carbon of Structure 5, by adjusting the blending amount of furfural relative to phloroglucinol to be within an appropriate range, the porous carbon contained in a resin composition or the like for producing a varistor element having appropriate varistor characteristics can be more easily obtained.
[0127] (Structure of porous carbon 6)
[0128] The porous carbon structure 6 is a porous carbon according to any one of the structures 1 to 3, and is produced by thermal decomposition of a raw material containing polyimide.
[0129] In the porous carbon of Structure 6, by using polyimide as a raw material, the porous carbon contained in a resin composition or the like for producing a varistor element having suitable varistor characteristics can be obtained more reliably.
[0130] By using the porous carbon (carbon aerogel) described above, a resin composition for forming a low-voltage varistor for producing a low-voltage varistor having excellent performance can be obtained.
[0131] <(B) Component>
[0132] The low voltage varistor forming resin composition of the present embodiment contains at least one selected from epoxy resin and acrylic resin as component (B).
[0133] The epoxy resin of component (B) preferably includes at least one selected from bisphenol A type epoxy resin, brominated bisphenol A type epoxy resin, bisphenol F type epoxy resin, biphenyl type epoxy resin, novolac type epoxy resin, alicyclic epoxy resin, naphthalene type epoxy resin, ether epoxy resin, polyether epoxy resin, and silicone epoxy copolymer resin.
[0134] By including a given epoxy resin in the resin composition, a varistor can be manufactured in which the material for the varistor is properly cured.
[0135] The resin composition for forming the low-voltage varistor of the present embodiment can use an acrylic resin in addition to the above-mentioned epoxy resin, or use an acrylic resin together with the epoxy resin as the (B) component. As a monomer of the acrylic resin, specifically, as an acrylic acid ester, methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, benzyl acrylate, dimethylaminoethyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, glycidyl acrylate, etc. are exemplified. As a methacrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, dimethylaminoethyl methacrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, glycidyl methacrylate, etc. are exemplified. In addition, a polymerization initiator for polymerizing the monomer to form an acrylic resin can be used.
[0136] <(C) Curing Agent>
[0137] The resin composition of the present embodiment preferably contains an amine compound, phenol, anhydride, imidazole compound or a mixture thereof as (C) a curing agent. The (C) curing agent preferably contains an amine compound and an imidazole compound. When the resin composition contains a given curing agent, the epoxy resin can be properly cured when manufacturing a varistor. In addition, in the following description, the (B) component and the (C) curing agent are sometimes referred to as "resin components".
[0138] The curing agent contained in the resin composition of the present embodiment preferably includes an imidazole compound. As the imidazole compound, imidazole and imidazole derivatives can be used. In the varistor of the present embodiment, when an imidazole compound, especially imidazole, is included as a curing agent, a varistor having better varistor characteristics, specifically, a higher nonlinear coefficient α can be obtained. Specifically, as an imidazole-based curing agent, "2P4MHZ-PW" manufactured by Shikoku Chemical Industries, Ltd. can be used. In addition, when the curing agent includes both an imidazole compound (especially imidazole) and an amine compound other than the imidazole compound, a varistor having a further higher nonlinear coefficient α can be obtained.
[0139] As amine compounds other than imidazole compounds, aliphatic amines, alicyclic amines, aromatic amines, 3,3'-diethyl-4,4'-diaminodiphenylmethane and diethyltoluenediamine can be selected and used. In particular, as amine compounds, 3,3'-diethyl-4,4'-diaminodiphenylmethane (aromatic amine curing agent "KAYAHARD AA", commercially available as (manufactured by Nippon Kayaku Co., Ltd.)) and / or diethyltoluenediamine (commercially available as "ETHACURE" manufactured by Albemarle Corporation) can be preferably used.
[0140] When the curing agent contained in the resin composition of the present embodiment includes an imidazole compound, the weight ratio of the imidazole compound contained in the total of the resin components (component (B) and curing agent (C)) is preferably 1 to 20 weight %, more preferably 2 to 15 weight %, and further preferably 5 to 10 weight %. By adding a predetermined amount of the imidazole compound, a varistor having a high nonlinear coefficient α can be reliably obtained.
