A composite amino acid assembly film on carbon steel surface and its preparation method and application
By using a composite synergist of amino acids and long-chain fatty acids or amines on the surface of carbon steel for gas-phase self-assembly to form a self-assembly film, the problem of poor volatility and toxic substance use of amino acid compounds in gas-phase corrosion inhibitors is solved, and the problem of poor volatile and toxic substances is achieved. It has efficient and environmentally friendly anti-corrosion effect of steel materials.
Patent Information
- Application Number
- CN202210602627.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-05-30
AI Technical Summary
The application of existing amino acid compounds in gas-phase corrosion inhibitors is limited by their high polarity and poor volatility. Traditional gas-phase corrosion inhibitors often contain toxic and harmful substances, resulting in low environmental protection and low use efficiency.
The combination and efficiency-synthesis method is adopted, combined with long-chain fatty acids or long-chain fatty amines as synergists and matches amino acids, and a self-assembly film is formed on the surface of carbon steel through gas-phase self-assembly technology to improve the volatility of amino acids and the density of the film. Avoid waste liquid discharge.
It effectively improves the corrosion resistance of steel materials, achieves an environmentally friendly gas-phase corrosion inhibition effect, avoids the use of toxic substances, is easy to operate, and is pollution-free.
Smart Images

Figure CN115233226B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal corrosion protection, and in particular to a carbon steel surface composite amino acid assembly film and a preparation method and application thereof. Background Art
[0002] Steel is one of the most widely used metal materials due to its low price and wide adaptability. It is widely used in automobiles, buildings, pipelines, etc. However, the existence of atmospheric corrosion seriously restricts the service life of steel materials. Therefore, improving the corrosion resistance of steel materials is extremely important for its production and application process.
[0003] Corrosion inhibitor is a commonly used anti-corrosion method. It has the characteristics of high protection efficiency, wide adaptability and low price, and plays an important role in metal protection. In the traditional anti-rust treatment process, people often use some low-cost but highly toxic corrosion inhibitors. With the increasingly stringent environmental protection requirements, it is urgent to develop environmentally friendly corrosion inhibitors.
[0004] Amino acid compounds can be prepared by protein hydrolysis and are non-toxic and easily degradable. Amino acid compounds contain heteroatoms such as S, N, and O, and can form coordination compounds with metal ions. They have good corrosion inhibition effects on metal materials and have become one of the main directions for the development of green and environmentally friendly corrosion inhibitors. Amino acids are amphoteric compounds, showing negative charge in alkaline solutions, positive charge in acidic media, and electrical neutrality under isoelectric point conditions. Amino acid molecules are highly polar and difficult to volatilize, and are often used as liquid phase corrosion inhibitors. Chinese invention patent application CN113801047A discloses a metal corrosion inhibitor and a preparation method thereof, which is characterized in that α-amino acid is used as a raw material, alkali solution and p-tert-butylbenzoyl chloride are added for reaction, and then extraction and purification are performed. Chinese invention patent application CN109136936A discloses a water-based metal corrosion inhibitor, which is characterized in that it contains one or more amino acids. The application of these metal surface treatment solutions containing amino acid compounds has the problems of wastewater pollution and large usage.
[0005] Gas phase corrosion inhibitor has the ability to volatilize and gasify. It automatically and continuously sublimates at room temperature, volatilizes into gas, reaches the metal surface to form a corrosion-inhibiting film, can effectively isolate the corrosive medium, thereby avoiding the corrosion of the metal, and becomes a main material for preventing atmospheric corrosion of metal products. At present, most of the gas phase corrosion inhibition materials used at home and abroad contain toxic and harmful substances such as nitrite, which seriously restricts the promotion and application of gas phase corrosion inhibition technology. Therefore, the development of gas phase corrosion inhibitors that do not contain nitrite has become a research focus. Chinese invention patent CN1320164C discloses a gas phase corrosion inhibitor for industrial equipment protection and its preparation method, the main components of which are cyclohexylamine, ethanolamine, etc. These gas phase corrosion inhibitors have certain toxicity and poor actual performance.