[0141] When the curing agent contained in the resin composition of the present embodiment includes an amine compound other than an imidazole compound, the weight ratio of the amine compound contained in the total of the resin components (component (B) and curing agent (C)) is preferably 10 to 35 weight %, more preferably 15 to 30 weight %, and further preferably 20 to 27 weight %. By adding a predetermined amount of the amine compound other than the imidazole compound, a varistor having a high nonlinear coefficient α can be reliably obtained.
[0142] The resin composition of the present embodiment and the varistor forming paste described later preferably do not contain inorganic components (fillers, etc.) other than porous carbon, that is, preferably no filler. When the resin composition of the present embodiment is used, even a resin composition and a varistor forming paste with a simple structure that do not contain inorganic components such as fillers can manufacture a varistor with suitable varistor characteristics.
[0143] <Variator Forming Paste>
[0144] By using the resin composition for forming a low-voltage varistor of the present embodiment described above, a paste for forming a varistor can be obtained. The resin composition for forming a low-voltage varistor of the present embodiment can be used directly as a paste for forming a varistor. However, in screen printing, etc., in order to better apply the paste, the paste for forming a varistor can further contain (D) a dispersant and a solvent.
[0145] The paste for forming a varistor of the present embodiment can further contain (D) a dispersant. As the (D) dispersant, it is preferred to use at least one selected from the group consisting of anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, hydrocarbon surfactants, fluorine surfactants, silicon surfactants, polycarboxylic acids, polyether carboxylic acids, polycarboxylates, alkyl sulfonates, alkylbenzene sulfonates, alkyl ether sulfonates, aromatic polymers, organic conductive polymers, polyoxyalkylene surfactants, inorganic salts, organic acid salts and aliphatic alcohols. The (D) dispersant is preferably blended in an amount of 0.05 to 1 part by weight, and more preferably 0.1 to 0.7 parts by weight, relative to a total of 100 parts by weight of the above-mentioned resin composition (epoxy resin, curing agent and porous carbon).
[0146] In addition, the varistor forming paste of the present embodiment can contain a solvent. Examples of the solvent include aromatic hydrocarbons such as toluene and xylene, ketones such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, and esters such as acetates corresponding thereto, and terpineol. The solvent is preferably mixed in an amount of 2 to 10 parts by weight relative to a total of 100 parts by weight of the above-mentioned resin composition (epoxy resin, curing agent, and porous carbon).
[0147] The varistor forming paste of this embodiment can further contain at least one selected from the group consisting of colorants such as inorganic pigments and organic pigments, ion capture agents, flame retardants, silane coupling agents, leveling agents, thixotropic agents, elastomers, curing accelerators, metal complexes, dispersants and defoaming agents.
[0148] The above-mentioned (A) at least one selected from carbon nanotubes and carbon aerogels and (B) at least one selected from epoxy resins and acrylic resins, and (C) a curing agent and other components such as a solvent used as appropriate, can be put into a mixer such as a meteor mixer, a dissolver, a bead mill, a crusher, a three-roll mill, a rotary mixer or a two-axis mixer, and mixed to produce the varistor forming paste of the present embodiment. The resin composition suitable for the manufacture of varistors can be produced in this way. The varistor forming paste of the present embodiment can be adjusted to a varistor forming paste having a viscosity suitable for screen printing, dipping, or other desired coating or wiring forming methods.
[0149] The varistor forming paste of the present embodiment described above is applied so as to contact predetermined electrodes and then cured, thereby manufacturing a varistor having appropriate varistor characteristics. Examples of the application method include screen printing and dipping.
[0150] According to this embodiment of the present invention, a varistor having excellent varistor characteristics capable of operating at a low voltage can be obtained.
[0151] Example
[0152] The following examples are used to specifically describe the embodiments of the present invention, but the present invention is not limited thereto.
[0153] <Materials and Mixing Ratios of Resin Compositions of Examples>
[0154] The materials used in the manufacture of the resin composition for forming a low-voltage varistor of the embodiment are as follows. The weight ratios of the materials of the embodiment and the comparative example are shown in Table 1. In addition, the weight ratios of the components shown in Table 1 are all expressed in parts by weight, with the weight of the epoxy resin (B) being 100 parts by weight.
[0155] As the component (A), the following (A1) carbon nanotubes and (A2) carbon aerogel were used.
[0156] As the carbon nanotube (A1), a single-walled carbon nanotube (TUBALL SWCNT 93%, manufactured by OCSIAL) was used. The carbon nanotube (A1) was used in Example 1.
[0157] As (A2) carbon aerogel, carbon aerogel powder (PC16-151-10 manufactured by eM-TECH) was used. Carbon aerogel powder (PC16-151-10 manufactured by eM-TECH) was manufactured by the above-mentioned manufacturing method 1. At this time, the molar ratio of furfural: phloroglucinol was set to 3:1, and the amount of ethanol during dissolution was adjusted so that the concentration of the total amount of furfural and phloroglucinol in the ethanol solution was 4 weight%. In addition, carbon aerogel powder (PCI6-151-10) was prepared by calcining the aerogel as a precursor at 1000°C under a nitrogen flow. In addition, (A2) carbon aerogel was used in Example 2.
[0158] (B) Epoxy resin
[0159] The epoxy resin used in Example 1 is the epoxy resin B1 described below, and the epoxy resin used in Example 2 is the epoxy resin B2 described below.
[0160] Epoxy resin B1 is an epoxy resin obtained by mixing 60 wt% of bisphenol F epoxy resin and 40 wt% of bisphenol A epoxy resin. Here, as the bisphenol F epoxy resin, "YDF-8170" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd. was used. As the bisphenol A epoxy resin, "jER1001" manufactured by Mitsubishi Chemical Corporation was used.
[0161] Epoxy resin B2 is an epoxy resin obtained by mixing 80% by weight of bisphenol F epoxy resin and 20% by weight of bisphenol A epoxy resin. Here, as the bisphenol F epoxy resin, "YDF-8170" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd. was used. As the bisphenol A epoxy resin, "jER1001" manufactured by Mitsubishi Chemical Corporation was used.
[0162] As the (C) curing agent, the following two types of curing agent C1 and curing agent C2 were used.
[0163] Curing agent C1: an amine-based curing agent, 3,3′-diethyl-4,4′-diaminodiphenylmethane (“KAYAHARDA-A (HDAA)” manufactured by Nippon Kayaku Co., Ltd.).
[0164] Curing agent C2: Imidazole curing agent ("2P4MHZ-PW" manufactured by Shikoku Chemical Industry Co., Ltd.)
[0165] As the (D) dispersant, a polyether carboxylic acid ("HIPLAAD ED 451" manufactured by Kusumoto Chemicals Co., Ltd.) was used.
[0166] The components (A) to (D) in the weight ratios shown in Table 1 were mixed in a three-roll mixer to prepare a resin composition for forming a low voltage varistor.
[0167] <Manufacturing of Varistor of Example>
[0168] For the fabrication of varistor, use Figure 1 A substrate 12 having comb-shaped electrodes 14a and 14b as shown. As the substrate 12, a polyimide film with copper foil having a thickness of 8 μm is used, and the electrodes 14a and 14b are formed by photolithography. Furthermore, a 0.2 μm tin film is formed on the surface of the comb-shaped electrodes 14a and 14b by plating. The line width W of the electrode lines constituting the comb-shaped electrodes 14a and 14b is 35 μm, and the space width S as the width between the electrode lines is 35 μm. The length L of the overlapping portion where the electrode lines of the opposing electrodes 14a and 14b overlap is 10 mm.
[0169] Next, if Figure 2 As shown in FIG. 1 , the resin composition for forming the low-voltage varistor of the above-mentioned embodiments 1 and 2 is applied by screen printing so as to cover the low-voltage varistor formed on the Figure 1 The intersecting parts of the comb-shaped electrodes 14a and 14b on the surface of the substrate 12 are formed. Then, the substrate 12 coated with the resin composition for forming a low-voltage varistor is heated at a temperature of 165°C for 2 hours to form a cured body 16 of the resin composition for forming a low-voltage varistor, thereby manufacturing a low-voltage varistor. The thickness of the cured body 16 is 15 μm.