[0006] Although amino acid compounds are used in metal surface treatment liquids, the high polarity and difficulty in volatilization of amino acid molecules limit their application in vapor phase corrosion inhibitors. Summary of the invention
[0007] The purpose of the present invention is to provide a composite amino acid assembled film on the surface of carbon steel and its preparation method and application in order to solve at least one of the above problems. The volatility of amino acids is improved by compounding and enhancing the effect, and a self-assembled film is formed on the steel surface by gas phase self-assembly to improve the corrosion resistance of the steel material.
[0008] The self-assembled membrane technology used in the present invention refers to a technology in which active molecules with appropriate structures spontaneously form ordered structure films on the surface of materials such as metal substrates. The applicant has realized the advantages of the self-assembled membrane technology from the beginning of the conception, such as fast film formation speed, few defects, high coverage, and low cost, and intends to apply it to metal surface treatment. At the same time, the applicant believes that the gas phase self-assembly technology has the characteristics of easy operation because it does not require the preparation of metal surface treatment solutions and there is no discharge of waste liquid.
[0009] The purpose of the present invention is achieved through the following technical solutions:
[0010] The first aspect of the present invention discloses a carbon steel surface composite amino acid assembly film, comprising the following components in percentage by mass:
[0011] Synergist 50-55%;
[0012] Amino acids 45-50%.
[0013] Preferably, the synergist is a long-chain fatty acid and / or a long-chain fatty amine. Long-chain fatty acids and long-chain fatty amines have an amphiphilic structure and can form a hydrophobic protective film on the metal surface.
[0014] Preferably, the long-chain fatty acid is a long-chain fatty acid having 8 or more carbon atoms.
[0015] Preferably, the long-chain fatty acid is lauric acid.
[0016] Preferably, the long-chain fatty amine is a long-chain fatty amine having 8 or more carbon atoms.
[0017] Preferably, the long-chain fatty amine is dodecylamine.
[0018] Preferably, the amino acid is alanine, lysine or phenylalanine. Alanine and phenylalanine are small molecular non-polar amino acids, and lysine is a basic amino acid. These amino acids are relatively volatile and more suitable for use in gas phase self-assembly.
[0019] The second aspect of the present invention discloses a method for preparing any one of the above carbon steel surface composite amino acid assembly films, comprising the following steps:
[0020] S1: Mix the synergist and the amino acid and grind them thoroughly to obtain a compound corrosion inhibitor;
[0021] S2: placing the compound corrosion inhibitor obtained in step S1 at the bottom of a sealed container, and placing the carbon steel to be treated above the compound corrosion inhibitor in the sealed container, and heating to obtain the carbon steel surface composite amino acid assembly film.
[0022] Preferably, the heating temperature in step S2 is 50-80°C and the heating time is 6-12 hours. Increasing the temperature and extending the time can improve the gas phase volatilization ability of the agent, thereby forming a good quality self-assembled film on the metal surface. However, too high a temperature and too long a time cannot improve the effect of gas phase self-assembly, but will reduce the efficiency of the treatment.
[0023] The third aspect of the present invention discloses an application of any of the above-mentioned composite amino acid assembled films on the surface of carbon steel in metal corrosion protection.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention adopts a composite synergistic method. By adding a synergist (long-chain fatty acid or long-chain fatty amine), the volatility of amino acids can be effectively improved, and the application range of amino acid corrosion inhibitors can be expanded; amino acids have good affinity with metal surfaces, and long-chain fatty acids or long-chain fatty amines can improve the hydrophobicity of the surface film, thereby improving the compactness and integrity of the self-assembled film on the surface of carbon steel. When used, a self-assembled film is formed on the steel surface by gas phase self-assembly. The raw materials used are simple, the operation is simple, and there is no pollution; after testing, the self-assembled film can effectively improve the corrosion resistance of steel materials.