[0170] <Comparative Examples 1 and 2>
[0171] Commercially available low-voltage multilayer ceramic chip varistors (chip-shaped multilayer varistors manufactured by Panasonic Corporation) were used as varistors in Comparative Examples 1 and 2. The product name of the varistor in Comparative Example 1 is "EZJS1VB822", and the product name of the varistor in Comparative Example 2 is "EZJS2VB223".
[0172] <Evaluation>
[0173] Regarding Examples 1 and 2 and Comparative Examples 1 and 2 described above, various characteristics were measured and performance was evaluated as follows.
[0174] (Measurement of the current-voltage characteristics of a varistor)
[0175] The current-voltage characteristics of the low-voltage varistor of the embodiment and the commercially available comparative example manufactured as described above were measured using a source meter 2611B manufactured by Keithley. Specifically, a voltage was applied to a pair of electrodes (electrodes 14a and 14b) of the varistor in a varying manner, and the current value when a given voltage was applied was measured, thereby measuring the current-voltage characteristics of the varistor. Figure 3 , Figure 4 , Figure 5 as well as Figure 6 The current-voltage characteristics of Examples 1 and 2 and Comparative Examples 1 and 2 are shown.
[0176] (Regarding the voltage of the resistor)
[0177] from Figures 3 to 6 The current-voltage characteristic measurement data can be used to obtain the varistor voltage (V 0.1mA Table 2 shows the varistor voltage (V 0.1mA ).
[0178] (Calculation of nonlinear coefficient α)
[0179] Next, according to Figures 3 to 6 Specifically, the simulator analyzes the current-voltage characteristic data and calculates the coefficient suitable for I=K·V by curve fitting. α The calculation results of the nonlinear coefficient α of the varistor of the embodiment and the comparative example are shown in Table 2. When the nonlinear coefficient α of the varistor is 7 or more, it can be said that the overvoltage protection characteristic is excellent performance, so it can be said that it has good varistor characteristics.
[0180] (Measurement of electrostatic capacitance)
[0181] The electrostatic capacitance was measured using a capacitance meter 4288A manufactured by Agilent at an oscillator voltage of 1 Vrms and an oscillator frequency of 1 kHz. Table 2 shows the results of measuring the electrostatic capacitance of the varistors of the examples and comparative examples.
[0182] (Evaluation results)
[0183] As shown in Table 2, it can be seen that the varistor voltage of the varistors of Example 1 and Example 2 is less than 10V, which is lower than the varistor voltage of Comparative Example 1 and Comparative Example 2. Therefore, it is clear that the varistors of Example 1 and Example 2 are excellent in the characteristics of low-voltage varistors. In addition, the nonlinear coefficient α of the varistors of Example 1 and Example 2 is greater than 7, which is higher than the nonlinear coefficient α of Comparative Example 1 and Comparative Example 2. Therefore, it is clear that the overvoltage protection characteristics of the varistors of Example 1 and Example 2 as varistors are more excellent. In addition, the static capacitance of the varistors of Example 1 and Example 2 is less than 200pF, which is lower than the static capacitance of Comparative Example 1 and Comparative Example 2. Therefore, it is clear that the varistors of Example 1 and Example 2 have high impedance at high frequencies and are more excellent as low-voltage varistors in the high-frequency region.
[0184] [Table 1]
[0185]
[0186] [Table 2]
[0187]
[0188] <Reference Examples and Comparative Examples>
[0189] Next, the reference examples and reference comparative examples of the present embodiment are described. The present invention is not limited to the reference examples and reference comparative examples. In addition, in the following description, the so-called "porous carbon" refers to carbon aerogel. The carbon aerogel (porous carbon) described below can be used as a raw material (carbon aerogel) of a resin composition for forming a low-voltage varistor for manufacturing the low-voltage varistor of the present embodiment.
[0190] <Production of porous carbon>
[0191] First, the method for producing the porous carbon used in the reference examples and the reference comparative examples will be described. Tables 3 and 4 show the materials and production conditions used in producing the porous carbon used in the reference examples and the reference comparative examples. The porous carbons of reference examples 2 to 4 and reference comparative examples 1 to 4 are produced by production method 1 using furfural and phloroglucinol as materials (raw materials). The porous carbons of reference example 1 and reference comparative example 5 are produced by production method 2 using pyromellitic acid and p-phenylenediamine as main materials (raw materials).
[0192] <Manufacturing Method 1: Manufacturing Method of Porous Carbon Referring to Examples 2 to 4 and Comparative Examples 1 to 4>
[0193] Table 3 shows the blending amounts of the materials of the porous carbons of Reference Examples 2 to 4, and Table 4 shows the blending amounts of the materials of the porous carbons of Reference Comparative Examples 1 to 4.
[0194] (Process of preparing materials)
[0195] In the method for producing porous carbon of Reference Examples 2 to 4 and Reference Comparative Examples 1 to 4 (Production Method 1), first, given amounts of furfural and phloroglucinol described in Tables 3 and 4 were prepared.
[0196] (Pre-treatment process)
[0197] Next, phloroglucinol is dissolved in ethanol. Next, furfural is dissolved in the ethanol solution of phloroglucinol. In addition, during the dissolution, ethanol is used so that the total weight of phloroglucinol and furfural becomes the initial concentration shown in Table 3 and Table 4. In the manufacturing method 1, the so-called initial concentration (weight %) refers to the concentration of the total amount of phloroglucinol and furfural in the ethanol solution (raw material concentration in the solvent).
[0198] (Gelation process)
[0199] Next, the ethanol solution of phloroglucinol and furfural obtained as described above is stirred and then allowed to stand at room temperature to form a gel.
[0200] (Cleaning process)
[0201] Next, the gelled solid is washed. Ethanol is used for washing. The gelled product is washed by repeatedly applying ethanol to the product obtained by gelling and draining the applied ethanol. In addition, washing is performed until the coloring of the drained ethanol disappears.
[0202] (Supercritical drying process)
[0203] Next, the washed gelled solid is taken out and supercritically dried. Specifically, the solid is placed in a sealed container and supercritical liquid CO is added. 2 Then, the state is maintained for a certain period of time, and then the supercritical liquid CO 2 By repeatedly performing supercritical liquid CO 2 The introduction and discharge of the supercritical drying are carried out.
[0204] (Thermal Decomposition Process)
[0205] The supercritically dried solid obtained as described above is placed in a furnace, and in a nitrogen atmosphere, the temperature is raised to 800°C or higher (specifically, the calcination temperature described in Tables 3 and 4) at a heating rate of 1°C / min in the case of the reference example, thereby performing thermal decomposition. After the temperature is raised, the temperature is maintained for 30 minutes. As a result, components other than carbon are removed, and porous carbon can be obtained.
[0206] (Crushing process)
[0207] The heated porous carbon was returned to room temperature and pulverized to obtain porous carbons of Reference Examples 2 to 4 and Reference Comparative Examples 1 to 4.
[0208] <Manufacturing Method 2: Manufacturing Method of Porous Carbon Referring to Example 1 and Comparative Example 5>
[0209] Table 3 shows the blending amounts of the porous carbon materials of Reference Example 1, and Table 4 shows the blending amounts of the porous carbon materials of Reference Comparative Example 5.
[0210] (Process of preparing materials)
[0211] In the method for producing porous carbon (production method 2) of Reference Example 1 and Reference Comparative Example 5, first, given amounts of pyromellitic acid and p-phenylenediamine described in Tables 3 and 4 were prepared.