[0026] 2. The assembled membrane of the present invention only contains amino acids and long-chain fatty acids or long-chain fatty amines, so the membrane is an environmentally friendly self-assembled membrane, avoiding the use of toxic and harmful substances such as nitrites contained in most existing vapor phase corrosion inhibition material formulas, and is more in line with market development and user needs. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 FT-IR reflection spectra of carbon steel samples: (a) carbon steel sample of Example 1; (b) carbon steel sample of Example 2;
[0028] Figure 2 The graphs are the results of the volatility weight loss experiments of the corrosion inhibitors of Example 1 and Example 2;
[0029] Figure 3The actual pictures of the wet heat test results are (a) blank carbon steel test piece; (b) carbon steel sample of Example 1; (c) carbon steel sample of Example 2;
[0030] Figure 4 (a) Nyquist plots of blank electrode and gas-phase assembled corroded electrode in 0.1 mol / L NaCl solution;
[0031] Figure 4 (b) Bode impedance film value diagram of blank electrode and gas phase assembled corroded electrode in 0.1 mol / L NaCl solution;
[0032] Figure 4 (c) Bode phase diagram of blank electrode and gas-phase assembled corroded electrode in 0.1 mol / L NaCl solution; Figure 4 (d) Electrochemical equivalent circuit diagram;
[0033] Figure 5 These are the polarization curves of the blank electrode and the gas phase assembled electrode in 0.1 mol / L NaCl solution. DETAILED DESCRIPTION
[0034] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0035] Unless otherwise specified, the reagents used in the following examples can be commercially available products that can be routinely purchased by those skilled in the art.
[0036] The corrosion inhibition performance evaluation method of the self-assembled film obtained by the present invention includes the following: using an electrochemical workstation (Solartron 1287 / Solartron 1260) to perform electrochemical impedance spectroscopy and polarization curves to determine the corrosion inhibition performance of the self-assembled film. Using a vapor phase corrosion inhibition capability experiment, the corrosion resistance of the vapor phase assembled film on the carbon steel surface is investigated by observing the corrosion morphology.
[0037] Example 1
[0038] Weigh 0.25g of lysine (LS) and 0.25g of dodecylamine (DA), grind them thoroughly and dry them to obtain the composite corrosion inhibitor sample of Example 1. Place the ground and dried composite corrosion inhibitor sample at the bottom of a 1L glass container, and place the polished carbon steel electrode on the partition 5cm away from the sample in the container without directly contacting the sample. Place the glass container in a 50°C electric oven and perform vapor phase self-assembly for 6h to form a corrosion inhibition film on the carbon steel surface to obtain the carbon steel sample of Example 1, and its infrared reflection spectrum is shown in FIG. Figure 1 (a), it can be seen that an organic protective film is formed on the surface of the carbon steel sample.
[0039] Example 2
[0040] Weigh 0.25g of lysine (LS) and 0.25g of dodecanoic acid (LA), grind them thoroughly and dry them to obtain the compound corrosion inhibitor sample of Example 2. Place the ground and dried compound corrosion inhibitor sample at the bottom of a 1L glass container, and place the polished carbon steel electrode on the partition 5cm away from the sample in the container without direct contact with the drug. Place the glass container in an electric oven at 60°C and perform vapor phase self-assembly for 6h to form a corrosion inhibition film on the carbon steel surface to obtain the carbon steel sample of Example 2, and its infrared reflection spectrum is shown in FIG. Figure 1 (b), it can be seen that an organic protective film is formed on the surface of the carbon steel sample.
[0041] Example 3
[0042] 2g of the corrosion inhibitor sample of Example 1 and 2g of the corrosion inhibitor sample of Example 2 were evenly distributed in a 5cm diameter surface dish. The surface dishes were then placed in a 50°C oven for 72 hours. The surface dishes were taken out every 24 hours to weigh the mass loss and calculate the weight loss. The results are shown in Figure 2 It can be seen that the volatility of the corrosion inhibitor samples of Example 1 and Example 2 is improved compared with lysine.