[0212] (Pre-treatment process)
[0213] Next, pyromellitic acid and p-phenylenediamine are used as materials to synthesize polyamic acid solution. In addition, as the solvent during the synthesis, a solvent (dimethylacetamide and toluene) is used to make the total weight of pyromellitic anhydride and p-phenylenediamine as raw materials become the weight of the initial concentration shown in Table 3 and Table 4 in the polyamic acid solution. The solvent used as solvent uses a mixed solvent of dimethylacetamide and toluene. The synthesis of polyamic acid solution is carried out by mixing pyromellitic acid and p-phenylenediamine and heating. As a result, polyamic acid solution can be synthesized. Next, the polyamic acid solution obtained as above is added with a given amount of pyridine and acetic anhydride recorded in Table 3 and Table 4. As a result, polyimide solution can be obtained.
[0214] (Gelation process)
[0215] Next, the mixture is stirred and then left to stand at room temperature to obtain a gelled solid.
[0216] (Other processes)
[0217] Thereafter, the porous carbon of Reference Example 1 and Reference Comparative Example 5 can be produced by performing the washing step, supercritical drying step, thermal decomposition step, and pulverization step in the same manner as in Production Method 1. The temperature after the heating step is set to the temperature described in Tables 3 and 4.
[0218] In addition, the pulverization step was performed so that the average particle size D50 of the porous carbon of the reference example and the reference comparative example became 25 nm.
[0219] <Scanning electron microscope (SEM) photo>
[0220] Scanning electron microscope (SEM) photographs of the surfaces of the porous carbons of Reference Example 1, Reference Example 2 and Reference Comparative Example 2 obtained as described above were taken. Figures 7 to 12 The SEM photograph of Reference Example 1 is shown in Figure 7 (magnification: 10,000 times) and Figure 8 (magnification: 100,000 times) is shown. Fig. 9 (magnification: 10,000 times) and Fig.10 (magnification: 100,000 times) is shown. Fig.11 (magnification: 10,000 times) and Fig.12 (Magnification: 100,000 times) In the SEM photographs of Reference Example 1 and Reference Example 2, a large number of pores less than 1 μm can be seen. In contrast, in the SEM photograph of Reference Comparative Example 2, it cannot be said that a large number of pores less than 1 μm exist, and a relatively smooth surface can be seen.
[0221] <Measurement by Raman spectroscopy>
[0222] The porous carbons of the reference examples and reference comparative examples obtained as described above were measured by Raman spectroscopy to obtain Raman spectra. Figures 13-15 Raman spectra of Reference Example 1, Reference Example 2, and Reference Comparative Example 2 are shown respectively. Figures 13-15 The horizontal axis is the Raman shift (unit: cm -1 ), the vertical axis is the signal intensity of Raman scattered light (arbitrary unit).
[0223] In addition, as a Raman spectroscopic measuring device, "Cora 7100" (manufactured by Anton Paar) was used. The irradiated laser was set to have a wavelength of 532 nm and an intensity of 50 mW, and the measuring time was set to 60 seconds. Figures 13-15 As clearly shown in the Raman spectrum, a wavelength of 1590 cm -1 The peak of the G band near 1350cm -1 In addition, processing such as subtracting the background from the obtained signal can be performed as needed.
[0224] The Raman spectrum at 1590 cm was calculated from the Raman spectrum obtained by Raman spectroscopy. -1 The cumulative intensity of the peak of the G band near G and 1350cm -1 The accumulated intensity of the peak value of the D band near D , calculate the ratio of the cumulative intensity of the G band and the D band (I D / I GThe ratio of the cumulative intensity of the G band and the D band of the porous carbon of the reference example and the reference comparative example (I D / I G ) are shown in Table 3 and Table 4.
[0225] Similarly, the maximum intensity M of the peak of the G band is obtained from the obtained Raman spectrum by Raman spectroscopy. G and the maximum intensity M of the peak of the D band D , calculate the ratio of the maximum intensities of the peaks of the G band and the D band (M D / M G The ratio of the maximum intensities of the peaks of the G band and the D band of the reference example and the reference comparative example (M D / M G ) are shown in Table 3 and Table 4.
[0226] <Materials and Mixing Ratios of Resin Composition>
[0227] The materials used in the resin compositions of the reference examples and reference comparative examples are as follows. Tables 3 and 4 show the mixing ratios of the materials of the reference examples and reference comparative examples.