[0043] Example 4
[0044] Insert an aluminum tube (outer diameter d=16mm, wall thickness 1.5mm, length 114mm) into the rubber stopper of a 500mL wide-mouth bottle. Place the assembled blank carbon steel specimen, the carbon steel sample of Example 1, and the carbon steel sample of Example 2 at the bottom of the aluminum tube, respectively. Pour 10mL of deionized water into a 1L wide-mouth bottle. After the wide-mouth bottle was placed at 25°C for 20 hours, an ice / water mixture was filled into the above aluminum tube. Condensation caused dew to form on the surface of the carbon steel sample. After 3 hours of condensation, it was taken out for observation. The results are shown in Table 1.
[0045] Table 1 Corrosion of different carbon steel samples under the gas phase corrosion inhibition test
[0046]
[0047] As can be seen from Table 1, the corrosion phenomenon of the blank carbon steel test piece under condensation is more serious, with an average number of rust points of 25.3, and uniform corrosion occurs on the metal surface. Compared with the blank test piece, the number of rust points of the carbon steel sample in Example 1 and the carbon steel sample in Example 2 is significantly reduced.
[0048] Example 5
[0049] The wet heat lamination test accelerates the corrosion of the test piece by simulating a high temperature and humid environment. The blank carbon steel test piece, the carbon steel sample of Example 1 and the carbon steel sample of Example 2 were respectively attached together with two plexiglass plates with four fixing screws. A torque wrench was used to apply a force of 5N to each screw. After tightening, they were placed in a wet heat box for the experiment. The temperature of the wet heat box was 49°C and the humidity was 98%. After 24 hours, the test piece was taken out to observe the rust condition. Figure 3 The blank carbon steel test piece showed serious corrosion, with rust evenly distributed on the metal surface, and the corrosion at the edge was more serious. The rust of the carbon steel sample in Example 1 and the carbon steel sample in Example 2 was much reduced, and basically no rust occurred.
[0050] Example 6
[0051] The carbon steel samples of Example 1 and Example 2 were made into working electrodes respectively, and electrochemical impedance spectroscopy was tested using a three-electrode system, with a platinum electrode as an auxiliary electrode (CE), a saturated calomel electrode (SCE) as a reference electrode (RE), and a 0.1 mol / L NaCl solution as the measuring electrolyte. The electrochemical impedance used a 5 mV sinusoidal signal with a scanning frequency of 100 kHz to 0.01 Hz.
[0052] Corrosion inhibition rate η R The calculation formula is as follows:
[0053]
[0054] Among them, R p is the polarization resistance of the carbon steel electrode assembled with the corrosion inhibition film, R p,0 is the polarization resistance of the blank carbon steel electrode. The obtained electrochemical impedance spectrum is Figure 4 , where the electrochemical equivalent circuit diagram is shown in Figure 4 (d), Table 2 shows the fitted electrochemical impedance parameters.
[0055] Table 2 Electrochemical impedance spectroscopy fitting parameters of blank electrode and gas phase assembled electrode in 0.1 mol / L NaCl solution
[0056]
[0057] Figure 4 (a) shows that the impedance arc radius of the carbon steel sample in Example 1 and the carbon steel sample in Example 2 is significantly larger than the impedance arc radius of the blank electrode, reflecting the inhibitory effect of the vapor phase assembled film on the corrosion process of carbon steel. Figure 4 (b) and Figure 4(c) shows that the impedance modulus of the gas phase self-assembled carbon steel electrode is significantly larger than that of the blank carbon steel electrode, the phase angle maximum moves toward the high frequency direction, and two time constant characteristics appear, which indicates that a self-assembled film is formed on the carbon steel surface, which can effectively protect the carbon steel substrate.