[0228] (Epoxy resin)
[0229] The epoxy resin used in the reference examples and reference comparative examples is a mixture of bisphenol F epoxy resin ("YDF-8170" manufactured by Nippon Steel & Sumitomo Metal Corporation) (80 wt%) and bisphenol A epoxy resin ("1001" manufactured by Mitsubishi Chemical Corporation) (20 wt%).
[0230] (Curing agent)
[0231] In the resin compositions of the reference examples and the reference comparative examples, a mixture of an amine-based curing agent and an imidazole-based curing agent was used as a curing agent.
[0232] As the amine-based curing agent, “KAYAHARD AA (HDAA)” (3,3′-diethyl-4,4′-diaminodiphenylmethane) manufactured by Nippon Kayaku Co., Ltd. was used.
[0233] As the imidazole-based curing agent, "2P4MHZ-PW" manufactured by Shikoku Chemicals Co., Ltd. was used.
[0234] (Compounding ratio of epoxy resin and curing agent)
[0235] The amounts of the epoxy resin and the curing agent (total 100 wt%) were 67.63 wt% of the epoxy resin, 25.61 wt% of the amine curing agent, and 6.76 wt% of the imidazole curing agent.
[0236] (Porous carbon (carbon aerogel))
[0237] In the resin compositions of the reference example and the reference comparative example, the blending amounts of the epoxy resin and the curing agent were set to 100 parts by weight, and 5 parts by weight of the porous carbon was used.
[0238] (Other ingredients)
[0239] In the resin compositions of the reference examples and reference comparative examples, in addition to the epoxy resin, the curing agent and the porous carbon, 0.50 parts by weight of a silane coupling agent (KBM-403 manufactured by Shin-Etsu Silicone Co., Ltd.) and 0.25 parts by weight of a dispersant (HIPLAAD ED-451 manufactured by Kusumoto Chemicals Co., Ltd.) are used when the amount of the epoxy resin and the curing agent is set to 100 parts by weight.
[0240] Next, the epoxy resin, curing agent, porous carbon, silane coupling agent, and dispersant in the above-mentioned mixing ratio were mixed with a planetary mixer, and further dispersed and paste-formed with a three-roll mill to produce a varistor element forming paste.
[0241] <Trial production of varistor elements>
[0242] use Figure 1 The substrate 12 has comb-shaped electrodes 14a and 14b as shown. A multilayer printed wiring board (with copper foil) made of FR-4 is used as the substrate 12. The electrodes 14a and 14b are formed by patterning the copper foil of the multilayer printed wiring board.
[0243] Next, if Figure 2 As shown in FIG. 1 , the resin composition of the reference example and the reference comparative example manufactured as described above was screen-printed so as to cover the comb-shaped electrodes 14a and 14b formed on the surface of the substrate 12, and the epoxy resin was cured to form a cured body 16. The epoxy resin was cured by keeping it at a temperature of 165° C. for 2 hours. The thickness of the cured epoxy resin was 90 μm in all cases. The varistor elements of the reference example and the reference comparative example were trial-produced as described above.
[0244] <Measurement of Current-Voltage Characteristics of Varistor Element and Calculation of Nonlinear Coefficient α>
[0245] The current-voltage characteristics of the varistor elements of the reference example and the reference comparative example manufactured as described above are measured. Specifically, a given voltage is applied to a pair of electrodes (electrode 14a and electrode 14b) of the varistor element, and the current value flowing therethrough is measured, thereby measuring the current-voltage characteristics of the varistor element.
[0246] <Calculation of Nonlinear Coefficient α>
[0247] K can be set as a constant, α can be set as a nonlinear coefficient, and I = K·V α The current-voltage characteristic of the varistor element is approximated. The nonlinear coefficient α is calculated by fitting based on the current-voltage characteristic of the varistor element. Tables 3 and 4 show the calculation results of the nonlinear coefficient α of the varistor element of the reference embodiment and the reference comparative example. When the nonlinear coefficient α of the varistor element is 6.5 or more, it can be said that it has suitable varistor characteristics that can withstand use.