[0058] Table 2 shows the impedance values after fitting. The polarization resistance (R p ) is much larger than the blank electrode R p The value indicates that the gas phase assembled membrane improves the corrosion resistance of carbon steel and effectively inhibits the corrosion of carbon steel. R ) reached 89.6%, and the protection efficiency of Example 2 reached 88.9%.
[0059] Example 7
[0060] The samples of Example 1 and Example 2 were made into working electrodes, and electrochemical impedance spectroscopy was measured using a three-electrode system, with a platinum electrode as the auxiliary electrode (CE), a saturated calomel electrode (SCE) as the reference electrode (RE), and a 0.1 mol / L NaCl solution as the measuring electrolyte. The polarization curve was scanned at a speed of 1 mV / s. The Tafel slopes of the cathode and anode were βc and βa, respectively, and the corrosion potential and corrosion current density were E corr and i corr The polarization curve is represented by the curve of the measured current density I changing with the value of the electrode potential E. The Tafel extrapolation method is usually used to determine the corrosion current density. Protection efficiency η i The calculation method is as follows:
[0061]
[0062] Among them, i corr,0 and i corr They are the corrosion current density of the blank carbon steel electrode and the carbon steel electrode modified by vapor phase assembly.
[0063] Figure 5 Table 3 shows the polarization curves of the carbon steel sample in Example 1 and the carbon steel sample in Example 2. Table 4 shows the fitted electrochemical polarization curve parameters.
[0064] Table 3 Electrochemical polarization fitting parameters of blank electrode and gas phase assembled electrode in 0.1 mol / L NaCl solution
[0065]
[0066] from Figure 5It can be seen from Table 3 that the corrosion potential of the gas phase self-assembled carbon steel electrode moves in the positive direction compared with the corrosion potential of the blank carbon steel electrode. The gas phase self-assembled film has a significant inhibition on the corrosion anodic process of the carbon steel electrode, and the corrosion electric density of the gas phase assembled carbon steel electrode is significantly reduced, which shows that the gas phase assembly technology of the present invention has a good anti-corrosion protection effect on carbon steel.
[0067] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing a composite amino acid assembly film on a carbon steel surface, characterized in that: The carbon steel surface composite amino acid assembly film comprises the following components in percentage by mass: Synergist 50-55%; Amino acids 45-50%; The synergist is a long-chain fatty acid and / or a long-chain fatty amine; The preparation method is to form a self-assembled film on the steel surface by gas phase self-assembly, comprising the following steps: S1: Mix the synergist and the amino acid and grind them thoroughly to obtain a compound corrosion inhibitor; S2: placing the compound corrosion inhibitor obtained in step S1 at the bottom of a sealed container, and placing the carbon steel to be treated above the compound corrosion inhibitor in the sealed container, and heating to obtain the carbon steel surface composite amino acid assembly film; The heating temperature in step S2 is 50-80° C. and the heating time is 6-12 hours.
2. The method for preparing a carbon steel surface composite amino acid assembly film according to claim 1, characterized in that: The long-chain fatty acid is a long-chain fatty acid with carbon atoms greater than or equal to 8.
3. The method for preparing a composite amino acid assembled film on carbon steel surface according to claim 2, characterized in that: The long-chain fatty acid is lauric acid.
4. The method for preparing a carbon steel surface composite amino acid assembly film according to claim 1, characterized in that: The long-chain fatty amine is a long-chain fatty amine with carbon atoms greater than or equal to 8.
5. The method for preparing a carbon steel surface composite amino acid assembly film according to claim 4, characterized in that: The long-chain fatty amine is dodecylamine.
6. The method for preparing a carbon steel surface composite amino acid assembly film according to claim 1, characterized in that: The amino acid is alanine, lysine or phenylalanine.
7. Use of the method for preparing the composite amino acid assembled film on the surface of carbon steel as claimed in any one of claims 1 to 6 in metal corrosion protection.