[0248] As is clear from Tables 3 and 4, the nonlinear coefficients α of Reference Examples 1 to 4 are all 6.5 or more, which are higher than those of Comparative Examples 1 and 2. This means that in the Raman spectrum of porous carbon, if the integrated intensity I including the peak of the G band is used, G and the cumulative intensity of the peak value of the D band I D The ratio (I D / I G ) is 2.0 or more, a varistor element having suitable varistor characteristics that can be used with durability can be manufactured. In addition, in the Raman spectra of the porous carbon of Reference Examples 1 to 4, the maximum intensity M of the peak of the G band is G and the maximum intensity M of the peak of the D band D The ratio (M D / M G ) is greater than 0.80.
[0249] In contrast, the nonlinear coefficients α of all comparative examples 1 to 5 were less than 2.2, and they did not have suitable varistor characteristics for durability. G and the cumulative intensity of the peak value of the D band I D The ratio (I D / I G ) is less than 2. In addition, the maximum intensity M of the peak of the G band of the porous carbon of reference examples 1 to 5 is G and the maximum intensity M of the peak of the D band D The ratio (M D / M G ) is less than 0.8.
[0250] From the above, it was found that a varistor element having suitable varistor characteristics that can withstand use can be obtained by using a resin composition containing porous carbon having a predetermined Raman spectrum.
[0251] [Table 3]
[0252]
[0253] [Table 4]
[0254]
[0255] Description of Reference Numerals
[0256] 10. Varistor
[0257] 12. Substrate
[0258] 14a, 14b Electrode
[0259] 16 solid body
Claims
1. A low voltage varistor having a varistor voltage of 10 V or less, comprising a cured product of a resin composition for forming a low voltage varistor, The low voltage resistor is characterized in that The resin composition for forming a low voltage varistor comprises: (A) at least one selected from carbon nanotubes and carbon aerogels; and (B) epoxy resin, or epoxy resin and acrylic resin, The content of the carbon nanotubes is 0.01 parts by weight or more and less than 0.05 parts by weight based on 100 parts by weight of the epoxy resin (B), or the content of the carbon aerogel is 0.1 to 10 parts by weight based on 100 parts by weight of the epoxy resin (B).
2. The low voltage resistor according to claim 1, characterized in that: When the inflow current of the low-voltage resistor is 0.1mA, the resistor voltage is 0.3~10V.
3. The low voltage resistor according to claim 1 or 2, characterized in that: When the current-voltage characteristic of the low-voltage resistor is I=KV α When characterizing, the nonlinear coefficient α is 7 to 20. Wherein, V is the applied voltage, I is the inflow current, K is a constant, and α is the nonlinear coefficient.
4. The low voltage resistor according to claim 1 or 2, characterized in that: The electrostatic capacitance is 0.5~200pF.
5. The low voltage resistor according to claim 1 or 2, characterized in that: The resin composition for forming a low voltage varistor includes carbon aerogel, In the Raman spectrum obtained by measuring carbon aerogel using Raman spectroscopy, In 1590cm -1 The cumulative intensity of the peak value of the G band nearby is set to I G 、1350cm -1 The accumulated intensity of the peak value of the nearby D band is set to I D When D / I G is 2.0 or above, The maximum intensity of the peak value of the G band is set to M G , set the maximum intensity of the peak value of the D band to M D When M D / M G It is above 0.
80.
6. A circuit substrate, characterized in that: The low-voltage varistor according to any one of claims 1 to 5 is mounted.
7. A semiconductor component package, characterized in that: The low-voltage varistor according to any one of claims 1 to 5 is mounted.
8. An internal plug-in unit, characterized in that: The low-voltage varistor according to any one of claims 1 to 5 is mounted.
Citation Information
Patent Citations
Laminated ceramic varistor and method for manufacture thereof
JP2001093706A
Resin composition, paste for forming a varistor element, and varistor element
US10141090B2
Device applications for voltage switchable dielectric material having high aspect ratio particles
US7695644B2
Polymer-carbon composites for temperature-dependent electrical switching applications
US20170261456A1
Resin composition for forming varistor, and varistor
WO2019116955A1